Black highlight polyester powder coating and preparation method thereof

By adding high-gloss additives and fillers to polyester powder coatings, the gloss and aging resistance of the coating are improved, the problem of performance degradation of polyester powder coatings after ultraviolet irradiation is solved, and high gloss, wear resistance, and environmental protection are achieved. coating effect.

CN118755366AActive Publication Date: 2024-10-11ZHEJIANG ZHIMA NETWORK TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410972887.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-11
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The performance of existing polyester powder coatings deteriorates after long-term UV irradiation, the glossiness decreases, and the wear resistance decreases, which affects its service life.

Method used

Adopting a black high-gloss polyester powder coating formula, including unsaturated polyester resin, curing agent, carbon black, high-gloss additives, fillers (such as titanium dioxide and calcium carbonate), antioxidants and leveling agents, through specific mixing and processing Methods prepare high-gloss additives and fillers to improve the gloss and aging resistance of the coating.

Benefits of technology

The formed coating has high gloss, good hiding power and mechanical properties, which significantly improves the durability and gloss-preserving properties of the coating, avoids solvent volatilization, and ensures green and environmental safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755366A_ABST
    Figure CN118755366A_ABST
Patent Text Reader

Abstract

The invention discloses a black high-gloss polyester powder coating and a preparation method thereof, and relates to the technical field of coatings, and the black high-gloss polyester powder coating is prepared from the following components: polyester resin, a curing agent, carbon black, a high-gloss auxiliary agent, a filler, an antioxidant and a flatting agent. Wherein the mixing mass ratio of the carbon black to the highlight additive is 4: 1; wherein the adopted polyester resin is unsaturated polyester resin; after the polyester powder coating prepared by the invention is sprayed, a formed coating does not fall off, does not blister and has relatively high glossiness. The polyester powder coating prepared by the invention does not contain a solvent, does not generate a volatilization phenomenon of an organic solvent, and is green and safe. The glossiness of a coating can be greatly improved through the prepared highlight additive, the gloss retention performance of the coating is greatly improved, grooves and holes in the surface of the coating can be effectively filled by introducing the highlight additive prepared through the method, and therefore the compactness degree of the surface layer of the coating is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, in particular to a black high-gloss polyester powder coating and a preparation method thereof. Background Art

[0002] Powder coating is a green coating without volatile solvents. Since it does not require solvents, powder coating has many advantages such as low pollution, high material utilization rate, and low energy consumption. It is widely used in many fields.

[0003] Powder coatings are divided into two categories: thermoplastic and thermosetting. Thermoplastic powder coatings have poor coating appearance (gloss and leveling), but the adhesion between thermoplastic powder coatings and substrates is relatively poor. Thermosetting powder coatings use thermosetting synthetic resins as film-forming materials. During the drying process, the resin first melts and then solidifies into a smooth and hard coating after chemical cross-linking.

[0004] Thermosetting powder coatings mainly utilize the cross-linking reaction between resin and curing agent after heating to form an infusible hard coating. Even if the ambient temperature is high, the coating will only decompose and will not soften like thermoplastic resin coatings. Therefore, it has stronger mechanical properties.

[0005] As an important type of powder coating, polyester powder coating has good weather resistance and climate stability, good adhesion ability, and good bonding strength with a variety of substrates. However, due to the properties of polyester itself, polyester will deteriorate after long-term ultraviolet exposure, resulting in reduced durability, a significant decrease in gloss, reduced wear resistance and other shortcomings, which seriously affect its use.

[0006] Based on this, a black high-gloss polyester powder coating and a preparation method thereof are provided to solve the existing technical problems. Summary of the invention

[0007] The purpose of the present invention is to provide a black high-gloss polyester powder coating and a preparation method thereof, so as to solve the deficiencies in the prior art.

[0008] The technical solution adopted by the present invention is as follows:

[0009] A black high-gloss polyester powder coating, comprising the following components by weight: 85-94 parts of polyester resin, 6-8 parts of curing agent, 2-3.2 parts of carbon black, 0.5-0.8 parts of high-gloss auxiliary agent, 23-25 ​​parts of filler, 0.8-1.2 parts of antioxidant, and 1-2 parts of leveling agent;

[0010] Among them, the mixing mass ratio of carbon black and high gloss additive is 4:1;

[0011] Wherein, the polyester resin used is unsaturated polyester resin.

