SnO2-based composite target material as well as preparation method and application thereof
By introducing synergistic co-doping of Ag, Cu and La into SnO2, the problems of difficulty in sintering and insufficient performance of SnO2-based TCO films are solved, and high conductivity and mechanical properties are improved, which is suitable for high-efficiency photovoltaics and perovskites. Battery applications.
Patent Information
- Application Number
- CN202410728978.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-06
AI Technical Summary
SnO2-based TCO films face the problems of difficult sintering, insufficient conductivity and limited mechanical properties under high performance requirements.
By introducing synergistic co-doping of Ag, Cu and La into SnO2, the conductivity, mechanical properties and sintering performance are improved, a highly conductive network and stabilized grain interface are formed, and densification and thermal shock stability are promoted.
It significantly improves the density and conductivity of the target, reduces the resistivity, and enhances the thermal stability and mechanical properties. It is suitable for TCO films of high-efficiency photovoltaic heterojunction cells and perovskite cells.
Smart Images

Figure BDA0004879621870000041 
Figure BDA0004879621870000042
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of target material preparation, and in particular to a SnO2-based composite target material and a preparation method and application thereof. Background Art
[0002] Tin oxide (SnO2)-based TCO thin films have become a research hotspot due to their abundant raw material reserves, non-toxic and good chemical stability. Tin dioxide (SnO2) has attracted much attention for its excellent optical transparency, good chemical stability and electrical properties, especially in cutting-edge technology fields such as energy, environmental protection, information storage and optoelectronics. However, despite the natural properties of SnO2, it still faces many challenges such as sintering difficulties, insufficient conductivity and limited mechanical properties under high performance requirements.
[0003] Therefore, it is necessary to develop a SnO2-based composite target. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the first aspect of the present invention provides a SnO2-based composite target material, which can improve the sintering performance and electrical properties of the SnO2 target material.
[0005] The second aspect of the present invention also provides a method for preparing a SnO2-based composite target material.
[0006] The third aspect of the present invention also provides an application of a SnO2-based composite target material.
[0007] The SnO2-based composite target provided by the first embodiment of the present invention includes the following components in percentage by mass:
[0008] The content of SnO2 is 91.5% to 95.5%, the content of silver is 3% to 5%, the content of copper oxide is 1% to 2%, the content of lanthanum oxide is 0.5% to 1.5%, and the sum of the amounts of each component is 100%.
[0009] The SnO2-based composite target material according to the embodiment of the present invention has at least the following beneficial effects:
[0010] In the related art, the sintering of SnO2 usually requires extremely high temperatures to achieve material densification, which not only consumes a lot of energy but also may cause excessive grain growth, thereby damaging the conductivity and optical transparency of the material.
[0011] The present invention systematically improves the conductivity, mechanical properties and sintering properties of SnO2 by introducing the synergistic co-doping of Ag, Cu and La. It further improves the density of the target material and reduces the resistivity of the target material. The target material density is 6.74g / m 3 ~6.86g / m3 Between; target resistivity 7.07×10 -4 Ω·cm~9.82×10 -4 Ω·cm.
[0012] During the entire sintering process, Cu acts as a sintering aid to promote mass transfer and defect repair in the sintered body. At the same time, the addition of Ag forms a highly conductive network, while the introduction of La is conducive to the stabilization of the grain interface, thereby effectively controlling the grain size and improving the thermal shock stability of the material.
[0013] Specifically, Cu doping plays a key role in improving sintering activity. Since CuO can produce a liquid phase during the sintering process, it can effectively promote the wetting and rearrangement between SnO2 particles, which is beneficial to material densification and shortening the sintering time. While reducing energy consumption, it is beneficial to the uniform doping of Ag and La elements. The introduction of Ag can not only significantly improve the conductivity of the material, but also maintain a superior conductive network structure at high temperatures. This is because Ag can form a good conductive path in the SnO2 matrix. At the same time, because Ag has good interface properties, it helps the microstructure of the material to be more uniform during the sintering process.
[0014] In addition, the addition of La provides a significant advantage for the present invention. As a rare earth element, La exhibits a unique electronic environment and excellent chemical stability when doped into the SnO2 lattice. 3+ The introduction of lanthanum can cause a strain effect in the lattice, which helps to fix the oxygen vacancies in the lattice, thereby increasing the electron density of the crystal, improving the conductivity, and effectively inhibiting the grain growth at high temperature, so that the mechanical properties of the sintered body are significantly improved. The addition of lanthanum also helps to reduce the phase change and grain boundary migration of the material during the thermal cycle, thereby enhancing the thermal stability of the sintered body.
