Acid-resistant and wear-resistant coating for inner wall of metal clean flue of boiler as well as preparation method and use method of acid-resistant and wear

By using modified epoxy resin and chemical-resistant epoxy phenolic resin combined with nano-titanium dioxide, silicon carbide and other fillers, the problem of insufficient acid resistance and wear resistance of the existing boiler metal clean flue inner wall anti-corrosion coatings has been solved, and the problem has been achieved. Effective anti-corrosion and long-term protection in high temperature and high pressure environments extend the service life of the equipment.

CN118755364APending Publication Date: 2024-10-11NORTH PAINT & COATINGS IND RES & DESIGN INS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411035240.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The anti-corrosion coating on the inner wall of the existing boiler metal clean flue has insufficient acid resistance and wear resistance, and cannot effectively prevent corrosion in high-temperature and high-pressure acidic environments. Maintenance is frequent and equipment operation is discontinuous.

Method used

Using modified epoxy resin and chemical-resistant epoxy phenolic resin as the base material, with nano-titanium dioxide, silicon carbide, boron nitride and other fillers, combined with reactive diluents and additives, an acid-resistant product is prepared through a specific process. Anti-wear coating to improve the acid resistance and wear resistance of the coating.

Benefits of technology

It has achieved a coating with excellent acid resistance and wear resistance at high temperatures of 240°C, extending the service life of the metal clean flue, reducing maintenance costs, and improving the continuous operation capability of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004970897080000011
    Figure BDA0004970897080000011
  • Figure BDA0004970897080000021
    Figure BDA0004970897080000021
  • Figure BDA0004970897080000071
    Figure BDA0004970897080000071
Patent Text Reader

Abstract

The invention discloses an acid-resistant and wear-resistant coating for the inner wall of a metal clean flue of a boiler, which is prepared by the following steps of: performing ring opening modification on epoxy resin through soya oil acid, compounding and modifying epoxy phenolic resin as a base material, adding wear-resistant fillers such as high-temperature flue ash, nano titanium dioxide, silicon carbide and boron nitride, adding modified graphite and inert fillers, and matching with a bifunctional reactive diluent, thereby obtaining the acid-resistant and wear-resistant coating. According to the present invention, the coating material is coated on the flue purification metal structure, the paint film has characteristics of good acid resistance, 240 DEG C high temperature resistance, high film crosslinking degree, excellent wear resistance, good corrosion resistance after the coating material is coated on the inner wall of the metal flue purification, and the service life of the metal flue purification can be prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of boiler coatings, in particular to an acid-resistant and wear-resistant coating for the inner wall of a boiler metal clean flue and a preparation method and a use method thereof. Background Art

[0002] The inner wall of the boiler metal clean flue is often coated with anti-corrosion coatings, which are generally based on epoxy resin or silicone resin, and nano titanium dioxide, quartz powder, silicon carbide, etc. as fillers. The flue gas of metal industrial boilers often contains a large amount of corrosion products, the main components of which are chlorides, sulfides, iron oxides and a small amount of K+, Ca+, Zn+, etc. When high-temperature and high-pressure acidic gases and particulate smoke pass through the smoke cleaning equipment pipeline, they will adhere to the inner wall of the flue to form a dilute acid environment, causing strong corrosion to the flue. At the same time, the particulate smoke will strongly scour the inner wall of the flue with the high-pressure airflow, further exacerbating the corrosion. Effective anti-corrosion coatings can improve the long-term working stability of the clean flue and reduce maintenance costs.

[0003] Although the use of existing flue anticorrosion coatings has a certain effect, it also has obvious defects and cannot guarantee effective anticorrosion protection. The acid resistance of existing anticorrosion coatings is poor. It is difficult to ensure anticorrosion performance in the acidic environment formed by clean flue flue gas. Frequent maintenance and repair are required, and the continuous operation of equipment is hindered. Existing flue anticorrosion coatings do not have good wear resistance. Facing the scouring of the inner wall of the flue by solid particles carried by high-velocity flue gas, they cannot provide long-term protection. Summary of the invention

[0004] Aiming at the insufficient acid resistance and wear resistance of the existing flue anti-corrosion coatings, the present invention prepares an acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue. The coating is prepared by modifying the epoxy resin by ring-opening of soybean oil acid, compounding an epoxy phenolic resin with excellent chemical resistance as a base material, taking high-temperature flue ash, acid-resistant and wear-resistant powders such as nano-titanium dioxide, silicon carbide, and boron nitride as fillers, and adding active diluents, additives, etc.