[0012] As a further technical solution: the preparation method of the high gloss auxiliary agent is:

[0013] (1) adding an organic solvent into a reaction kettle, and then sequentially adding butyl acrylate, methyl methacrylate, and graphene into the reaction kettle, stirring and mixing at a speed of 550 r / min for 20 min to obtain a base liquid;

[0014] (2) adding the initiator to the organic solvent, stirring and mixing at a speed of 500 r / min to obtain an initiator solution;

[0015] (3) The prepared initiator solution is added dropwise into the reaction kettle, and then the mixture is stirred and reacted at 80° C. for 2 hours. A portion of the organic solvent is first removed by atmospheric distillation, and then the remaining organic solvent is removed by reduced pressure distillation. Finally, the mixture is crushed and then sieved through a 500-mesh sieve to obtain a high-gloss additive.

[0016] As a further technical solution: the graphene is pre-modified:

[0017] Add graphene and maleic anhydride to the nitric acid solution, adjust the temperature to 60°C, keep warm and stir for 15 minutes, then adjust the temperature to 85°C, continue to keep warm and stir for 20 minutes, then filter, wash with water to neutrality, and dry to constant weight to obtain preliminary graphene;

[0018] The preliminary graphene and cerium chloride obtained above were mixed evenly in a mass ratio of 1000:1, and then plasma treated for 1 hour under a nitrogen atmosphere at a power of 300 W, and then discharged, washed with a 50% ethanol solution by mass, and then filtered and dried to constant weight to complete the treatment;

[0019] Among them, the mixing mass ratio of graphene, maleic anhydride and nitric acid solution is 1:3:10;

[0020] The mass fraction of the nitric acid solution is 12%;

[0021] Among them, the drying temperature is 60°C and the drying time is 40 minutes.

[0022] As a further technical solution: the organic solvent is xylene;

[0023] The mixed mass ratio of xylene, butyl acrylate, methyl methacrylate and graphene is 30:5-8:4-6:0.6-0.8;

[0024] The initiator is dibenzoyl peroxide;

[0025] The mass fraction of the initiator solution is 5%;

[0026] The mixing mass ratio of the initiator solution to the base liquid is 1:5-6.

[0027] As a further technical solution: the curing agent is diaminophenyl sulfone.

[0028] As a further technical solution: the filler is a mixture of titanium dioxide and calcium carbonate;

[0029] Among them, the mixing mass ratio of titanium dioxide and calcium carbonate is 1:8.

[0030] As a further technical solution: the antioxidant is antioxidant 1010.

[0031] As a further technical solution: the leveling agent is polyacrylate.

[0032] A method for preparing a black high-gloss polyester powder coating comprises the following steps:

[0033] S1. First, a polyester resin, a curing agent, carbon black, a high gloss agent, a filler, an antioxidant, and a leveling agent are added to a mixer and stirred for 15 minutes to obtain a mixture;

[0034] High-speed mixing speed is 800r / min;

[0035] S2. The mixture obtained above is then added to a dryer for drying;

[0036] Among them, the drying temperature is 60°C and the drying time is 2 hours;

[0037] S3. The dried mixture is added to a twin-screw extruder and melt-extruded;

[0038] S4. After the melt is extruded through a twin-screw extruder, it is transported to a tablet press for tableting to obtain a sheet, and then the sheet is crushed and sieved to obtain a finished black high-gloss polyester powder coating;

[0039] Among them, the average particle size of the black high-gloss polyester powder coating is 30μm.

[0040] Beneficial effects:

[0041] After the polyester powder coating prepared by the invention is sprayed, the formed coating does not fall off or bubble and has high gloss.

[0042] The polyester powder coating prepared by the invention does not contain solvent, does not generate volatilization of organic solvent, and is green and safe.

