Composite coating and preparation method thereof
By forming a composite coating structure on the surface of the core parts of the engine, combined with cold spray technology and ceramic coating, the problem of hydrogen corrosion and difficulty in coating formation is solved, achieving efficient hydrogen penetration and corrosion resistance protection, reducing costs and ensuring environmentally friendly process.
Patent Information
- Application Number
- CN202410746194.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-11
AI Technical Summary
Hydrogen combustion causes hydrogen corrosion in engines, and it is difficult to form coatings on existing cast iron and steel surfaces, resulting in poor protection of core engine components.
Adopt a composite coating structure, including transition layer, anti-corrosion layer and hydrogen barrier coating. Al-Ni or Al-Cr coating and ceramic coating are formed on the surface of the substrate through cold spray technology, combined with high-purity nitrogen spraying to avoid hydrogen Introduced to enhance resistance to hydrogen penetration and corrosion resistance.
It effectively improves the protection effect of the core components of the engine, avoids hydrogen corrosion, reduces process costs, is environmentally friendly and feasible, and breaks through the limitations of a single coating's performance.
Smart Images

Figure CN118756129A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal surface coatings, and in particular to a composite coating and a preparation method thereof. Background Art
[0002] Due to its fast combustion speed, high calorific value, wide sources and no pollution, hydrogen is known as the most promising alternative fuel. However, during the service of the engine, hydrogen or combustion products will cause hydrogen corrosion to the core parts of the engine. At present, it is difficult to form coatings such as electroplating / chemical plating on the surface of cast iron, and electroplating / chemical plating on the surface of steel is easy to introduce hydrogen, resulting in poor protection of the core parts of the engine. Therefore, it is urgent to carry out research on the hydrogen penetration resistance and corrosion resistance of the surface of core parts. Summary of the invention
[0003] In view of the problems existing in the background technology, the present application provides a composite coating and a preparation method thereof. The composite coating has a good hydrogen barrier effect, high corrosion resistance and resistance to hydrogen diffusion, and can enhance the protection of the core components of the engine.
[0004] According to one aspect of the present invention, there is provided a composite coating, comprising: a transition layer connected to the surface of a substrate; an anti-corrosion layer connected to the surface of the transition layer away from the substrate; and a hydrogen barrier coating connected to the surface of the anti-corrosion layer away from the anti-corrosion layer.
[0005] In some embodiments of the present invention, the transition layer is an Al coating.
[0006] In some embodiments of the present invention, the anti-corrosion layer is an Al-Ni or Al-Cr coating.
[0007] In some embodiments of the present invention, the hydrogen barrier coating is an Al2O3, Y2O3, Cr2O3 or ZrO2 coating.
[0008] In some embodiments of the present invention, the composite coating has a thickness of 100 μm-400 μm.
[0009] According to another aspect of the present invention, a method for preparing a composite coating is provided, comprising: S1, pre-treating a substrate for spraying; S2, using a first powder and adopting a cold spraying technique to prepare a transition layer on the surface of the substrate; S3, using a second powder and adopting a cold spraying technique to prepare an anti-corrosion layer on the transition layer; S4, using a third powder and adopting a spraying technique to prepare a hydrogen barrier coating on the anti-corrosion layer.
[0010] In some embodiments of the present invention, the pretreatment uses sandblasting to remove oil and rust from the surface of the substrate.
[0011] In some embodiments of the present invention, the roughness of the substrate surface after pretreatment is 0.8-1 μm.
[0012] In some embodiments of the present invention, the first powder is Al powder, the second powder is Al-Ni alloy powder or Al-Cr alloy powder, and the third powder is ceramic powder.
[0013] In some embodiments of the present invention, each powder is dried at 100-120° C. before use.
[0014] The present invention provides a composite coating and a preparation method thereof, wherein the hydrogen barrier coating located on the outermost layer of a substrate can prevent the penetration of hydrogen or combustion products, while the anti-corrosion layer located on the next layer has high corrosion resistance and resistance to hydrogen penetration and diffusion, breaking through the limitation of the performance of a single coating, and based on the transition layer, the bonding strength of the transition layer, the anti-corrosion layer and the hydrogen barrier coating as well as the overall bonding strength with the substrate are high, thereby effectively improving the protection of the core components of the engine; the preparation method avoids the introduction of hydrogen or hydrogen gas during the preparation of the composite coating, and there will be no phenomenon that the anti-corrosion layer cannot be plated on the surface of the cast iron, thereby reducing the process cost, and having no pollution to the environment, thereby ensuring the feasibility of the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Also, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:
[0016] Figure 1 It is a schematic diagram of the overall structure of the composite coating of the present invention.