[0005] The technical solution of the present invention is: an acid-resistant and wear-resistant coating for the inner wall of a boiler metal clean flue, which is composed of the following components by mass percentage:

[0006]

[0007] Furthermore, the acid-resistant and wear-resistant paint for the inner wall of the boiler metal clean flue is composed of the following components by mass percentage:

[0008]

[0009] Furthermore, the modified ring-opening epoxy resin is composed of the following components by mass percentage:

[0010] Soybean oil acid 10%~17%

[0011] Epoxy resin powder 60%~74%

[0012] Xylene 15% to 25%;

[0013] The preparation process of the modified ring-opening epoxy resin is as follows: slowly add the amount of xylene to a 500ml three-necked flask with a thermometer, a stirring head and a water separator, start stirring, slowly add the amount of epoxy resin powder under stirring, start heating and continue stirring until the resin is completely dissolved, slowly add the amount of soybean oil acid after the resin is completely dissolved, continue stirring and heat to 170°C to start condensation reflux dehydration, the reflux dehydration solvent in the water separator is xylene, continue reflux dehydration for 8 hours until no water is generated in the system, continue to keep warm and stir for 30 minutes, determine the acid value is less than 3, then cool and discharge to obtain the modified ring-opening epoxy resin;

[0014] Furthermore, the epoxy resin powder is epoxy E-20 resin powder.

[0015] Furthermore, the modified phenolic epoxy resin is one or more of DEN-431, DEN-438, and NPPN 638S; the wear-resistant filler is one or more of nano titanium dioxide, silicon carbide, boron nitride, and aluminum oxide; the inert filler is one or more of mica powder, talc powder, silicon micropowder, and precipitated barium sulfate;

[0016] Furthermore, the dispersing agent is BYK-163; the thixotropic agent is polyamide wax; the silane coupling agent is KH-560; the rheological agent is BYK-410; and the active diluent 2 is one or more of the bifunctional active diluents polypropylene glycol diglycidyl ether XY207 and XY217.

[0017] Furthermore, the modified amine curing agent is one or more of D6280, D230, 593, and T31; the active diluent 1 is one or more of the bifunctional active diluent polypropylene glycol diglycidyl ether XY207 and XY217.

[0018] The present invention also provides a method for preparing an acid-resistant and wear-resistant coating for the inner wall of a boiler metal clean flue, comprising the following steps:

[0019] (1) Preparing an acid-resistant and wear-resistant paint for the inner wall of a clean metal flue of a boiler: adding a reactive diluent 2 according to the formula amount into a stirring kettle, adding a modified open-ring epoxy resin and a modified phenolic epoxy resin in the formula amount, starting stirring, and stirring at a medium speed until uniform; adding a dispersing aid and a thixotropic agent in the formula amount, and starting high-speed dispersion for 5 minutes; then adjusting the stirring speed to medium-low speed, adding a wear-resistant filler, high-temperature flue ash, and an inert filler in the formula amount, adding 70% propylene glycol methyl ether, and dispersing at a high speed for 40 minutes, and when the system temperature reaches 55° C. to 65° C., reducing the stirring speed to medium speed and maintaining the temperature for 10 minutes; after the insulation is completed, adding a silane coupling agent and a rheological aid in the formula amount while stirring at a low speed; adjusting the viscosity with the remaining propylene glycol methyl ether, and thus obtaining an acid-resistant and wear-resistant paint for the inner wall of a clean metal flue of a boiler;

[0020] (2) Add the acid-resistant and anti-wear paint for the inner wall of the boiler metal clean flue prepared in step (1), the modified amine curing agent, PAPI, and the active diluent 1 into a beaker according to the formula amount, and stir and mix them evenly under normal temperature and pressure to obtain the acid-resistant and anti-wear coating for the inner wall of the boiler metal clean flue.

