Controllable hybrid LPSO phase reinforced magnesium-based composite material and preparation method thereof

By adopting a controllable hybrid LPSO phase enhancement method in magnesium-based composite materials, the problems of uneven distribution and oxidation of LPSO precipitation phases in traditional casting methods are solved, and the high strength, plasticity and elastic modulus of magnesium-based composite materials are realized. promote.

CN118755980BActive Publication Date: 2024-11-29GUANGDONG INST OF NEW MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411252772.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-29
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

In the magnesium-based composite materials prepared by traditional casting methods, the distribution of the LPSO precipitation phase is uneven, which affects the toughness and mechanical properties of the composite material, and is prone to oxidation at high temperatures, resulting in a decrease in mechanical properties.

Method used

Using a controlled method of preparing a magnesium-based composite material with a controlled hybrid LPSO phase reinforced magnesium-based composite material, the magnesium-rare earth alloy matrix, transition metal powder and nanometal reinforced particle powder are mixed in a specific proportion, and high-energy ball mill and low-energy ball mill are followed by sintering. and thermal extrusion deformation, regulating the volume fraction, orientation and type of LPSO phase.

Benefits of technology

The uniform distribution and controllability of the LPSO phase in magnesium-based composite materials are achieved, the tensile strength, yield strength, elongation and elastic modulus of the composite materials are improved, the oxidation phenomenon is reduced, and the mechanical properties are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755980B_ABST
    Figure CN118755980B_ABST
Patent Text Reader

Abstract

The invention discloses a controllable hybrid LPSO phase-enhanced magnesium-based composite material and a preparation method thereof, and belongs to the technical field of magnesium-based composite materials. The raw materials for preparing the magnesium-based composite material include a magnesium-rare earth alloy matrix, a transition metal powder and a nano-metal-enhanced particle powder; the mass ratio of the transition metal powder to the matrix is ​​1:99 to 3:97; the ratio of the nano-metal-enhanced particle powder to the total mass of the magnesium-rare earth alloy matrix and the transition metal powder is 1:99 to 3:97, and the content of rare earth elements in the matrix is ​​8wt% to 15wt%; in the composite material, the volume of the hybrid LPSO phase in the crystal accounts for 10% to 50% of the magnesium-based composite material, and there are discontinuously distributed nano-metal-enhanced particles at the grain boundaries. The magnesium-based composite material has high tensile strength, yield strength, elongation and elastic modulus. Its preparation method is simple to operate, low in cost, and can be industrially produced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnesium-based composite materials, and in particular to a controllable hybrid LPSO phase-reinforced magnesium-based composite material and a preparation method thereof. Background Art

[0002] Among many metal matrices, magnesium-transition metal-rare earth alloy is considered to be a matrix that can be used to prepare high-strength and tough magnesium-based composite materials. However, the traditional casting method is usually used to prepare magnesium-based composite materials. The resulting composite materials are prone to have a network of bulk LPSO precipitation phases distributed on the grain boundaries, which hinders the transfer of loads on the interface and affects the toughness of the composite materials. The needle-like LPSO phases in the crystals are arranged in parallel and have obvious preferential orientation, which makes the texture orientation of the composite materials obvious, affecting the practical application of the composite materials. At the same time, the casting method is carried out at a relatively high temperature, which easily leads to severe oxidation of magnesium, rare earth and transition elements in the high-temperature liquid phase, affecting the mechanical properties of the composite materials. Even if measures such as condition optimization and post-treatment are attempted, the improvement of the comprehensive mechanical properties of the composite materials is relatively limited.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The object of the present invention is to provide a controllable hybrid LPSO phase reinforced magnesium-based composite material and a preparation method thereof, so as to solve or improve the above technical problems.

[0005] The present invention can be implemented like this:

[0006] In a first aspect, the present invention provides a controllable hybrid LPSO phase-reinforced magnesium-based composite material, wherein the raw materials for preparing the hybrid LPSO phase-reinforced magnesium-based composite material include a magnesium-rare earth alloy matrix, a transition metal powder and a nano-metal reinforcement particle powder;

[0007] The ratio of the mass of the transition metal powder to the mass of the magnesium-rare earth alloy matrix is ​​1:99 to 3:97, and the ratio of the mass of the nano-metal reinforced particle powder to the total mass of the magnesium-rare earth alloy matrix and the transition metal powder is 1:99 to 3:97; the content of the rare earth element in the magnesium-rare earth alloy matrix is ​​8wt% to 15wt%;

[0008] In the hybrid LPSO phase reinforced magnesium-based composites, the volume of the hybrid LPSO phase in the crystal accounts for 10%~50% of the hybrid LPSO phase reinforced magnesium-based composites. The types of hybrid LPSO phases in the crystal include lamellar 18R type and needle-shaped 14H type, and there are discontinuously distributed nano-metal reinforcement particles on the grain boundary interface; and, with the increase of the mass ratio of transition metal elements to rare earth elements in the preparation raw materials, the total volume fraction of the hybrid LPSO phase also increases accordingly. The hybrid LPSO phase changes from being dominated by the 14H type LPSO phase at the beginning to being dominated by the 18R type LPSO phase in the end.

[0009] In an optional embodiment, the rare earth element in the magnesium-rare earth alloy matrix includes at least one of Gd, Y, Tb, Dy, Ho and Er;

[0010] and / or, the transition metal in the transition metal powder includes at least one of Zn, Al and Cu;

[0011] And / or, the metal in the nano metal reinforcement particle powder is a metal that is not soluble in the magnesium matrix.

[0012] In an optional embodiment, the average particle size of the magnesium-rare earth alloy matrix is ​​60 μm to 100 μm;

[0013] and / or, the average particle size of the transition metal powder is 500 nm to 2 μm;

[0014] And / or, the average particle size of the nano metal reinforcement particle powder is 50nm~200nm.

[0015] In an optional embodiment, the hybrid LPSO phase reinforced magnesium-based composite material further has at least one of the following characteristics:

[0016] Feature 1: With the increase of the mass ratio of transition metal elements to rare earth elements in the raw materials, the distribution of the mixed LPSO phase gradually grows from the position near the grain boundary in the crystal to the center, and the orientation of the mixed LPSO phase presents a wheel-shaped distribution until it fills the entire crystal, and then the mixed LPSO phase coarsens and grows;

[0017] Feature 2: The average grain size of the hybrid LPSO phase reinforced magnesium matrix composite material does not exceed 2 μm;

[0018] Feature 3: The tensile strength of the hybrid LPSO phase reinforced magnesium-based composite material is not less than 400MPa;

[0019] Feature 4: The yield strength of the hybrid LPSO phase reinforced magnesium-based composite material is not less than 380MPa;

[0020] Feature 5: The elongation of the hybrid LPSO phase reinforced magnesium matrix composite material is not less than 12%;

[0021] Feature 6: The elastic modulus of the hybrid LPSO phase reinforced magnesium-based composite material is not less than 50 GPa.