[0043] The high gloss additive prepared by the present invention can greatly improve the gloss of the coating, and has a greatly improved light retention performance of the coating. By introducing the high gloss additive prepared by the present invention, the grooves and holes on the surface of the coating can be effectively filled, thereby greatly improving the density of the surface layer of the coating. After the uneven surface of the coating is filled into a smooth surface, the reflection effect of the coating surface on light can be greatly improved, thereby improving the gloss performance of the coating.

[0044] The present invention introduces titanium dioxide and calcium carbonate as fillers into the coating, which can not only effectively improve the mechanical properties of the coating, but also provide the coating with good covering power, so that the coating can completely and completely cover the surface of the substrate, so that the coating has good uniformity, and the titanium dioxide introduced therein can further improve the smoothness of the coating, so that the coating surface can present a better bright effect. Since the titanium dioxide is evenly distributed in the coating, it can play a significant ultraviolet absorption role in combination with the high-gloss auxiliary agent, thereby greatly improving the aging resistance of the coating, and the light retention performance is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a histogram of the gloss retention of the embodiments and comparative examples. DETAILED DESCRIPTION

[0046] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] Example 1

[0048] A black high-gloss polyester powder coating, comprising the following components by weight: 85 parts of polyester resin, 6 parts of diaminophenyl sulfone, 2 parts of carbon black, 0.5 parts of high-gloss additive, 23 parts of filler, 10100.8 parts of antioxidant, and 1 part of polyacrylate;

[0049] Among them, the mixing mass ratio of carbon black and high gloss additive is 4:1;

[0050] Wherein, the polyester resin used is di(2-ethylhexyl) phthalate.

[0051] The preparation method of the high gloss additive is as follows:

[0052] (1) adding xylene into a reaction kettle, and then sequentially adding butyl acrylate, methyl methacrylate, and graphene into the reaction kettle, stirring and mixing at a speed of 550 r / min for 20 min to obtain a base liquid;

[0053] (2) adding the initiator to xylene, stirring and mixing at a speed of 500 r / min to obtain an initiator solution;

[0054] (3) The prepared initiator solution is added dropwise into the reactor, and then the mixture is stirred and reacted at 80° C. for 2 hours. A portion of the xylene is first removed by atmospheric distillation, and then the remaining xylene is removed by reduced pressure distillation. Finally, the mixture is crushed and then sieved through a 500-mesh sieve to obtain a high-gloss additive.

[0055] Graphene is pre-modified:

[0056] Add graphene and maleic anhydride to the nitric acid solution, adjust the temperature to 60°C, keep warm and stir for 15 minutes, then adjust the temperature to 85°C, continue to keep warm and stir for 20 minutes, then filter, wash with water to neutrality, and dry to constant weight to obtain preliminary graphene;

[0057] The preliminary graphene and cerium chloride obtained above were mixed evenly in a mass ratio of 1000:1, and then plasma treated for 1 hour under a nitrogen atmosphere at a power of 300 W, and then discharged, washed with a 50% ethanol solution by mass, and then filtered and dried to constant weight to complete the treatment;

[0058] Among them, the mixing mass ratio of graphene, maleic anhydride and nitric acid solution is 1:3:10;

[0059] The mass fraction of the nitric acid solution is 12%;

[0060] Among them, the drying temperature is 60°C and the drying time is 40 minutes.

[0061] The mixed mass ratio of xylene, butyl acrylate, methyl methacrylate and graphene is 30:5:4:0.6;

[0062] The initiator is dibenzoyl peroxide;

[0063] The mass fraction of the initiator solution is 5%;

[0064] The mass ratio of the initiator solution to the base solution is 1:5; the filler is a mixture of titanium dioxide and calcium carbonate;

[0065] Among them, the mixing mass ratio of titanium dioxide and calcium carbonate is 1:8.

[0066] A method for preparing a black high-gloss polyester powder coating comprises the following steps:

[0067] S1. First, a polyester resin, a curing agent, carbon black, a high gloss agent, a filler, an antioxidant, and a leveling agent are added to a mixer and stirred for 15 minutes to obtain a mixture;

[0068] High-speed mixing speed is 800r / min;

[0069] S2. The mixture obtained above is then added to a dryer for drying;

[0070] Among them, the drying temperature is 60°C and the drying time is 2 hours;

[0071] S3. The dried mixture is added to a twin-screw extruder and melt-extruded;

[0072] S4. After the melt is extruded through a twin-screw extruder, it is transported to a tablet press for tableting to obtain a sheet, and then the sheet is crushed and sieved to obtain a finished black high-gloss polyester powder coating;

[0073] Among them, the average particle size of the black high-gloss polyester powder coating is 30μm.