[0021] The present invention also provides a method for using the acid-resistant and wear-resistant coating for the inner wall of a boiler metal clean flue, comprising the following steps: scrubbing a substrate with butyl acetate or xylene to clean the surface of the substrate and drying it; spraying the prepared acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue evenly onto the surface of the substrate in the form of air spraying, and then placing the substrate under normal temperature and pressure conditions for static curing for 48 hours to obtain the acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue.

[0022] The present invention prepares an acid-resistant and wear-resistant coating for the inner wall of a boiler metal clean flue. The coating is applied on the metal structure of the clean flue. The paint film has good acid resistance and is resistant to high temperatures of 240°C. At the same time, the paint film has a high degree of cross-linking and excellent wear resistance. When applied to the inner wall of the metal clean flue, it can have good anti-corrosion performance and increase the service life of the metal clean flue.

[0023] The beneficial effects of the present invention are:

[0024] (1) The coating resin synthesis process of the present invention is simple and is less affected by the external environment;

[0025] (2) The present invention uses soy acid to ring-open the epoxy resin, and then mixes it with modified amine-cured epoxy phenolic resin with excellent chemical resistance as the base material. The cross-linking density is high, the chemical resistance is good, and the anti-corrosion performance can be guaranteed under a high temperature environment of 240°C;

[0026] (3) The present invention uses fillers such as aluminum oxide, boron nitride, and high-temperature flue ash to ensure the paint film's temperature resistance while also ensuring wear resistance and chemical resistance;

[0027] (4) When the coating of the present invention is applied on the metal structure of the clean flue, the paint film has better acid resistance and excellent wear resistance under high temperature conditions. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Embodiment 1:

[0030] Preparation of modified ring-opening epoxy resin: slowly add 96g of xylene solvent to a 500ml three-necked flask with a thermometer, a stirring head and a water separator, start stirring, slowly add 321.6g of epoxy E-20 resin powder under stirring, start heating and continue stirring until the resin is completely dissolved, slowly add 62.4g of soybean oil acid after the resin is completely dissolved, continue stirring and heat to 170°C to start condensation reflux dehydration, the reflux dehydration solvent in the water separator is xylene, continue reflux dehydration for 8h until no water is produced in the system, continue to keep warm and stir for 30min, determine the acid value <3, then cool and discharge, and obtain a light yellow transparent resin, which is the modified ring-opening epoxy resin 1;

[0031] Preparation of acid-resistant and wear-resistant paint for the inner wall of the clean metal flue of the boiler: add 7.5g of active diluent XY217 into a stirring kettle, add 100g of the prepared modified open-ring epoxy resin 1 and 100g of DEN-438 resin into the kettle, start stirring, stir at medium speed for 5min until uniform; add 3.5g of BYK-163 and 3.5g of polyamide wax, and disperse at high speed for 5min; add 45g of nano titanium dioxide, 60g of aluminum oxide, 45g of aluminum oxide under medium-low speed stirring; g high-temperature flue ash, 37.5 g modified graphite, 40 g silicon powder and 22.5 g mica powder, add 30 g propylene glycol methyl ether, disperse at high speed for 40 min, when the system temperature reaches 55°C-65°C, reduce the stirring speed to medium speed and keep warm and stir for 10 min; after the insulation is completed, add 3 g KH-560 and 3.5 g BYK-410 with low speed stirring; use the remaining 8 g propylene glycol methyl ether to adjust the viscosity, and prepare the acid-resistant and wear-resistant paint 1 for the inner wall of the boiler metal clean flue.

[0032] Preparation of acid-resistant and wear-resistant coating for the inner wall of boiler metal clean flue: Take 100g of acid-resistant and wear-resistant paint 1 for the inner wall of boiler metal clean flue, 9g of modified amine curing agent D6280, 7g of PAPI and 4g of active diluent XY217 into a beaker, stir and mix evenly without bubbles at normal temperature and pressure to obtain acid-resistant and wear-resistant coating 1 for the inner wall of boiler metal clean flue.