[0022] In a second aspect, the present invention provides a method for preparing a controllable hybrid LPSO phase reinforced magnesium-based composite material as described in any of the aforementioned embodiments, comprising the following steps: mixing a magnesium-rare earth alloy matrix with a transition metal powder and performing high-energy ball milling to obtain a high-energy ball mill material; mixing the high-energy ball mill material with a nano-metal reinforced particle powder and performing low-energy ball milling to obtain a low-energy ball mill material; and sintering and hot extrusion deforming the low-energy ball mill material.

[0023] In an optional embodiment, the high energy ball milling has at least one of the following characteristics:

[0024] Feature 7: The speed of high energy ball mill is 200r / min~300r / min;

[0025] Feature 8: The ball-to-material ratio of high-energy ball milling is 20:1 to 30:1 by mass;

[0026] Feature 9: High energy ball milling time is 2h~4h.

[0027] In an optional embodiment, the low energy ball milling has at least one of the following characteristics:

[0028] Feature 10: The speed of low-energy ball mill is 100r / min~120r / min;

[0029] Feature 11: The ball-to-material ratio of low-energy ball milling is 10:1 to 20:1 by mass;

[0030] Feature 12: The time of low-energy ball milling is 1h~2h.

[0031] In an optional embodiment, the sintering has at least one of the following characteristics:

[0032] Feature 13: The sintering temperature is 480℃~500℃;

[0033] Feature 14: The sintering pressure is 30MPa~50MPa;

[0034] Feature 15: The sintering time is 5min~10min;

[0035] Feature 16: After sintering, water cooling is performed first and then hot extrusion deformation is performed.

[0036] In an optional embodiment, the hot extrusion deformation has at least one of the following characteristics:

[0037] Feature 17: The temperature of hot extrusion deformation is 380℃~400℃;

[0038] Feature 18: The extrusion ratio of hot extrusion deformation is 20:1 to 30:1;

[0039] Feature 19: The speed of hot extrusion deformation is 0.3m / min~0.5m / min.

[0040] In an optional embodiment, before mixing the magnesium-rare earth alloy matrix with the transition metal powder, the transition metal powder is first dispersed by vibration; before mixing the high energy ball mill material with the nano metal reinforced particle powder, the nano metal reinforced particle powder is first dispersed by vibration;

[0041] The frequency of vibration dispersion is 10Hz~30Hz, and the time of vibration dispersion is 0.5h~1h.

[0042] The beneficial effects of the present invention include:

[0043] The magnesium-based composite material proposed by the present invention is prepared by mixing a magnesium-rare earth alloy matrix, a transition metal powder and a nano-metal reinforcement particle powder according to a specific ratio, so that the volume proportion of the mixed LPSO phase in the crystal of the magnesium-based composite material is adjustable in the range of 10% to 50%, the mixed LPSO phase types in the crystal include lamellar 18R type and needle-shaped 14H type, and discontinuously distributed nano-metal reinforcement particles exist at the grain boundary; and, as the mass ratio of the transition metal element to the rare earth element in the preparation raw material increases, the total volume fraction of the mixed LPSO phase also increases accordingly, and the mixed LPSO phase is mainly composed of the 14H type LPSO phase at the beginning and becomes mainly composed of the 18R type LPSO phase at the end.

[0044] The tensile strength, yield strength and elastic modulus of the hybrid LPSO phase are higher than those of the magnesium matrix, which helps it to play the role of an excellent reinforcement phase. In addition, the LPSO phase can act as a heterogeneous nucleation site to promote the occurrence of dynamic recrystallization and hinder the movement of the grain boundaries of the recrystallized grains. The final effect is to significantly refine the grains to the nanocrystalline level. Moreover, the LPSO phase can hinder<c+a> The movement of dislocations presents a large-scale twisted shape during deformation, which increases the storage energy of the composite material and helps improve the mechanical properties. In addition, excess rare earth metal elements can be dissolved into the magnesium matrix, reducing the critical shear stress of basal and non-basal slip, promoting the activation of non-basal slip systems, and helping to improve plasticity. In addition, with the increase in the mass ratio of transition metal elements to rare earth elements, the volume share of the LPSO phase increases significantly.

[0045] That is, the kink strengthening, precipitation strengthening and pinning dislocation strengthening mechanism of LPSO phase itself and the grain boundary strengthening of Ti particles can improve the strength of magnesium-based composites; the good interface bonding of LPSO phase and the cone surface stimulated by the solid solution of rare earth elements and<a+c> The activation of the slip system can ensure that the ductility of the magnesium-based composite material is not lost; the strengthening effect of the LPSO phase itself can increase the elastic modulus of the magnesium-based composite material.

[0046] Therefore, the magnesium-based composite material provided by the present invention can simultaneously have high tensile strength, yield strength, elongation and elastic modulus. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0048] Figure 1This is a cross-sectional morphology diagram of the magnesium-based composite material prepared in Example 4;

[0049] Figure 2 This is a longitudinal cross-sectional morphology diagram of the magnesium-based composite material prepared in Example 4;

[0050] Figure 3 This is a phase morphology of 14H-LPSO in the magnesium-based composite material prepared in Example 4;

[0051] Figure 4 This is a phase morphology of 18R-LPSO in the magnesium-based composite material prepared in Example 4;

[0052] Figure 5 The high-density dislocation diagram of the magnesium-based composite material prepared in Example 4;

[0053] Figure 6 for Figure 5 A magnified image of

[0054] Figure 7 This is a dynamic recrystallized grain diagram of the magnesium-based composite material prepared in Example 4;

[0055] Figure 8 This is a cross-sectional morphology diagram of the magnesium-based composite material prepared in Example 1;

[0056] Fig. 9 This is a longitudinal cross-sectional morphology diagram of the magnesium-based composite material prepared in Example 1;

[0057] Fig.10 This is a cross-sectional morphology diagram of the magnesium-based composite material prepared in Example 5;

[0058] Fig.11 This is a longitudinal cross-sectional morphology diagram of the magnesium-based composite material prepared in Example 5;

[0059] Fig.12 This is a cross-sectional morphology of the Mg10Y alloy without LPSO phase reinforcement prepared in Comparative Example 1;

[0060] Fig.13 This is the longitudinal cross-sectional morphology of the Mg10Y alloy without LPSO phase reinforcement prepared in Comparative Example 1. DETAILED DESCRIPTION

[0061] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0062] The controllable hybrid LPSO phase reinforced magnesium-based composite material and the preparation method thereof provided by the present invention are described in detail below.

[0063] The invention provides a controllable hybrid LPSO phase reinforced magnesium-based composite material. The raw materials for preparing the hybrid LPSO phase reinforced magnesium-based composite material include a magnesium-rare earth alloy matrix, transition metal powder and nano-metal reinforcement particle powder.

[0064] Among them, the mixed LPSO phase types include the lamellar 18R-type LPSO phase (referred to as "18R-LPSO phase") and the needle-shaped 14H-type LPSO phase (referred to as "14H-LPSO phase").