[0017] The reference numerals in the accompanying drawings represent the following: 1. substrate; 2. transition layer; 3. anti-corrosion layer; 4. hydrogen barrier coating. DETAILED DESCRIPTION
[0018] It should be clear that the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0019] When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present application. Instead, they are only examples of devices and methods consistent with some aspects of the present application as detailed in the attached claims.
[0020] In the description of the present application, it should be understood that the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance. For those of ordinary skill in the art, the specific meanings of the above terms in the present application can be understood according to the specific circumstances. In addition, in the description of the present application, unless otherwise specified, "multiple" refers to two or more. "And / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. The character " / " generally indicates that the objects associated before and after are in an "or" relationship.
[0021] The present application discloses a composite coating. Figure 1 As shown, the composite coating includes a transition layer 2, an anti-corrosion layer 3 and a hydrogen barrier coating 4; wherein the transition layer 2 is connected to the surface of the substrate 1; the anti-corrosion layer 3 is connected to the surface of the transition layer 2 away from the substrate 1; and the hydrogen barrier coating 4 is connected to the surface of the anti-corrosion layer 3 away from the anti-corrosion layer 3.
[0022] By using the composite coating in the technical solution, firstly, the hydrogen barrier coating 4 located on the outermost layer of the substrate 1 can prevent the penetration of hydrogen or combustion products, while the anti-corrosion layer 3 located in the next layer has a higher ability to resist corrosion and hydrogen penetration and diffusion, breaking through the limitations of the performance of a single coating, and based on the transition layer 2, the bonding strength of the transition layer 2, the anti-corrosion layer 3 and the hydrogen barrier coating 4 as well as the overall bonding strength with the substrate 1 are high, thereby effectively improving the protection of the core components of the engine.
[0023] It should be noted that the material of the substrate 1 includes but is not limited to cast iron or steel.
[0024] In some embodiments of the present invention, the transition layer 2 is an Al coating, which is a self-healing coating that can automatically repair itself when damaged, thereby preventing the substrate 1 from contacting with the corrosive medium and thus avoiding corrosion.
[0025] In some embodiments of the present invention, the anti-corrosion layer 3 is an Al-Ni or Al-Cr coating, which is an intermediate layer and has a corrosion-resistant function.
[0026] In some embodiments of the present invention, the hydrogen barrier coating 4 is an Al2O3, Y2O3, Cr2O3 or ZrO2 coating, which is a surface layer and has a hydrogen barrier function.
[0027] Among them, Al2O3 is preferably α-Al2O3.
[0028] Specifically, in this embodiment, based on the Al coating, an Al-Ni or Al-Cr coating is first formed, and then an Al2O3, Y2O3, Cr2O3 or ZrO2 coating is formed. For example, an Al coating is first prepared on the substrate 1, and then an Al-Ni coating is prepared on the Al coating, and finally an Al2O3 coating is prepared on the Al-Ni coating, thereby obtaining an Al-Ni-Al2O3 wear-resistant, hydrogen-resistant and corrosion-resistant structural functional integrated coating.
[0029] In some embodiments of the present invention, the total thickness of the hydrogen barrier coating 4, the anti-corrosion layer 3 and the transition layer 2 is 100 μm-400 μm, for example, the thickness is 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, etc.
[0030] This embodiment also proposes a preparation method, which is used to prepare the above-mentioned composite coating, and the preparation method comprises the following steps:
[0031] S1, performing pretreatment on the substrate 1 to be sprayed.
[0032] S2. Using the first powder and adopting cold spraying technology, a transition layer 2 is prepared on the surface of the substrate 1.
[0033] S3. Use the second powder and adopt the cold spraying technology to prepare the anti-corrosion layer 3 on the transition layer 2.
[0034] S4. Using the third powder and adopting the spraying technology to prepare the hydrogen barrier coating 4 on the anti-corrosion layer 3.
[0035] Among them, cold spray technology is to preheat compressed gas to drive micron-sized powder particles through the Laval convergent-divergent nozzle to accelerate to supersonic speed, convert kinetic energy into plastic deformation, and combine on the substrate to form a coating or deposit.
[0036] Thermal spraying technology refers to heating and melting the coating material, atomizing it into extremely fine particles with a high-speed airflow, and spraying it onto the surface of the workpiece at a very high speed to form a coating.