[0033] Preparation of acid-resistant and wear-resistant coating for inner wall of clean metal flue of boiler: Use butyl acetate or xylene to scrub the substrate to make the surface of the substrate clean and dry; spray the prepared acid-resistant and wear-resistant coating 1 for inner wall of clean metal flue of boiler evenly on the surface of the substrate in the form of air spraying, and the coating amount is determined according to the actual use. Then place the substrate under normal temperature and pressure environment for curing for 48 hours to obtain the acid-resistant and wear-resistant coating for inner wall of clean metal flue of boiler with excellent acid resistance and wear resistance.

[0034] Example 2

[0035] Preparation of modified ring-opening epoxy resin: Slowly add 48g of xylene solvent to a 500ml three-necked flask equipped with a thermometer, a stirring head and a water separator, start stirring, slowly add 160g of epoxy E-20 resin powder while stirring, start heating and continue stirring until the resin is completely dissolved, slowly add 32g of soybean oil acid after the resin is completely dissolved, continue stirring and heat to 170°C to start condensation reflux dehydration, the reflux dehydration solvent in the water separator is xylene, continue reflux dehydration for 8h until no water is produced in the system, continue to keep warm and stir for 30min, determine the acid value <3, then cool and discharge the material to obtain a light yellow transparent resin, which is the modified ring-opening epoxy resin 2.

[0036] Preparation of acid-resistant and wear-resistant paint for the inner wall of boiler metal clean flue: add 1.5g active diluent XY217 into a stirring kettle, add 20g modified open-ring epoxy resin 2 and 18g DEN-431 resin into the kettle, start stirring, stir at medium speed for 5min until uniform; add 0.7g BYK-163 and 0.7g polyamide wax, disperse at high speed for 5min; add 9g modified graphite, 7.5g aluminum oxide, 7.5g tantalum and 10g tantalum under medium-low speed stirring; g silicon carbide, 7.5 g high-temperature flue ash and 12.5 g mica powder, add 5 g propylene glycol methyl ether, disperse at high speed for 40 minutes, when the system temperature reaches 55°C ~ 65°C, reduce the stirring speed to medium speed and keep warm and stir for 10 minutes; after the insulation is completed, add 0.7 g KH-560 and 0.7 g BYK-410 with low speed stirring; use the remaining 2.6 g propylene glycol methyl ether to adjust the viscosity, and prepare the boiler metal clean flue inner wall acid and wear resistant paint 2.

[0037] Preparation of acid-resistant and wear-resistant coating for the inner wall of boiler metal clean flue: Take 200g of acid-resistant and wear-resistant paint 2 for the inner wall of boiler metal clean flue, 18g of modified amine curing agent 593, 15g of PAPI and 8g of active diluent XY217 and add them into a beaker, stir and mix evenly at room temperature and pressure without bubbles, and you will get acid-resistant and wear-resistant coating 2 for the inner wall of boiler metal clean flue.

[0038] Preparation of acid-resistant and wear-resistant coating for the inner wall of boiler metal clean flue: Use butyl acetate or xylene to scrub the substrate to make the surface of the substrate clean and let it dry; spray the prepared acid-resistant and wear-resistant coating 2 for the inner wall of boiler metal clean flue evenly onto the surface of the substrate in the form of air spray, and the coating amount is determined according to the actual use. Then place the substrate under normal temperature and pressure conditions for static curing for 48 hours to obtain an acid-resistant and wear-resistant coating for the inner wall of boiler metal clean flue with excellent acid resistance and wear resistance.

[0039] Example 3

[0040] Preparation of modified ring-opening epoxy resin: Slowly add 20g of xylene solvent to a 150ml three-necked flask equipped with a thermometer, a stirring head and a water separator, start stirring, slowly add 67g of epoxy E-20 resin powder while stirring, turn on heating and continue stirring until the resin is completely dissolved, slowly add 13g of soybean oil acid after the resin is completely dissolved, continue stirring and heat to 170°C to start condensation reflux dehydration, the reflux dehydration solvent in the water separator is xylene, continue reflux dehydration for 8h until no water is produced in the system, continue to keep warm and stir for 30min, determine the acid value <3, then cool and discharge the material to obtain a light yellow transparent resin, which is the modified ring-opening epoxy resin 3.