[0065] Magnesium, transition metals and rare earth elements can form a long-period stacking phase that is coherent with the matrix, which is beneficial to improving mechanical properties; rare earth elements have a large solid solubility in the magnesium matrix, and the atomic radius of rare earth elements and magnesium elements is quite different. The solid solution of rare earth elements can cause serious lattice distortion in the magnesium matrix, and the equilibrium solubility will decrease exponentially with the decrease in temperature, which has a significant precipitation strengthening effect. Moreover, rare earth elements can reduce the critical shear stress difference between basal slip and non-basal slip, stimulate the activation of non-basal slip systems, and significantly improve the plasticity of composite materials.

[0066] In some optional embodiments, the rare earth elements in the magnesium-rare earth alloy matrix may include at least one of Gd, Y, Tb, Dy, Ho and Er. In the magnesium-rare earth alloy matrix, the content of rare earth elements may be 8wt%~15wt%, such as 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%, etc., or other values ​​within the range of 8wt%~15wt%. In some preferred embodiments, the rare earth element content in the magnesium-rare earth alloy matrix is ​​9wt%~12wt%; in some more preferred embodiments, the rare earth element content in the magnesium-rare earth alloy matrix is ​​8wt%.

[0067] If the content of rare earth elements in the magnesium-rare earth alloy matrix is ​​less than 8wt%, it is not easy to form LPSO phase; if the content of rare earth elements in the magnesium-rare earth alloy matrix is ​​greater than 15wt%, it will not only increase the cost but also easily form brittle phases (such as Mg2Y, etc.) and precipitate.

[0068] In some optional embodiments, the transition metal in the transition metal powder may include at least one of Zn, Al and Cu. The ratio of the mass of the transition metal powder to the mass of the magnesium-rare earth alloy matrix is ​​1:99 to 3:97, such as 1:99, 1.5:98.5, 2:98, 2.5:97.5 or 3:97, etc., and may also be other values ​​within the range of 1:99 to 3:97. In some preferred embodiments, the ratio of the mass of the transition metal powder to the mass of the magnesium-rare earth alloy matrix is ​​2:98.

[0069] If the amount of transition metal powder is too low, LPSO is not easily generated; if the amount of transition metal powder is too high, brittle alloy compounds (such as Mg-Zn, etc.) are easily formed.

[0070] In some optional embodiments, the metal in the nano-metal reinforced particle powder is a metal that is not soluble in the magnesium matrix, for example, by way of example but not limitation, it may include at least one of Ti, Zr, Nb, Cr, Mo and Mn, etc. The ratio of the mass of the nano-metal reinforced particle powder to the total mass of the magnesium-rare earth alloy matrix and the transition metal powder is 1:99 to 3:97, such as 1:99, 1.5:98.5, 2:98, 2.5:97.5 or 3:97, etc., and may also be other values ​​within the range of 1:99 to 3:97.

[0071] If the dosage of nano-metal reinforced particle powder is too high, it will be detrimental to the uniform distribution of the nano-metal reinforced particle powder, and the excessive nano-metal reinforced particle powder will easily agglomerate at the phase boundary, which is not conducive to the strong interface bonding between the reinforced particles and the matrix, and the material plasticity is poor; if the dosage of nano-metal reinforced particle powder is too low, the grain boundary strengthening effect is not significant.

[0072] As mentioned above, by limiting the content of rare earth elements and transition metal powders within the above range, it is possible to ensure the formation of a certain volume fraction of LPSO reinforcement phase to improve strength, while the remaining rare earth elements can be dissolved into the magnesium alloy matrix to improve plasticity and achieve the effect of grain refinement. By controlling the amount of nano-metal reinforcement particle powder within the above range, on the one hand, it is possible to avoid excessive nano-metal reinforcement particle powder, which makes it easy to agglomerate and distribute at the interface, affecting interface bonding, and on the other hand, it is possible to avoid too little nano-metal reinforcement particle powder, which leads to failure to strengthen the grain boundaries.

[0073] In addition, taking the nano-metal reinforced particle powder as Zn particle powder and the rare earth in the magnesium-rare earth alloy matrix as Y as an example, if the amount of Zn particle powder is too little, it will not be easy to generate LPSO phase; if the amount of Zn particle powder is too much, it is easy to form Mg-Zn brittle alloy compounds. If the Y element in the magnesium-rare earth alloy matrix is ​​too little, the volume fraction of LPSO phase will be small, and the Y element existing in the form of solid solution will be even less; if the Y element in the magnesium-rare earth alloy matrix is ​​too much, the proportion of 14H-LPSO phase refined in the grain will be greatly reduced, and the size and number of 18R-LPSO phase will increase significantly.

[0074] In some optional embodiments, the average particle size of the magnesium-rare earth alloy matrix can be 60 μm to 100 μm, such as 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm or 100 μm, etc., or other values ​​within the range of 60 μm to 100 μm. In some preferred embodiments, the average particle size of the magnesium-rare earth alloy matrix can be 75 μm to 85 μm. In some more preferred embodiments, the average particle size of the magnesium-rare earth alloy matrix is ​​80 μm.

[0075] If the average particle size of the magnesium-rare earth alloy matrix is ​​less than 60μm, due to the high activity of the magnesium alloy powder, the material is not only easily oxidized during the preparation process, but also there are safety risks, which is not conducive to industrial production. If the average particle size of the magnesium-rare earth alloy matrix is ​​greater than 100μm, the pores between the particles are large, which is not conducive to sintering density, affecting the density and final mechanical properties of the composite material.

[0076] In some optional embodiments, the average particle size of the transition metal powder may be 500 nm to 2 μm, such as 500 nm, 700 nm, 900 nm, 1 μm or 2 μm, or may be other values ​​within the range of 500 nm to 2 μm.

[0077] The finer the transition metal powder, the larger the specific surface area, the more active atoms on the surface, and the easier it is for the surface to diffuse. The transition metal powder with an average particle size of 500nm to 2μm used in the present invention has a high activity, is evenly distributed on the surface of the matrix, can promote alloying reaction with magnesium-rare earth alloy, and is conducive to the formation of LPSO phase. If the average particle size of the transition metal powder exceeds 2μm, the activity will decrease, and the gaps between particles will be large, and the reaction in the solid state is not conducive to the formation of a dense composite material.

[0078] In some optional embodiments, the average particle size of the nano metal reinforcement particle powder may be 50 nm to 200 nm, such as 50 nm, 100 nm, 150 nm or 200 nm, or may be other values ​​within the range of 50 nm to 200 nm.

[0079] Nano-metal reinforced particle powder is mainly distributed on the interface, playing a role in grain boundary strengthening. If the average particle size of the nano-powder is small, the specific surface energy is high, and the powder is easy to agglomerate and adsorb, which is not conducive to uniform dispersion. If the average particle size of the nano-powder is large, the interface bonding between the particles and the matrix is ​​affected, resulting in a significant decrease in the plasticity of the composite material.