[0074] Example 2

[0075] A black high-gloss polyester powder coating, comprising the following components by weight: 88 parts of polyester resin, 6.5 parts of diaminophenyl sulfone, 2.4 parts of carbon black, 0.6 parts of high-gloss auxiliary agent, 24 parts of filler, 0.9 parts of antioxidant 1010, and 1.5 parts of polyacrylate;

[0076] Among them, the mixing mass ratio of carbon black and high gloss additive is 4:1;

[0077] Wherein, the polyester resin used is di(2-ethylhexyl) phthalate.

[0078] The preparation method of the high gloss additive is as follows:

[0079] (1) adding xylene into a reaction kettle, and then sequentially adding butyl acrylate, methyl methacrylate, and graphene into the reaction kettle, stirring and mixing at a speed of 550 r / min for 20 min to obtain a base liquid;

[0080] (2) adding the initiator to xylene, stirring and mixing at a speed of 500 r / min to obtain an initiator solution;

[0081] (3) The prepared initiator solution is added dropwise into the reactor, and then the mixture is stirred and reacted at 80° C. for 2 hours. A portion of the xylene is first removed by atmospheric distillation, and then the remaining xylene is removed by reduced pressure distillation. Finally, the mixture is crushed and then sieved through a 500-mesh sieve to obtain a high-gloss additive.

[0082] Graphene is pre-modified:

[0083] Add graphene and maleic anhydride to the nitric acid solution, adjust the temperature to 60°C, keep warm and stir for 15 minutes, then adjust the temperature to 85°C, continue to keep warm and stir for 20 minutes, then filter, wash with water to neutrality, and dry to constant weight to obtain preliminary graphene;

[0084] The preliminary graphene and cerium chloride obtained above were mixed evenly in a mass ratio of 1000:1, and then plasma treated for 1 hour under a nitrogen atmosphere at a power of 300 W, and then discharged, washed with a 50% ethanol solution by mass, and then filtered and dried to constant weight to complete the treatment;

[0085] Among them, the mixing mass ratio of graphene, maleic anhydride and nitric acid solution is 1:3:10;

[0086] The mass fraction of the nitric acid solution is 12%;

[0087] Among them, the drying temperature is 60°C and the drying time is 40 minutes.

[0088] The mixed mass ratio of xylene, butyl acrylate, methyl methacrylate and graphene is 30:6:5:0.7;

[0089] The initiator is dibenzoyl peroxide;

[0090] The mass fraction of the initiator solution is 5%;

[0091] The mass ratio of the initiator solution to the base liquid is 1:5.5; the filler is a mixture of titanium dioxide and calcium carbonate;

[0092] Among them, the mixing mass ratio of titanium dioxide and calcium carbonate is 1:8.

[0093] A method for preparing a black high-gloss polyester powder coating comprises the following steps:

[0094] S1. First, a polyester resin, a curing agent, carbon black, a high gloss agent, a filler, an antioxidant, and a leveling agent are added to a mixer and stirred for 15 minutes to obtain a mixture;

[0095] High-speed mixing speed is 800r / min;

[0096] S2. The mixture obtained above is then added to a dryer for drying;

[0097] Among them, the drying temperature is 60°C and the drying time is 2 hours;

[0098] S3. The dried mixture is added to a twin-screw extruder and melt-extruded;

[0099] S4. After the melt is extruded through a twin-screw extruder, it is transported to a tablet press for tableting to obtain a sheet, and then the sheet is crushed and sieved to obtain a finished black high-gloss polyester powder coating;

[0100] Among them, the average particle size of the black high-gloss polyester powder coating is 30μm.