[0015] According to some embodiments of the present invention, the particle size of the silver is 20-30 nm.
[0016] According to some embodiments of the present invention, the specific surface area of SnO2 is 10m 2 / g~25m 2 / g.
[0017] According to the second aspect of the present invention, the method for preparing the SnO2-based composite target material provided by the embodiment comprises the following steps:
[0018] S1, mixing SnO2, silver, copper oxide, lanthanum oxide, a binder and a plasticizer to obtain a mixed powder, and ball milling to obtain a mixed powder;
[0019] S2, pressing the mixed powder into a mold to obtain an embryo;
[0020] S3, degreasing, sintering and cooling the embryo body.
[0021] According to some embodiments of the present invention, in step S2, the pressure of the pressing molding is 100 MPa to 200 MPa.
[0022] According to some embodiments of the present invention, the degreasing step includes: heating the temperature to 600° C. to 650° C. and keeping the temperature for 1 hour to 2 hours.
[0023] According to some embodiments of the present invention, the sintering steps are as follows:
[0024] Raise the temperature to 850-900℃ and keep it warm for 5-6h; then raise the temperature to 1200-1250℃ and keep it warm for 3-4h; then lower the temperature to 1000-1050℃ and keep it warm for 9-10h.
[0025] According to some embodiments of the present invention, the binder comprises polyvinyl alcohol.
[0026] According to some embodiments of the invention, the plasticizer comprises polyethylene glycol.
[0027] The third aspect of the present invention provides an application of the SnO2-based composite target material in the preparation of a TCO film for a photovoltaic heterojunction cell or a TCO film for a perovskite cell.
[0028] Therefore, the TCO film prepared by sputtering the SnO2-based composite target material of the present invention has good light transmittance and low resistivity, thereby improving the battery conversion efficiency.
[0029] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. DETAILED DESCRIPTION
[0030] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0031] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0032] Some of the raw materials used in the embodiments of the present invention are as follows:
[0033] SnO2: purity ≥99.99%, particle size 20-40 nm, purchased from Qinghe County Ruijiang Metal Materials Co., Ltd.;
[0034] Silver: purity ≥99.99%, particle size 15-35 nm, purchased from Xuzhou Jie Innovation Materials Technology Co., Ltd.;
[0035] Copper oxide: purity ≥99.99%, particle size 40-55 nm, purchased from Guangzhou Metal Metallurgy (Group) Co., Ltd.;
[0036] Lanthanum oxide: purity ≥99.99%, particle size 45-60 nm, purchased from Beijing October New Material Technology Co., Ltd.
[0037] Example 1
[0038] This example provides a SnO2-based composite target material, the components and amounts of which are shown in Table 1, and the preparation method is as follows:
[0039] S1. Mix SnO2, silver, copper oxide, lanthanum oxide, polyvinyl alcohol and polyethylene glycol to obtain a mixed powder, and perform ball milling; the ball milling uses 0.65 mm and 0.30 mm zirconium beads to grind, and spray dry to obtain a mixed oxide powder;
[0040] S2. Use a rotating target mold to inject the mixed oxide powder into the mold, use WCIP molding, the molding pressure is 100MPa-200MPa, and after static pressure strengthening, it becomes a target blank;
[0041] S3, placing the green blank obtained in step S2 into a sintering furnace; heating the temperature to 600-650°C at a heating rate of 1°C / min-3°C / min for degreasing, and keeping the temperature for 1-2 hours. After degreasing, heating the temperature to 850-900°C at 3°C / min, keeping the temperature for 6 hours; heating the temperature to 1200-1250°C at 1°C / min, keeping the temperature for 4 hours; then cooling the temperature to 1000-1050°C at 1°C / min, keeping the temperature for 10 hours; cooling to room temperature to obtain a target material.
[0042] Embodiments 2 to 6
[0043] Examples 2 to 6 provide a series of SnO2-based composite target materials, the component amounts of which are shown in Table 1, and the preparation method is the same as that of Example 1.
[0044] Table 1 Examples 1 to 6 (mass percentage %)
[0045] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 <![CDATA[SnO2]]> 91.5 93 93.5 94 95 95.5 silver 5 4 4 3.5 3 3 Copper Oxide 2 2 1.5 1.5 1 1 Lanthanum Oxide 1.5 1 1 1 1 0.5
[0046] Comparative Examples 1 to 7
[0047] Comparative Examples 1 to 7 provide a series of SnO2-based target materials, the component amounts are shown in Table 2, and the preparation method is the same as Example 1.