[0080] In the present invention, the mixed LPSO phase mainly exists in the crystal of the magnesium-based composite material, and the volume of the mixed LPSO phase in the crystal accounts for 10% to 50% of the mixed LPSO phase reinforced magnesium-based composite material, such as 10%, 20%, 30%, 40% or 50%, etc., and can also be other values ​​within the range of 10% to 50%. Specifically, the volume of the mixed LPSO phase in the crystal can be adjusted within 10% to 50% by adjusting the preparation process parameters. The mixed LPSO phase in the crystal includes 18R-LPSO phase and 14H-LPSO phase. There are discontinuously distributed nano-metal reinforcement particles at the grain boundary; and, as the mass ratio of transition metal elements to rare earth elements in the preparation raw materials increases, the total volume fraction of the mixed LPSO phase also increases, and the mixed LPSO phase is mainly 14H-type LPSO phase at the beginning, and finally becomes mainly 18R-type LPSO phase.

[0081] In addition, with the increase of the mass ratio of transition metal elements to rare earth elements in the preparation raw materials, the distribution of the mixed LPSO phase gradually grows from the position near the grain boundary in the crystal to the center, and the orientation of the mixed LPSO phase presents a wheel-shaped distribution until it fills the entire crystal, and then the mixed LPSO phase coarsens and grows.

[0082] In some optional embodiments, the average grain size of the controllable hybrid LPSO phase reinforced magnesium-based composite material does not exceed 2 μm, such as 0.7 μm to 1.2 μm, such as 0.79 μm, 0.80 μm, 0.88 μm, 0.92 μm, 0.98 μm, 1.01 μm, 1.05 μm, 1.09 μm or 1.13 μm, etc.

[0083] The magnesium-based composite material with the above average grain size has fine grains, a large number of grain boundaries, and greater resistance when dislocations move, which is conducive to enhancing the plastic deformation resistance of the magnesium alloy. In addition, the more grains there are, the more metal plastic deformation can be dispersed inside the grains, and the grain boundaries hinder the expansion of cracks, thereby improving the storage energy of the composite material.

[0084] In some optional embodiments, the tensile strength of the hybrid LPSO phase reinforced magnesium-based composite material is not less than 400 MPa, such as 400 MPa-420 MPa, such as 400 MPa, 401 MPa, 407 MPa, 411 MPa, 412 MPa, 414 MPa, 415 MPa, 418 MPa or 420 MPa.

[0085] In some optional embodiments, the yield strength of the hybrid LPSO phase reinforced magnesium-based composite material is not less than 380 MPa, such as 380 MPa~400 MPa, such as 385 MPa, 387 MPa, 390 MPa, 391 MPa, 393 MPa, 395 MPa, 398 MPa or 399 MPa.

[0086] In some optional embodiments, the elongation of the hybrid LPSO phase reinforced magnesium-based composite material is not less than 12%, such as 12% to 15%, such as 12%, 12.5%, 13%, 13.5%, 14% or 15%.

[0087] In some optional embodiments, the elastic modulus of the hybrid LPSO phase reinforced magnesium-based composite material is not less than 50 GPa, such as 50 GPa to 60 GPa, such as 50 GPa, 52 GPa, 53 GPa, 54 GPa, 55 GPa, 56 GPa, 58 GPa or 60 GPa.

[0088] As mentioned above, the magnesium-based composite material proposed in the present invention can be in-situ controllably regulated to form a mixed long-period stacking phase of 18R and 14H within the crystal by using a method of powder metallurgy combined with hot extrusion, and there are discontinuously distributed nano-metal reinforcement particles on the interface. The volume fraction, orientation, and 18R and 14H type ratios of the intracrystalline LPSO phase all change regularly with the change in the mass ratio of transition metal elements to rare earth elements. First, the LPSO phase is coherent with the magnesium matrix, and its own tensile strength, yield strength, and elastic modulus are higher than those of the magnesium matrix, which helps to play the role of an excellent reinforcement phase, especially the nanoscale effect is significant. Secondly, the LPSO phase can act as a heterogeneous nucleation site to promote the occurrence of dynamic recrystallization, and can also hinder the movement of the grain boundaries of recrystallized grains. The final effect is to significantly refine the grains to the nanocrystalline level. Moreover, the LPSO phase can hinder<c+a> The movement of dislocations presents a large-scale twisted shape during deformation, which increases the storage energy of the composite material and helps improve the mechanical properties. Finally, rare earth metal elements can be dissolved into the magnesium matrix, reduce the critical shear stress of basal and non-basal slip, promote the activation of non-basal slip systems, and help improve plasticity.

[0089] Moreover, with the increase of the mass ratio of transition metal elements to rare earth elements, the volume proportion of LPSO phase increases significantly. Fine structure analysis found that with the increase of the mass ratio of transition metal elements to rare earth elements, the overall volume fraction of 14H-type LPSO phase gradually decreases, and the overall volume fraction of 18R-type LPSO phase increases significantly, from the beginning of 14H-type LPSO phase to the end of 18R-type LPSO phase, and the texture characteristics are significantly weakened.

[0090] The controllable hybrid LPSO phase reinforced magnesium-based composite material provided by the present invention can simultaneously have high tensile strength, yield strength, elongation and elastic modulus. Among them, the improvement of strength is mainly attributed to the kink strengthening, precipitation strengthening and pinning dislocation strengthening mechanism of the LPSO phase itself and the grain boundary strengthening of Ti particles; the non-loss of ductility is mainly due to the fine grain strengthening, good interface bonding of the LPSO phase and the cone surface stimulated by the solid solution of rare earth metal elements. and<a+c> The slip system is activated; the increase in the elastic modulus mainly comes from the strengthening effect of the LPSO phase itself.

[0091] It should be noted that the 18R-LPSO phase prepared by the traditional casting method tends to form a coarse continuous network distribution at the grain boundary, which hinders the movement of dislocations and grain boundaries. The needle-shaped 14R-LPSO is distributed in the crystal and still presents a parallel directional arrangement, resulting in a significant texture orientation of the composite material, which is not conducive to the preparation of isotropic materials. More importantly, the size, distribution and type of LPSO in the composite material prepared by the casting method are difficult to finely control. Secondly, magnesium, rare earths and transition elements are easily severely oxidized during high-temperature casting, which seriously affects the mechanical properties of the cast composite material. Even though a large number of measures including casting preparation method optimization and post-processing have been applied to solve the above problems, the improvement of comprehensive mechanical properties is still very limited.

[0092] Based on this, the present invention also provides a method for preparing a controllable hybrid LPSO phase-reinforced magnesium-based composite material, comprising the following steps: mixing a magnesium-rare earth alloy matrix with a transition metal powder and performing high-energy ball milling to obtain a high-energy ball mill material; mixing the high-energy ball mill material with a nano-metal reinforced particle powder and performing low-energy ball milling to obtain a low-energy ball mill material; and sintering and hot extrusion deforming the low-energy ball mill material.