[0101] Example 3

[0102] A black high-gloss polyester powder coating, comprising the following components by weight: 90 parts of polyester resin, 7 parts of diaminophenyl sulfone, 2.8 parts of carbon black, 0.7 parts of high-gloss additive, 24 parts of filler, 10101 parts of antioxidant, and 1.5 parts of polyacrylate;

[0103] Among them, the mixing mass ratio of carbon black and high gloss additive is 4:1;

[0104] The polyester resin used is di(2-ethylhexyl) phthalate.

[0105] The preparation method of the high gloss additive is as follows:

[0106] (1) adding xylene into a reaction kettle, and then sequentially adding butyl acrylate, methyl methacrylate, and graphene into the reaction kettle, stirring and mixing at a speed of 550 r / min for 20 min to obtain a base liquid;

[0107] (2) adding the initiator to xylene, stirring and mixing at a speed of 500 r / min to obtain an initiator solution;

[0108] (3) The prepared initiator solution is added dropwise into the reactor, and then the mixture is stirred and reacted at 80° C. for 2 hours. A portion of the xylene is first removed by atmospheric distillation, and then the remaining xylene is removed by reduced pressure distillation. Finally, the mixture is crushed and then sieved through a 500-mesh sieve to obtain a high-gloss additive.

[0109] Graphene is pre-modified:

[0110] Add graphene and maleic anhydride to the nitric acid solution, adjust the temperature to 60°C, keep warm and stir for 15 minutes, then adjust the temperature to 85°C, continue to keep warm and stir for 20 minutes, then filter, wash with water to neutrality, and dry to constant weight to obtain preliminary graphene;

[0111] The preliminary graphene and cerium chloride obtained above were mixed evenly in a mass ratio of 1000:1, and then plasma treated for 1 hour under a nitrogen atmosphere at a power of 300 W, and then discharged, washed with a 50% ethanol solution by mass, and then filtered and dried to constant weight to complete the treatment;

[0112] Among them, the mixing mass ratio of graphene, maleic anhydride and nitric acid solution is 1:3:10;

[0113] The mass fraction of the nitric acid solution is 12%;

[0114] Among them, the drying temperature is 60°C and the drying time is 40 minutes.

[0115] The mixed mass ratio of xylene, butyl acrylate, methyl methacrylate and graphene is 30:7:5:0.7;

[0116] The initiator is dibenzoyl peroxide;

[0117] The mass fraction of the initiator solution is 5%;

[0118] The mass ratio of the initiator solution to the base liquid is 1:5.8; the filler is a mixture of titanium dioxide and calcium carbonate;

[0119] Among them, the mixing mass ratio of titanium dioxide and calcium carbonate is 1:8.

[0120] A method for preparing a black high-gloss polyester powder coating comprises the following steps:

[0121] S1. First, a polyester resin, a curing agent, carbon black, a high gloss agent, a filler, an antioxidant, and a leveling agent are added to a mixer and stirred for 15 minutes to obtain a mixture;

[0122] High-speed mixing speed is 800r / min;

[0123] S2. The mixture obtained above is then added to a dryer for drying;

[0124] Among them, the drying temperature is 60°C and the drying time is 2 hours;

[0125] S3. The dried mixture is added to a twin-screw extruder and melt-extruded;

[0126] S4. After the melt is extruded through a twin-screw extruder, it is transported to a tablet press for tableting to obtain a sheet, and then the sheet is crushed and sieved to obtain a finished black high-gloss polyester powder coating;

[0127] Among them, the average particle size of the black high-gloss polyester powder coating is 30μm.

[0128] Example 4

[0129] A black high-gloss polyester powder coating, comprising the following components by weight: 92 parts of polyester resin, 7 parts of diaminophenyl sulfone, 2.8 parts of carbon black, 0.7 parts of high-gloss additive, 24 parts of filler, 10101.2 parts of antioxidant, and 2 parts of polyacrylate;

[0130] Among them, the mixing mass ratio of carbon black and high gloss additive is 4:1;

[0131] The polyester resin used is di(2-ethylhexyl) phthalate.