[0037] Compared with traditional coating modification methods such as magnetron sputtering, chemical vapor deposition and chemical electroplating, by using the preparation method in the technical solution, a cold spraying technology is designed to prepare a hydrogen barrier-corrosion resistant coating. The cold spraying technology realizes the preparation of an environmentally friendly, efficient and controllable composite hydrogen barrier-corrosion resistant coating. Nitrogen / helium promotes the deposition of powder on the surface of the material while suppressing the introduction of hydrogen atoms. The supersonic air flow speed makes the deposition rate of cold spraying much higher than that of vapor deposition. Therefore, no hydrogen or hydrogen gas is introduced during the preparation of the hydrogen barrier-corrosion resistant coating, and there will be no phenomenon that the cast iron surface cannot be coated with the anti-corrosion layer 3, which reduces the process cost, does not pollute the environment, and ensures the feasibility of the process.
[0038] In some embodiments of the present invention, the process parameters of cold spraying technology are: high-purity nitrogen acceleration, gas temperature of 500°C to 800°C, gas pressure of 4 to 5MPa, spraying distance of 30mm, spray gun moving speed of 200 to 300mm / s, and powder feeding rate of 80 to 120g / min.
[0039] Compared with the thermal spraying process, the present invention strictly controls the temperature / environment. Since the spraying is carried out in a nitrogen environment, there is no pollution from other elements such as oxygen and water.
[0040] The composite coating prepared by the present invention has high bonding strength and controllable thickness, and controllable preparation of wear-resistant and hydrogen-blocking composite coatings on the surface of materials in hydrogen environments can be obtained according to requirements.
[0041] In some embodiments of the present invention, the pretreatment is performed by sandblasting to remove oil and rust from the surface of the substrate 1 .
[0042] Furthermore, the roughness of the surface of the substrate 1 after pretreatment is 0.8-1 μm.
[0043] In some embodiments of the present invention, the transition layer 2 is made of Al powder, the anti-corrosion layer 3 is made of Al-Ni alloy powder or Al-Cr alloy powder, and the hydrogen barrier coating 4 is made of ceramic powder.
[0044] Among them, ceramic powders include but are not limited to α-Al2O3, Y2O3, Cr2O3, ZrO2 and other powders.
[0045] Furthermore, each powder is dried at 100-120° C. before use to remove water and moisture.
[0046] It should be noted that the Al-Ni alloy powder is obtained by mixing Al powder and Ni-based alloy powder and then drying; the Al-Cr alloy powder is obtained by mixing Al powder and Cr-based alloy powder and then drying.
[0047] In some embodiments of the present invention, the spraying technology of step S4 can specifically adopt cold spraying technology. Considering that the effect of spraying ceramic particles by cold spraying technology is insufficient, coating sealing technology can be further used for processing.
[0048] In other embodiments, the spraying technology in step S4 may also be thermal spraying technology.
[0049] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A composite coating, characterized in that: include: Transition layer, connected to the surface of the substrate: An anti-corrosion layer connected to a surface of the transition layer away from the substrate: The hydrogen barrier coating is connected to the surface of the anti-corrosion layer away from the anti-corrosion layer.
2. The composite coating according to claim 1, characterized in that: The transition layer is an Al coating.
3. The composite coating according to claim 1, characterized in that: The anti-corrosion layer is an Al-Ni or Al-Cr coating.
4. The composite coating according to claim 1, characterized in that: The hydrogen barrier coating is Al2O3, Y2O3, Cr2O3 or ZrO2 coating.
5. The composite coating according to claim 1, characterized in that: The thickness of the composite coating is 100 μm-400 μm.
6. A method for preparing a composite coating, characterized in that: include: S1, pre-treating the substrate to be sprayed; S2, using the first powder and adopting cold spraying technology to prepare a transition layer on the surface of the substrate; S3, using the second powder and adopting the cold spraying technology to prepare the anti-corrosion layer on the transition layer; S4. Use the third powder and adopt the spraying technology to prepare the hydrogen barrier coating on the anti-corrosion layer.
7. The preparation method according to claim 6, characterized in that: The pretreatment uses sandblasting to remove oil and rust from the surface of the substrate.
8. The preparation method according to claim 7, characterized in that: The roughness of the substrate surface after pretreatment is 0.8-1 μm.
9. The preparation method according to claim 6, characterized in that: The first powder is Al powder, the second powder is Al-Ni alloy powder or Al-Cr alloy powder, and the third powder is ceramic powder.
10. The preparation method according to claim 9, characterized in that: Each powder was dried at 100-120°C before use.
Citation Information
Patent Citations
Corrosion-resisting heat-insulating coating system and preparation method thereof
CN107190260A
Composite hydrogen retention coating and preparation method thereof
CN110551984A