[0093] In some embodiments, the rotation speed of the high energy ball mill can be 200 r / min to 300 r / min, such as 200 r / min, 220 r / min, 250 r / min, 280 r / min or 300 r / min, or other values ​​within the range of 200 r / min to 300 r / min.

[0094] The ball-to-material ratio of the high energy ball mill can be 20:1 to 30:1 by mass, such as 20:1, 25:1 or 30:1, etc., or other values ​​within the range of 20:1 to 30:1.

[0095] The high energy ball milling time can be 2 h to 4 h, such as 2 h, 2.5 h, 3 h, 3.5 h or 4 h, etc., or other values ​​within the range of 2 h to 4 h.

[0096] High-energy ball milling can promote the alloying of transition metal elements, magnesium and rare earth elements to form a high volume fraction, nanoscale, wheel-shaped LPSO phase.

[0097] In some embodiments, the rotation speed of the low-energy ball mill can be 100 r / min~120 r / min, such as 100 r / min, 105 r / min, 110 r / min, 115 r / min or 120 r / min, or other values ​​within the range of 100 r / min~120 r / min.

[0098] The ball-to-material ratio of the low-energy ball mill can be 10:1 to 20:1 by mass, such as 10:1, 15:1 or 20:1, or other values ​​within the range of 10:1 to 20:1.

[0099] The time of low-energy ball milling can be 1 h to 2 h, such as 1 h, 1.5 h or 2 h, or other values ​​within the range of 1 h to 2 h.

[0100] Low-energy ball milling helps to evenly and discontinuously distribute nano-reinforced particles on the alloy surface, maximizing the interface strengthening effect.

[0101] If the magnesium-rare earth alloy matrix, transition metal powder and nano-metal reinforced particle powder are directly mixed at one time and subjected to high-energy ball milling, the nano-metal particles are easily directly alloyed with the transition metal particles to form a brittle second phase, affecting the microstructure and properties of the composite material; if the magnesium-rare earth alloy matrix, transition metal powder and nano-metal reinforced particle powder are directly mixed at one time and subjected to low-energy ball milling, it is not conducive to the in-situ precipitation of the LPSO phase in the crystal, and is not conducive to the controllable preparation of composite materials with characteristic structures.

[0102] In some embodiments, sintering may be performed using spark plasma sintering.

[0103] The sintering temperature may be 480°C to 500°C, such as 480°C, 485°C, 490°C, 495°C or 500°C, or other values ​​within the range of 480°C to 500°C.

[0104] When using spark plasma sintering powder, at a sintering temperature below 480°C, many holes or defects can be observed in the sintered blank, and the material density is poor; above 500°C, the magnesium alloy powder reaches the melting point and melts into liquid, which is not conducive to the material's formability.

[0105] The sintering pressure may be 30 MPa to 50 MPa, such as 30 MPa, 35 MPa, 40 MPa, 45 MPa or 50 MPa, or other values ​​within the range of 30 MPa to 50 MPa.

[0106] The sintering time may be 5 min to 10 min, such as 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, etc., or may be other values ​​within the range of 5 min to 10 min.

[0107] If the sintering time is too long, the grain structure will grow too coarse; if the sintering time is too short, the interface reaction and diffusion between the powder particles will be weak, which is not conducive to the diffusion of magnesium, transition metals, and rare earth elements to form LPSO phase.

[0108] After sintering, water cooling is performed first and then hot extrusion deformation is performed. The cooling rate can be 1°C / min~3°C / min, such as 1°C / min, 2°C / min or 3°C / min.

[0109] In some embodiments, the temperature of hot extrusion deformation may be 380°C to 400°C, such as 380°C, 385°C, 390°C, 395°C or 400°C, or other values ​​within the range of 380°C to 400°C.

[0110] The extrusion ratio of the hot extrusion deformation can be 20:1 to 30:1, such as 20:1, 22:1, 25:1, 28:1 or 30:1, or other values ​​within the range of 20:1 to 30:1.

[0111] The speed of hot extrusion deformation can be 0.3m / min~0.5m / min, such as 0.3m / min, 0.35m / min, 0.4m / min, 0.45m / min or 0.5m / min, etc., and can also be other values ​​within the range of 0.3m / min~0.5m / min.

[0112] In some optional embodiments, before the magnesium-rare earth alloy matrix is ​​mixed with the transition metal powder, the transition metal powder is first dispersed by vibration. The frequency of the vibration dispersion can be 10 Hz to 30 Hz, such as 10 Hz, 15 Hz, 20 Hz, 25 Hz or 30 Hz, or other values ​​within the range of 10 Hz to 30 Hz. The time of the vibration dispersion can be 0.5 h to 1 h, such as 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h or 1 h, or other values ​​within the range of 0.5 h to 1 h.

[0113] In some optional embodiments, before the high-energy ball mill is mixed with the nano-metal reinforced particle powder, the nano-metal reinforced particle powder is first subjected to vibration dispersion. Similarly, the frequency of the vibration dispersion can be 10Hz~30Hz, such as 10Hz, 15Hz, 20Hz, 25Hz or 30Hz, etc., or other values ​​within the range of 10Hz~30Hz. The time of vibration dispersion can be 0.5h~1h, such as 0.5h, 0.6h, 0.7h, 0.8h, 0.9h or 1h, etc., or other values ​​within the range of 0.5h~1h.

[0114] If the frequency of vibration dispersion is too low, it is not conducive to the uniform dispersion of nanoparticles; if the frequency of vibration dispersion is too high, there will be more friction and collision between powder particles, which will easily generate high heat and is not conducive to safe preparation.

[0115] Before mixing with the magnesium-rare earth alloy matrix, the transition metal powder is first vibrated and dispersed, which helps to reduce the proportion of powder agglomeration and dispersion, and is more conducive to the occurrence of magnesium-transition metal-rare earth element alloying. In addition, the nano-metal reinforced particle powder is first vibrated and dispersed before mixing with the high-energy ball abrasive, which is beneficial to improve the uniform dispersion of the nano-metal reinforced particle powder on the surface of the high-energy ball abrasive.

[0116] As mentioned above, the preparation method of the controllable hybrid LPSO phase reinforced magnesium-based composite material provided by the present invention is simple to operate and has low cost, and can control the volume fraction, orientation distribution and even the ratio of 18R and 14H types of the intracrystalline LPSO phase in the composite material.

[0117] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0118] Example 1

[0119] This embodiment provides an in-situ controllable regulated intracrystalline 18R and 14H mixed long-period stacking phase reinforced magnesium-based composite material, and the preparation method thereof includes:

[0120] S1: Zn powder with an average particle size of 800 nm and nano-Ti powder with an average particle size of 80 nm were respectively dispersed by vibration, and the frequency of the vibration dispersion was 30 Hz and the time was 1 hour.