[0132] The preparation method of the high gloss additive is as follows:

[0133] (1) adding xylene into a reaction kettle, and then sequentially adding butyl acrylate, methyl methacrylate, and graphene into the reaction kettle, stirring and mixing at a speed of 550 r / min for 20 min to obtain a base liquid;

[0134] (2) adding the initiator to xylene, stirring and mixing at a speed of 500 r / min to obtain an initiator solution;

[0135] (3) The prepared initiator solution is added dropwise into the reactor, and then the mixture is stirred and reacted at 80° C. for 2 hours. A portion of the xylene is first removed by atmospheric distillation, and then the remaining xylene is removed by reduced pressure distillation. Finally, the mixture is crushed and then sieved through a 500-mesh sieve to obtain a high-gloss additive.

[0136] Graphene is pre-modified:

[0137] Add graphene and maleic anhydride to the nitric acid solution, adjust the temperature to 60°C, keep warm and stir for 15 minutes, then adjust the temperature to 85°C, continue to keep warm and stir for 20 minutes, then filter, wash with water to neutrality, and dry to constant weight to obtain preliminary graphene;

[0138] The preliminary graphene and cerium chloride obtained above were mixed evenly in a mass ratio of 1000:1, and then plasma treated for 1 hour under a nitrogen atmosphere at a power of 300 W, and then discharged, washed with a 50% ethanol solution by mass, and then filtered and dried to constant weight to complete the treatment;

[0139] Among them, the mixing mass ratio of graphene, maleic anhydride and nitric acid solution is 1:3:10;

[0140] The mass fraction of the nitric acid solution is 12%;

[0141] Among them, the drying temperature is 60°C and the drying time is 40 minutes.

[0142] The mixed mass ratio of xylene, butyl acrylate, methyl methacrylate and graphene is 30:6:5:0.6;

[0143] The initiator is dibenzoyl peroxide;

[0144] The mass fraction of the initiator solution is 5%;

[0145] The mass ratio of the initiator solution to the base solution is 1:5; the filler is a mixture of titanium dioxide and calcium carbonate;

[0146] Among them, the mixing mass ratio of titanium dioxide and calcium carbonate is 1:8.

[0147] A method for preparing a black high-gloss polyester powder coating comprises the following steps:

[0148] S1. First, a polyester resin, a curing agent, carbon black, a high gloss agent, a filler, an antioxidant, and a leveling agent are added to a mixer and stirred for 15 minutes to obtain a mixture;

[0149] High-speed mixing speed is 800r / min;

[0150] S2. The mixture obtained above is then added to a dryer for drying;

[0151] Among them, the drying temperature is 60°C and the drying time is 2 hours;

[0152] S3. The dried mixture is added to a twin-screw extruder and melt-extruded;

[0153] S4. After the melt is extruded through a twin-screw extruder, it is transported to a tablet press for tableting to obtain a sheet, and then the sheet is crushed and sieved to obtain a finished black high-gloss polyester powder coating;

[0154] Among them, the average particle size of the black high-gloss polyester powder coating is 30μm.

[0155] Example 5

[0156] A black high-gloss polyester powder coating, comprising the following components by weight: 94 parts of polyester resin, 8 parts of diaminophenyl sulfone, 3.2 parts of carbon black, 0.8 parts of high-gloss additive, 25 parts of filler, 10101.2 parts of antioxidant, and 2 parts of polyacrylate;

[0157] Among them, the mixing mass ratio of carbon black and high gloss additive is 4:1;

[0158] The polyester resin used is di(2-ethylhexyl) phthalate.

[0159] The preparation method of the high gloss additive is as follows:

[0160] (1) adding xylene into a reaction kettle, and then sequentially adding butyl acrylate, methyl methacrylate, and graphene into the reaction kettle, stirring and mixing at a speed of 550 r / min for 20 min to obtain a base liquid;

[0161] (2) adding the initiator to xylene, stirring and mixing at a speed of 500 r / min to obtain an initiator solution;

[0162] (3) The prepared initiator solution is added dropwise into the reactor, and then the mixture is stirred and reacted at 80° C. for 2 hours. A portion of the xylene is first removed by atmospheric distillation, and then the remaining xylene is removed by reduced pressure distillation. Finally, the mixture is crushed and then sieved through a 500-mesh sieve to obtain a high-gloss additive.