[0048] Table 2 Comparative Examples 1 to 7 (mass percentage %)
[0049]
[0050]
[0051] Performance Testing
[0052] The targets prepared in Examples 1 to 6 of the present invention and Comparative Examples 1 to 7 were subjected to the following tests; the results are shown in Table 3.
[0053] Density: Measured by Archimedes displacement method.
[0054] Resistivity: Use a resistivity meter to test the resistivity of the target material.
[0055] Table 3 Examples 1 to 6 and Comparative Examples 1 to 7
[0056]
[0057] From the data in Table 3, it can be seen that: Comparative Example 1 is pure tin oxide without doping. Under this sintering process, there are many pores between the grains, the density of the prepared target material is low, the resistivity is too high, and there is almost no conductive performance. Comparative Example 2 reduces the resistivity of the target material by doping with Ag, but the density of the target material is low. Comparative Example 3 improves the sintering density by doping with CuO, and the resistivity decreases slightly but cannot achieve the ideal effect. Comparative Example 4 is doped with La2O3, and the resistivity decreases slightly. Comparative Example 5 is doped with Ag and CuO at the same time, and the density of the target material has been significantly improved, while the resistivity further decreases, but it still cannot reach the ideal resistance value. Comparative Example 6 is doped with CuO and La2O3 at the same time, and the target material density is increased while the resistivity further decreases. It can be seen that the addition of CuO has a modified effect on the doping of La, but it still cannot reach the ideal resistance value. Comparative Example 7 is doped with Ag, CuO and La2O3 at the same time, but the doping amount is too high, resulting in large lattice distortion and cracking after sintering.
[0058] In Examples 1 to 6 of the present invention, Ag, CuO and La2O3 are doped at the same time and are within the scope of the present invention. Ag and Cu co-doping improves the density of the target material, and La is doped on this basis to finally obtain a sintered body with good density and further reduced resistivity compared with the comparative example. The sintered target material is excellent in resistivity and density, and the processed target material can be stably used for sputtering coating.
[0059] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A SnO 2 Composite target material, It is characterized in that The components include the following mass percentages: SnO 2 The content of copper is 91.5% to 95.5%, the content of silver is 3% to 5%, the content of copper oxide is 1% to 2%, the content of lanthanum oxide is 0.5% to 1.5%, and the sum of the amounts of each component is 100%.
2. SnO according to claim 1 2 Composite target material, It is characterized in that The particle size of the silver is 20 to 30 nm.
3. SnO according to claim 1 2 Composite target material, It is characterized in that The SnO 2 The specific surface area is 10m 2 / g~25m 2 / g.
4. The SnO according to any one of claims 1 to 3 2 Preparation method of composite target material, It is characterized in that The steps include: S1, SnO 2 , silver, copper oxide, lanthanum oxide, a binder and a plasticizer are mixed to obtain a mixed powder, and ball milled to obtain a mixed powder; S2, pressing the mixed powder into a mold to obtain an embryo; S3, degreasing, sintering and cooling the embryo body.
5. SnO according to claim 4 2 Preparation method of composite target material, It is characterized in that In step S2, the pressure of the pressing molding is 100 MPa to 200 MPa.
6. SnO according to claim 4 2 Preparation method of composite target material, It is characterized in that The degreasing step comprises: heating the temperature to 600° C. to 650° C. and keeping the temperature for 1 hour to 2 hours.
7. SnO according to claim 4 2 Preparation method of composite target material, It is characterized in that The sintering steps are as follows: Raise the temperature to 850-900℃ and keep it warm for 5-6h; then raise the temperature to 1200-1250℃ and keep it warm for 3-4h; then lower the temperature to 1000-1050℃ and keep it warm for 9-10h.
8. SnO according to claim 4 2 Preparation method of composite target material, It is characterized in that The binder includes polyvinyl alcohol.
9. SnO according to claim 4 2 Preparation method of composite target material, It is characterized in that The plasticizer includes polyethylene glycol.
10. SnO according to any one of claims 1 to 3 2 Application of composite target materials in the preparation of TCO films for photovoltaic heterojunction cells or TCO films for perovskite cells.
Citation Information
Patent Citations
Tin Oxide Ceramic Sputtering Target And Method Of Producing It
CN102811971A
Preparation method of tin oxide-based thin film varistor
CN107293384A
Tin oxide target material doped with silver as well as preparation method and application thereof
CN110257786A
Tin oxide-based sintered body and method for manufacturing same
CN111727179A
Tin oxide-based target material as well as preparation method and application thereof
CN117986010A
Cited By
Up-conversion luminescence TCO film and preparation method and application thereof
CN121272344A