[0121] S2: First, the Zn powder after vibration dispersion was mixed with a magnesium-rare earth alloy matrix with an average particle size of 80 μm (Mg-10Y powder containing 10wt% Y) at a mass ratio of 1:99, and then high-energy ball milling was performed to obtain Mg10Y1Zn alloy powder (i.e., high-energy ball milling material). The ball-to-material ratio was 25:1 (mass ratio), the rotation speed was 200 r / min, and the time was 2h.

[0122] S3: Mix the nano-Ti powder dispersed by vibration with the Mg10Y1Zn alloy powder in a mass ratio of 2:98, and perform low-energy ball milling to obtain Ti / Mg10Y1Zn composite powder (i.e., low-energy ball milling material). The ball-to-material ratio is 20:1 (mass ratio), the rotation speed is 100 r / min, and the time is 1 h.

[0123] S4: The Ti / Mg10Y1Zn composite powder is subjected to spark plasma sintering treatment, and after sintering, the powder is cooled to room temperature by water (at a cooling rate of 2°C / min) to obtain a sintered part. The sintering temperature is 500°C, the time is 6 minutes, and the pressure is 38 MPa.

[0124] S5: After the sintered part and the extrusion die are kept at 400°C for 30 minutes, hot extrusion is performed at an extrusion ratio of 25:1 and an extrusion speed of 0.5 m / min, and finally an in-situ controllable magnesium-based composite material with a mixed long-period stacking phase reinforced with 18R and 14H in the crystal is obtained.

[0125] In the magnesium-based composite material prepared in this embodiment, the mixed LPSO phase in the crystal accounts for about 18% (volume percentage) of the entire magnesium-based composite material. The mixed LPSO phase is mainly distributed in the crystal near the grain boundary. The mixed LPSO phase includes two types: lamellar 18R and needle-shaped 14H, with the 14H type LPSO phase being the main one, and the average grain size is 0.98 μm.

[0126] Example 2

[0127] This embodiment provides an in-situ controllable regulated intracrystalline 18R and 14H mixed long-period stacking phase reinforced magnesium-based composite material, and the preparation method thereof includes:

[0128] S1: Al powder with an average particle size of 500 nm and nano Mo powder with a particle size of 50 nm were respectively dispersed by vibration, and the frequency of the vibration dispersion was 10 Hz and the time was 1 hour.

[0129] S2: First, the Al powder after vibration dispersion and the magnesium-rare earth alloy matrix with an average particle size of 60μm (Mg-9Er powder containing 9wt% Er) were mixed at a mass ratio of 2:98, and then high-energy ball milling was performed to obtain high-energy ball milling material. The ball-to-material ratio was 20:1 (mass ratio), the rotation speed was 250r / min, and the time was 4h.

[0130] S3: After the vibration-dispersed nano Mo powder and the high-energy ball mill material are mixed at a mass ratio of 1:99, low-energy ball milling is performed to obtain low-energy ball mill material, wherein the ball-to-material ratio is 10:1 (mass ratio), the rotation speed is 110r / min, and the time is 2h.

[0131] S4: The low-energy ball abrasive is subjected to spark plasma sintering treatment, and after sintering, the temperature is cooled to room temperature by water (the cooling rate is 1°C / min) to obtain a sintered part. The sintering temperature is 490°C, the time is 10 minutes, and the pressure is 30 MPa.

[0132] S5: After the sintered part and the extrusion die are kept at 380°C for 30 minutes, hot extrusion is performed at an extrusion ratio of 20:1 and an extrusion speed of 0.3 m / min, and finally an in-situ controllable magnesium-based composite material with a mixed long-period stacking phase reinforced with 18R and 14H in the crystal is obtained.

[0133] In the magnesium-based composite material prepared in this embodiment, the mixed LPSO phase in the crystal accounts for 35% (volume percentage) of the entire magnesium-based composite material, and the mixed LPSO phase occupies the entire crystal. The mixed LPSO phase includes two types: lamellar 18R and needle-shaped 14H, with the 14H type LPSO phase being the main type, and the average grain size is 0.80 μm.

[0134] Example 3

[0135] This embodiment provides an in-situ controllable regulated intracrystalline 18R and 14H mixed long-period stacking phase reinforced magnesium-based composite material, and the preparation method thereof includes:

[0136] S1: Cu powder with an average particle size of 2 μm and nano-Cr powder with a particle size of 200 nm were respectively dispersed by vibration, and the frequency of the vibration dispersion was 20 Hz and the time was 0.5 h.

[0137] S2: First, the Cu powder after vibration dispersion and the magnesium-rare earth alloy matrix with an average particle size of 100μm (Mg-8Gd powder containing 8wt% Gd) were mixed at a mass ratio of 3:97, and then high-energy ball milling was performed to obtain high-energy ball milling material. Among them, the ball-to-material ratio was 30:1 (mass ratio), the rotation speed was 300r / min, and the time was 3h.

[0138] S3: After the vibration-dispersed nano-Cr powder and the high-energy ball mill material are mixed at a mass ratio of 3:97, low-energy ball milling is performed to obtain low-energy ball mill material, wherein the ball-to-material ratio is 15:1 (mass ratio), the rotation speed is 120r / min, and the time is 1.5h.

[0139] S4: The low-energy ball abrasive is subjected to spark plasma sintering treatment, and after sintering, the temperature is cooled to room temperature by water (the cooling rate is 3°C / min) to obtain a sintered part. The sintering temperature is 480°C, the time is 5 minutes, and the pressure is 50 MPa.

[0140] S5: After the sintered part and the extrusion die are kept at 390°C for 30 minutes, hot extrusion is performed at an extrusion ratio of 30:1 and an extrusion speed of 0.4 m / min, and finally an in-situ controllable magnesium-based composite material with a mixed long-period stacking phase reinforced with 18R and 14H in the crystal is obtained.

[0141] In the magnesium-based composite material prepared in this embodiment, the mixed LPSO phase in the crystal accounts for 40% (volume percentage) of the entire magnesium-based composite material. The mixed LPSO phase is mainly distributed in the crystal and obviously coarsens and grows. The mixed LPSO phase includes two types: lamellar 18R and needle-shaped 14H, mainly 18R type LPSO phase, and the average grain size is 1.05μm.

[0142] Example 4

[0143] The difference between this embodiment and embodiment 1 is that in S2, the zinc powder and the magnesium-rare earth alloy matrix are mixed in a mass ratio of 2:98.

[0144] Example 5

[0145] The difference between this embodiment and embodiment 1 is that in S2, the zinc powder and the magnesium-rare earth alloy matrix are mixed in a mass ratio of 3:97.

[0146] Example 6

[0147] The difference between this embodiment and embodiment 1 is that in S2, the average particle size of the transition metal powder is 600 nm.

[0148] Example 7

[0149] The difference between this embodiment and embodiment 1 is that in S2, the average particle size of the transition metal powder is 1.5 μm.

[0150] Example 8

[0151] The difference between this embodiment and embodiment 1 is that in S2, the average particle size of the magnesium-rare earth alloy matrix is ​​75 μm.

[0152] Example 9

[0153] The difference between this embodiment and embodiment 1 is that in S2, the average particle size of the magnesium-rare earth alloy matrix is ​​85 μm.