[0163] Graphene is pre-modified:

[0164] Add graphene and maleic anhydride to the nitric acid solution, adjust the temperature to 60°C, keep warm and stir for 15 minutes, then adjust the temperature to 85°C, continue to keep warm and stir for 20 minutes, then filter, wash with water to neutrality, and dry to constant weight to obtain preliminary graphene;

[0165] The preliminary graphene and cerium chloride obtained above were mixed evenly in a mass ratio of 1000:1, and then plasma treated for 1 hour under a nitrogen atmosphere at a power of 300 W, and then discharged, washed with a 50% ethanol solution by mass, and then filtered and dried to constant weight to complete the treatment;

[0166] Among them, the mixing mass ratio of graphene, maleic anhydride and nitric acid solution is 1:3:10;

[0167] The mass fraction of the nitric acid solution is 12%;

[0168] Among them, the drying temperature is 60°C and the drying time is 40 minutes.

[0169] The mixed mass ratio of xylene, butyl acrylate, methyl methacrylate and graphene is 30:8:6:0.8;

[0170] The initiator is dibenzoyl peroxide;

[0171] The mass fraction of the initiator solution is 5%;

[0172] The mass ratio of the initiator solution to the base liquid is 1:6; the filler is a mixture of titanium dioxide and calcium carbonate;

[0173] Among them, the mixing mass ratio of titanium dioxide and calcium carbonate is 1:8.

[0174] A method for preparing a black high-gloss polyester powder coating comprises the following steps:

[0175] S1. First, a polyester resin, a curing agent, carbon black, a high gloss agent, a filler, an antioxidant, and a leveling agent are added to a mixer and stirred for 15 minutes to obtain a mixture;

[0176] High-speed mixing speed is 800r / min;

[0177] S2. The mixture obtained above is then added to a dryer for drying;

[0178] Among them, the drying temperature is 60°C and the drying time is 2 hours;

[0179] S3. The dried mixture is added to a twin-screw extruder and melt-extruded;

[0180] S4. After the melt is extruded through a twin-screw extruder, it is transported to a tablet press for tableting to obtain a sheet, and then the sheet is crushed and sieved to obtain a finished black high-gloss polyester powder coating;

[0181] Among them, the average particle size of the black high-gloss polyester powder coating is 30μm.

[0182] Comparative Example 1:

[0183] The difference from Example 1 is that no high gloss auxiliary agent is added, and the rest of the technical solutions remain unchanged.

[0184] test:

[0185] Test Method

[0186] The coatings of the embodiment and the comparative example were sprayed onto the surface of the glass plate (10 in each group, taking the average value), with the thickness difference not exceeding 0.05 mm. After being cured under the same conditions, the glossiness of the coating was measured according to ISO 2813:

[0187] Table 1

[0188]

[0189]

[0190] It can be seen from Table 1 that the powder coating prepared by the present invention has a higher gloss after curing.

[0191] The test was continued by exposing the coated glass plates (ten per group, average value) to the strong light of a xenon lamp. The gloss was measured 2000 hours after the start of exposure to the xenon lamp.

[0192] Gloss retention = (gloss after test) / (gloss before test) × 100%:

[0193] Table 2

[0194] Gloss retention % Example 1 98 Example 2 98 Example 3 99 Example 4 98 Example 5 96 Comparative Example 1 58

[0195] It can be seen from Table 2 that the coating formed by the powder coating prepared in the present invention has relatively poor gloss retention.

[0196] Continue the test, take Example 1 as the basic sample, and compare the effect of different xenon lamp irradiation time on the gloss retention of the coating:

[0197] Table 3

[0198] Time / h Gloss retention % 0 100 1000 100 2000 98 4000 92 6000 88 8000 73

[0199] It can be seen from Table 3 that the light retention of the coating formed by the coating of the present invention gradually decreases as the strong light exposure time increases.

[0200] The above description is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown. Any changes made in accordance with the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the specification, should be within the protection scope of the present invention.

Claims

1. A black high-gloss polyester powder coating, characterized in that: The following ingredients are included by weight: 85-94 parts of polyester resin, 6-8 parts of curing agent, 2-3.2 parts of carbon black, 0.5-0.8 parts of high gloss additive, 23-25 ​​parts of filler, 0.8-1.2 parts of antioxidant, and 1-2 parts of leveling agent; Among them, the mixing mass ratio of carbon black and high gloss additive is 4:1; Wherein, the polyester resin used is unsaturated polyester resin.