[0041] Preparation of acid-resistant and wear-resistant paint for the inner wall of boiler metal clean flue: 4.5g of active diluent XY217 was added to a stirred tank, 54g of modified open-ring epoxy resin 3 and 60g of modified phenolic epoxy resin NPPN were added. 638S was added into the kettle, stirring was started, and stirring was carried out at medium speed for 5 minutes until uniform; 2.1g BYK-163 and 2.1g polyamide wax were added, and high-speed dispersion was carried out for 5 minutes; 30g modified graphite, 22.5g aluminum oxide, 22.5g boron nitride, 30g high-temperature flue ash, 30g talcum powder and 15g mica powder were added under medium-low speed stirring, and 16g propylene glycol methyl ether was added, and high-speed dispersion was carried out for 40 minutes. When the system temperature reached 55°C-65°C, the stirring speed was reduced to medium speed and the mixture was kept warm and stirred for 10 minutes; after the insulation was completed, 2.3g silane coupling agent KH-560 and 2.3g BYK-410 were added under low speed stirring; the remaining 7g propylene glycol methyl ether was used to adjust the viscosity to prepare the acid-resistant and wear-resistant paint 3 for the inner wall of the boiler metal clean flue.

[0042] Preparation of acid-resistant and wear-resistant coating for the inner wall of boiler metal clean flue: Take 200g of acid-resistant and wear-resistant paint 3 for the inner wall of boiler metal clean flue, 15g of modified amine curing agent D6280, 17g of PAPI and 8g of active diluent XY217 into a beaker, stir and mix evenly at room temperature and pressure without bubbles, and obtain acid-resistant and wear-resistant coating 3 for the inner wall of boiler metal clean flue.

[0043] Preparation of acid-resistant and wear-resistant coating for the inner wall of boiler metal clean flue: Use butyl acetate or xylene to scrub the substrate to make the surface of the substrate clean and let it dry; spray the prepared acid-resistant and wear-resistant coating 3 for the inner wall of boiler metal clean flue evenly on the surface of the substrate in the form of air spray, and the coating amount is determined according to the actual use. Then place the substrate under normal temperature and pressure conditions for static curing for 48 hours to obtain an acid-resistant and wear-resistant coating for the inner wall of boiler metal clean flue with excellent acid resistance and wear resistance.

[0044] The test was carried out in accordance with the national standards "GB / T 1728-2020 Determination of drying time of paint film and putty film", "GB / T10125-2021 Artificial atmosphere corrosion test salt spray test", "GB / T 1735-2009 Determination of heat resistance of paints and varnishes", and "GB / T 1768-2006 Determination of abrasion resistance of paints and varnishes rotating rubber grinding wheel method". The test results are as follows

[0045]

[0046] The present disclosure has been described by the above-mentioned relevant embodiments, but the above-mentioned embodiments are only examples for implementing the present disclosure. It must be pointed out that the disclosed embodiments do not limit the scope of the present disclosure. On the contrary, changes and modifications made without departing from the spirit and scope of the present disclosure are all within the scope of patent protection of the present disclosure.

Claims

1. An acid-resistant and wear-resistant coating for the inner wall of a boiler metal clean flue, characterized in that: By mass percentage, it is composed of the following components:

2. The acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue according to claim 1, characterized in that: The acid-resistant and wear-resistant paint for the inner wall of the boiler metal clean flue is composed of the following components by mass percentage:

3. The acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue according to claim 2 is characterized by: The modified ring-opening epoxy resin is composed of the following components by mass percentage: Soybean oil acid 10%~17% Epoxy resin powder 60%~74% Xylene 15% to 25%; The preparation process of the modified ring-opening epoxy resin is as follows: slowly add the amount of xylene to a 500ml three-necked flask with a thermometer, a stirring head and a water separator, start stirring, slowly add the amount of epoxy resin powder under stirring, start heating and continue stirring until the resin is completely dissolved, slowly add the amount of soybean oil acid after the resin is completely dissolved, continue stirring and heat to 170°C to start condensation reflux dehydration, the reflux dehydration solvent in the water separator is xylene, continue reflux dehydration for 8 hours until no water is produced in the system, continue to keep warm and stir for 30 minutes, determine the acid value <3, then cool and discharge to obtain the modified ring-opening epoxy resin; the epoxy resin powder is epoxy E-20 resin powder.

4. The acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue according to claim 2, characterized in that: The modified phenolic epoxy resin is one or more of DEN-431, DEN-438 and NPPN 638S.

5. The acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue according to claim 2, characterized in that: The wear-resistant filler is one or more of nano titanium dioxide, silicon carbide, boron nitride and aluminum oxide.

6. The acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue according to claim 2, characterized in that: The inert filler is one or more of mica powder, talcum powder, silica powder and precipitated barium sulfate.

7. The acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue according to claim 2, characterized in that: The dispersing agent is BYK-163; the thixotropic agent is polyamide wax; the silane coupling agent is KH-560; the rheological agent is BYK-410; and the active diluent 2 is one or more of the bifunctional active diluents polypropylene glycol diglycidyl ether XY207 and XY217.

8. The acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue according to claim 1, characterized in that: The modified amine curing agent is one or more of D6280, D230, 593, and T31; the active diluent 1 is one or more of bifunctional active diluent polypropylene glycol diglycidyl ether XY207 and XY217.

9. A method for preparing the acid-resistant and wear-resistant coating for the inner wall of a boiler metal clean flue as claimed in any one of claims 1 to 8, characterized in that: The steps include: (1) Preparing an acid-resistant and wear-resistant paint for the inner wall of a clean metal flue of a boiler: adding a reactive diluent 2 according to the formula amount into a stirring kettle, adding a modified open-ring epoxy resin and a modified phenolic epoxy resin in the formula amount, starting stirring, and stirring at a medium speed until uniform; adding a dispersing aid and a thixotropic agent in the formula amount, and starting high-speed dispersion for 5 minutes; then adjusting the stirring speed to medium-low speed, adding a wear-resistant filler, high-temperature flue ash, and an inert filler in the formula amount, adding 70% propylene glycol methyl ether, and dispersing at a high speed for 40 minutes, and when the system temperature reaches 55° C. to 65° C., reducing the stirring speed to medium speed and maintaining the temperature for 10 minutes; after the insulation is completed, adding a silane coupling agent and a rheological aid in the formula amount while stirring at a low speed; adjusting the viscosity with the remaining propylene glycol methyl ether, and thus obtaining an acid-resistant and wear-resistant paint for the inner wall of a clean metal flue of a boiler; (2) Add the acid-resistant and anti-wear paint for the inner wall of the boiler metal clean flue prepared in step (1), the modified amine curing agent, PAPI, and the active diluent 1 into a beaker according to the formula amount, and stir and mix them evenly under normal temperature and pressure to obtain the acid-resistant and anti-wear coating for the inner wall of the boiler metal clean flue.

10. A method for using the acid-resistant and wear-resistant coating for the inner wall of a boiler metal clean flue according to any one of claims 1 to 8, characterized in that: The following steps are involved: The substrate is scrubbed with butyl acetate or xylene to make the surface of the substrate clean and dry; the prepared acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue is evenly sprayed onto the surface of the substrate in the form of air spraying, and then the substrate is placed under normal temperature and pressure conditions for static curing for 48 hours to obtain the acid-resistant and wear-resistant coating for the inner wall of the boiler metal clean flue.

Citation Information

Patent Citations

  • Liquid level coating material of wet-process smelting electrolytic zinc negative plate and preparation method for liquid level coating material

    CN109609009A

  • Acid-resistant and high-temperature-resistant phenolic epoxy anticorrosive paint and preparation method thereof