[0154] Comparative Example 1

[0155] The difference between this comparative example and Example 1 is that the preparation raw material does not contain Zn powder and nano-Ti powder, and the magnesium-rare earth alloy matrix is ​​directly subjected to spark plasma sintering and hot extrusion to obtain pure Mg-10Y alloy.

[0156] Comparative Example 2

[0157] The difference between this comparative example and Example 1 is that the content of rare earth elements in the magnesium-rare earth alloy matrix is ​​5wt%.

[0158] Comparative Example 3

[0159] The difference between this comparative example and Example 1 is that the content of rare earth elements in the magnesium-rare earth alloy matrix is ​​20wt%.

[0160] Comparative Example 4

[0161] The difference between this comparative example and Example 1 is that the Zn powder and the magnesium-rare earth alloy matrix are mixed in a mass ratio of 10:90.

[0162] Comparative Example 5

[0163] The difference between this comparative example and Example 1 is that the Zn powder and the magnesium-rare earth alloy matrix are mixed in a mass ratio of 0.5:99.5.

[0164] Comparative Example 6

[0165] The difference between this comparative example and Example 1 is that the nano-Ti powder and the high-energy ball mill are mixed in a mass ratio of 5:95.

[0166] Comparative Example 7

[0167] The difference between this comparative example and Example 1 is that the nano-Ti powder and the high-energy ball mill are mixed in a mass ratio of 0.5:99.5.

[0168] Comparative Example 8

[0169] The difference between this comparative example and Example 1 is that the average particle size of the magnesium-rare earth alloy matrix is ​​130 μm.

[0170] Comparative Example 9

[0171] The difference between this comparative example and Example 1 is that the average particle size of the transition metal powder is 3 μm.

[0172] Comparative Example 10

[0173] The difference between this comparative example and Example 1 is that the average particle size of the nano metal reinforcement particle powder is 20 nm.

[0174] Comparative Example 11

[0175] The difference between this comparative example and Example 1 is that step S1 is not performed, that is, the transition metal powder and the nano-metal reinforcement particle powder are not vibrated and dispersed.

[0176] Comparative Example 12

[0177] The difference between this comparative example and Example 1 is that in S1, the vibration dispersion frequency of the transition metal powder and the nano-metal reinforced particle powder is 50 Hz.

[0178] Comparative Example 13

[0179] The difference between this comparative example and Example 1 is that after S1, the Ti powder, the nano Zn powder and the magnesium-rare earth alloy matrix are directly subjected to high-energy ball milling together; and then the high-energy ball milled material is subjected to spark plasma sintering and hot extrusion.

[0180] Comparative Example 14

[0181] The difference between this comparative example and Example 1 is that after S1, the Ti powder, the nano Zn powder and the magnesium-rare earth alloy matrix are directly subjected to low-energy ball milling together; and then the low-energy ball milled material is subjected to spark plasma sintering and hot extrusion.

[0182] Comparative Example 15

[0183] The difference between this comparative example and Example 1 is that in S2, the rotation speed of the high energy ball mill is 500 r / min.

[0184] Comparative Example 16

[0185] The difference between this comparative example and Example 1 is that in S4, the sintering temperature is 450°C.

[0186] Comparative Example 17

[0187] The difference between this comparative example and Example 1 is that in S4, the sintering time is 15 minutes.

[0188] Comparative Example 18

[0189] The difference between this comparative example and Example 1 is that in S4, the sintering time is 2 minutes.

[0190] Test example

[0191] ①. The morphology of the magnesium-based composite materials obtained in Example 1, Example 4, Example 5 and Comparative Example 1 was measured, and the transmission crystal structure of the LPSO phase formed in the above examples was characterized. The results are as follows: Figures 1 to 13 shown.

[0192] Combination Figures 1 to 11 It can be concluded that: in the magnesium-based composite material prepared in Example 1, the LPSO phase is mainly distributed inside the grain near the grain boundary, with a volume fraction of about 18%. In the magnesium-based composite material prepared in Example 4, the LPSO phase basically occupies the entire interior of the grain, with a volume fraction of about 39%, and a grain size of 0.79 μm. In the magnesium-based composite material prepared in Example 5, the LPSO phase grows and coarsens, with a volume fraction of about 42%, and a grain size of 1.09 μm.

[0193] Through the fine structure characterization of the LPSO phase, it was found that the 14H-LPSO phase appeared to be needle-shaped (such as Figure 3 ), the 18R-LPSO phase appears as a sheet (e.g. Figure 4 ). Combining the results of Example 1 and Examples 4-5, as the mass ratio of transition metal Zn to rare earth Y increases, the total volume fraction of LPSO phase increases significantly, first dominated by 14H-LPSO phase, and finally dominated by 18R-LPSO phase. The discontinuous distribution of nano-Ti at the grain boundary position helps to maximize the effect of grain boundary strengthening.

[0194] In addition, by Figure 5 and Figure 6 It can be seen that the LPSO phase interacts with dislocations, and this feature can hinder<c+a> The movement of dislocations helps to improve strength.

[0195] Depend on Figure 7 It can be seen that the LPSO phase inhibits the occurrence of dynamic recrystallization, and this feature is conducive to the grain refinement of the composite material.

[0196] Depend on Fig.12 and Fig.13 It can be seen that a large amount of Mg2Y phase is precipitated in the Mg10Y alloy without LPSO phase precipitation, and the grain size is relatively large.

[0197] Depend on Figure 1~Figure 4 as well as Figure 8~Figure 13It can be seen that the grain size of the magnesium-based composite material prepared by the method provided in the embodiment of the present application can be refined to the submicron level, and the LPSO phase with high strength, plasticity and elastic modulus precipitated in a wheel-shaped distribution inside the grains helps to weaken the texture strength; the discontinuous distribution of nano-reinforced particles on the grain boundaries helps to strengthen the grain boundaries, resulting in the simultaneous improvement of the strength and elastic modulus of the composite material, while the plasticity is basically maintained at the same level as the matrix.

[0198] ② The magnesium-based composite materials obtained in Examples 1 to 9 and Comparative Examples 1 to 18 were subjected to mechanical property tests and the average grain sizes were statistically analyzed. The results are shown in Table 1.

[0199] Among them, the yield strength, tensile strength and room temperature elongation are tested in accordance with "GB / T 228.1-2021", and the elastic modulus is tested in accordance with "GB / T 32376-2015‌".

[0200] Table 1 Grain size and mechanical properties test results

[0201]

[0202] It can be seen from Table 1 that the magnesium-based composite material provided by the present invention can have high strength and elastic modulus at the same time, and the plasticity is consistent with that of the matrix.