2. The black high-gloss polyester powder coating according to claim 1, characterized in that: The preparation method of the high gloss auxiliary agent is: (1) adding an organic solvent into a reaction kettle, and then sequentially adding butyl acrylate, methyl methacrylate, and graphene into the reaction kettle, stirring and mixing at a speed of 550 r / min for 20 min to obtain a base liquid; (2) adding the initiator to the organic solvent, stirring and mixing at a speed of 500 r / min to obtain an initiator solution; (3) The prepared initiator solution is added dropwise into the reaction kettle, and then the mixture is stirred and reacted at 80° C. for 2 hours. A portion of the organic solvent is first removed by atmospheric distillation, and then the remaining organic solvent is removed by reduced pressure distillation. Finally, the mixture is crushed and then sieved through a 500-mesh sieve to obtain a high-gloss additive.

3. The black high-gloss polyester powder coating according to claim 2, characterized in that: The graphene is pre-modified by adding graphene and maleic anhydride to a nitric acid solution, adjusting the temperature to 60° C., stirring for 15 minutes, then adjusting the temperature to 85° C., stirring for 20 minutes, then filtering, washing with water to neutrality, and drying to constant weight to obtain preliminary graphene; The preliminary graphene and cerium chloride obtained above were mixed evenly in a mass ratio of 1000:1, and then plasma treated for 1 hour under a nitrogen atmosphere at a power of 300 W, and then discharged, washed with a 50% ethanol solution by mass, and then filtered and dried to constant weight to complete the treatment; Among them, the mixing mass ratio of graphene, maleic anhydride and nitric acid solution is 1:3:10; The mass fraction of the nitric acid solution is 12%; Among them, the drying temperature is 60°C and the drying time is 40 minutes.

4. The black high-gloss polyester powder coating according to claim 2, characterized in that: The organic solvent is xylene; The mixing mass ratio of xylene, butyl acrylate, methyl methacrylate and graphene is 30:5-8:4-6:0.6-0.8; The initiator is dibenzoyl peroxide; The mass fraction of the initiator solution is 5%; The mixing mass ratio of the initiator solution to the base liquid is 1:5-6.

5. The black high-gloss polyester powder coating according to claim 1, characterized in that: The curing agent is diaminophenyl sulfone.

6. The black high-gloss polyester powder coating according to claim 1, characterized in that: The filler is a mixture of titanium dioxide and calcium carbonate; Among them, the mixing mass ratio of titanium dioxide and calcium carbonate is 1:

8.

7. The black high-gloss polyester powder coating according to claim 1, characterized in that: The antioxidant is antioxidant 1010.

8. The black high-gloss polyester powder coating according to claim 1, characterized in that: The leveling agent is polyacrylate.

9. The method for preparing a black high-gloss polyester powder coating according to claim 1, characterized in that: The following steps are involved: S1. First, a polyester resin, a curing agent, carbon black, a high gloss agent, a filler, an antioxidant, and a leveling agent are added to a mixer and stirred for 15 minutes to obtain a mixture; High-speed mixing speed is 800r / min; S2. The mixture obtained above is then added to a dryer for drying; Among them, the drying temperature is 60°C and the drying time is 2 hours; S3. The dried mixture is added to a twin-screw extruder and melt-extruded; S4. After the melt is extruded through a twin-screw extruder, it is transported to a tablet press for tableting to obtain a sheet, and then the sheet is crushed and sieved to obtain a finished black high-gloss polyester powder coating; Among them, the average particle size of the black high-gloss polyester powder coating is 30μm.

Citation Information

Patent Citations

  • Fast-curing polyester powder coating and preparation method thereof

    CN110229591A

  • Ultrahigh-gloss black plastic powder coating and preparation method thereof

    CN110669428A

  • Black high-gloss powder coating for coating automobile hub

    CN111690311A

  • Weather-resistant highlight powder coating composition and coating thereof

    CN112745746A