[0203] In summary, the intracrystalline long-period stacking phase volume fraction of the magnesium-based composite material provided by the present invention can be controllably adjusted, and the volume fraction accounts for 10% to 50%; the intracrystalline long-period stacking phase types include 18R type and 14H type, and as the mass ratio of transition metal powder to rare earth elements increases, the total volume fraction of the mixed LPSO phase also increases, and the mixed LPSO phase is mainly 14H type LPSO phase from the beginning to the end. The 18R type LPSO phase is mainly distributed, and the distribution of the mixed LPSO phase gradually grows from the position near the grain boundary in the crystal to the center, and the orientation of the mixed LPSO phase presents a wheel-shaped distribution until it fills the entire crystal, and then the size of the mixed LPSO phase gradually coarsens and grows. In addition, the above-mentioned LPSO phase and the magnesium alloy matrix are coherent interfaces, have good interface bonding, are in-situ self-generated and uniformly distributed inside the magnesium grains, and present a wheel-shaped uniform distribution feature, which helps to weaken the texture orientation. In addition, the intracrystalline LPSO phase inhibits the occurrence of dynamic recrystallization, refines the grain structure, and greatly improves the mechanical properties of the composite material.

[0204] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A controllable hybrid LPSO phase reinforced magnesium-based composite material, characterized in that: The raw materials for preparing the hybrid LPSO phase reinforced magnesium-based composite material include a magnesium-rare earth alloy matrix, transition metal powder and nano-metal reinforcement particle powder; The ratio of the mass of the transition metal powder to the mass of the magnesium-rare earth alloy matrix is ​​1:99 to 3:97, and the ratio of the mass of the nano-metal reinforced particle powder to the total mass of the magnesium-rare earth alloy matrix and the transition metal powder is 1:99 to 3:97; the content of rare earth elements in the magnesium-rare earth alloy matrix is ​​8wt% to 15wt%; In the hybrid LPSO phase-reinforced magnesium-based composite material, the volume of the hybrid LPSO phase in the crystal accounts for 10% to 50% of the hybrid LPSO phase-reinforced magnesium-based composite material, the hybrid LPSO phase types in the crystal include lamellar 18R type and needle-shaped 14H type, and there are discontinuously distributed nano-metal reinforcement particles at the grain boundaries; and, as the mass ratio of transition metal elements to rare earth elements in the preparation raw materials increases, the total volume fraction of the hybrid LPSO phase also increases, and the hybrid LPSO phase is mainly composed of 14H type LPSO phase at the beginning and becomes mainly composed of 18R type LPSO phase at the end; The rare earth element in the magnesium-rare earth alloy matrix is ​​at least one of Gd, Y, Tb, Dy, Ho and Er; the transition metal in the transition metal powder is at least one of Zn, Al and Cu; the metal in the nano-metal reinforced particle powder is at least one of Ti, Mo and Cr; The preparation of the controllable hybrid LPSO phase reinforced magnesium-based composite material comprises the following steps: mixing the magnesium-rare earth alloy matrix with the transition metal powder and performing high-energy ball milling to obtain high-energy ball mill material; mixing the high-energy ball mill material with the nano-metal reinforced particle powder and performing low-energy ball milling to obtain low-energy ball mill material; and sintering and hot extrusion deforming the low-energy ball mill material.

2. The hybrid LPSO phase reinforced magnesium-based composite material according to claim 1, characterized in that: The average particle size of the magnesium-rare earth alloy matrix is ​​60 μm to 100 μm; And / or, the average particle size of the transition metal powder is 500nm~2μm; And / or, the average particle size of the nano metal reinforcement particle powder is 50nm~200nm.

3. The hybrid LPSO phase reinforced magnesium-based composite material according to claim 1 or 2, characterized in that: The hybrid LPSO phase reinforced magnesium-based composite material also has at least one of the following characteristics: Feature 1: As the mass ratio of transition metal elements to rare earth elements in the raw materials increases, the distribution of the mixed LPSO phase gradually grows from the position near the grain boundary in the crystal to the center, and the orientation of the mixed LPSO phase presents a wheel-shaped distribution until it fills the entire crystal, and then the mixed LPSO phase coarsens and grows; Feature 2: The average grain size of the hybrid LPSO phase reinforced magnesium-based composite material does not exceed 2 μm; Feature 3: The tensile strength of the hybrid LPSO phase reinforced magnesium-based composite material is not less than 400 MPa; Feature 4: The yield strength of the hybrid LPSO phase reinforced magnesium-based composite material is not less than 380 MPa; Feature 5: The elongation of the hybrid LPSO phase reinforced magnesium-based composite material is not less than 12%; Feature 6: The elastic modulus of the hybrid LPSO phase reinforced magnesium-based composite material is not less than 50 GPa.

4. A method for preparing a hybrid LPSO phase reinforced magnesium-based composite material according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: mixing the magnesium-rare earth alloy matrix with the transition metal powder and performing high-energy ball milling to obtain high-energy ball mill material; mixing the high-energy ball mill material with the nano-metal reinforced particle powder and performing low-energy ball milling to obtain low-energy ball mill material; and sintering and hot extrusion deformation of the low-energy ball mill material.

5. The preparation method according to claim 4, characterized in that: High energy ball milling has at least one of the following characteristics: Feature 7: The speed of high energy ball mill is 200r / min~300r / min; Feature 8: The ball-to-material ratio of high-energy ball milling is 20:1 to 30:1 by mass; Feature 9: High energy ball milling time is 2h~4h.

6. The preparation method according to claim 4, characterized in that: Low energy ball milling has at least one of the following characteristics: Feature 10: The speed of low-energy ball mill is 100r / min~120r / min; Feature 11: The ball-to-material ratio of low-energy ball milling is 10:1 to 20:1 by mass; Feature 12: The time of low-energy ball milling is 1h~2h.

7. The preparation method according to claim 4, characterized in that: Sintering has at least one of the following characteristics: Feature 13: The sintering temperature is 480℃~500℃; Feature 14: The sintering pressure is 30MPa~50MPa; Feature 15: The sintering time is 5min~10min; Feature 16: After sintering, water cooling is performed first and then hot extrusion deformation is performed.

8. The preparation method according to claim 4, characterized in that: Hot extrusion deformation has at least one of the following characteristics: Feature 17: The temperature of hot extrusion deformation is 380℃~400℃; Feature 18: The extrusion ratio of hot extrusion deformation is 20:1 to 30:1; Feature 19: The speed of hot extrusion deformation is 0.3m / min~0.5m / min.

9. The preparation method according to claim 4, characterized in that: Before mixing the magnesium-rare earth alloy matrix with the transition metal powder, the transition metal powder is firstly vibrated and dispersed; before mixing the high energy ball mill with the nano metal reinforced particle powder, the nano metal reinforced particle powder is firstly vibrated and dispersed; The frequency of vibration dispersion is 10Hz~30Hz, and the time of vibration dispersion is 0.5h~1h.

Citation Information

Patent Citations

  • Layered / acicular two-phase composite enhanced rare earth magnesium alloy and preparation technology thereof

    CN104894447A

  • Medical Mg-Gd-Zn (-Ca) magnesium alloy with LPSO structure and preparation method thereof

    CN106244882A