A corrosion inhibitor for storage tank wall in alkaline liquid environment and preparation method thereof
By combining modified polyaspartic acid with sodium tungstate, thiourea, sodium gluconate, hexamethyltetramine and zinc chloride, a synergistic reaction is formed, and the resistance of polyaspartic acid in alkaline seawater is solved. The problem of unstable scale effect achieves efficient corrosion inhibition and scale dispersion performance, extending the service life of marine storage tanks.
Patent Information
- Application Number
- CN202411244687.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-06
AI Technical Summary
In the prior art, polyaspartic acid has a scale inhibition effect in alkaline seawater environments that is easily affected by temperature, and a single corrosion inhibition performance is insufficient, making it difficult to meet the multi-faceted needs of marine storage tanks in practical applications.
Modified polyaspartic acid is used as the main agent for compound corrosion inhibitor, combining sodium tungstate, thiourea, sodium gluconate, hexamethyltetramine and zinc chloride to form a synergistic reaction to improve scale inhibition dispersion and long Effective corrosion inhibitory performance.
In an alkaline environment, it significantly extends the service life of the storage tank, inhibits the formation of scale such as calcium carbonate, reduces the economic losses caused by equipment failure, and achieves a more complete protective effect by forming a multi-layer protective structure.
Smart Images

Figure CN118756144B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of marine environmental corrosion and protection technology, and specifically relates to a corrosion inhibitor for a storage tank wall in an alkaline liquid environment and a preparation method thereof. Background Art
[0002] The chemical properties of seawater resources in the ocean have a significant impact on the equipment and structural materials in or in contact with them. Seawater is generally slightly alkaline, with a pH value that fluctuates roughly between 8 and 8.5. This alkaline environment is determined by a variety of dissolved salts and minerals in seawater, the most important of which is sodium chloride, but also includes other alkaline substances such as carbonates.
[0003] Marine storage tank applications are generally divided into offshore storage tanks and submarine storage tanks. Offshore storage tanks are usually installed on offshore platforms or ships for the development or transportation of offshore oil and gas fields. These tanks can resist the erosion of the marine environment and ensure the safety of stored materials; submarine storage tanks are storage facilities located completely below the water surface and are mainly used in marine engineering. They can make more efficient use of marine space while reducing the impact on the surface landscape.
[0004] When using marine storage tanks in the seawater field, it is necessary to consider the scaling and corrosion of marine storage tank materials in alkaline seawater environments. The above problems will shorten the life of marine storage tanks during actual use. In the prior art, polyaspartic acid (PASP) is a biodegradable and environmentally friendly scale inhibitor and dispersant with good scale inhibition and corrosion inhibition capabilities. It controls the crystal morphology by inhibiting the nucleation rate of calcium carbonate to distort the crystal structure, so that calcium carbonate and other crystals can no longer adhere to the tank wall surface to form scale. At the same time, it can form a protective film on the tank wall surface to inhibit the corrosion rate of the metal. However, PASP has a single functional group. When the seawater environment changes, such as when the temperature rises, its scale inhibition effect will deteriorate. In addition, the corrosion inhibition performance of a single PASP is general, and the scale inhibition and dispersibility performance and corrosion inhibition effect are far behind other corrosion inhibitors, making it difficult to meet the various needs of marine storage tanks in actual applications. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a corrosion inhibitor for the tank wall in an alkaline liquid environment and a preparation method thereof. The present invention uses modified polyaspartic acid as the main agent of the composite corrosion inhibitor, and selects sodium tungstate, thiourea, sodium gluconate, hexamethyltetramine, and zinc chloride to compound it, which can form a good synergistic reaction, has excellent scale inhibition and dispersibility and long-term corrosion inhibition performance, and meets the long-term use requirements of marine storage tanks.
[0006] The technical solutions adopted by the present invention to achieve the above-mentioned purpose are as follows:
[0007] A corrosion inhibitor for a storage tank wall in an alkaline liquid environment, the corrosion inhibitor comprising the following components in parts by mass: 30-50 parts of modified polyaspartic acid, 18-28 parts of sodium tungstate, 2-8 parts of thiourea, 2-10 parts of sodium gluconate, 10-30 parts of hexamethyltetramine, and 5-13 parts of zinc chloride;
[0008] The modified polyaspartic acid is aminosulfonic acid and amino acid modified polyaspartic acid.
[0009] Preferably, the corrosion inhibitor comprises the following components in parts by mass: 35-45 parts of modified polyaspartic acid, 20-25 parts of sodium tungstate, 4-6 parts of thiourea, 4-8 parts of sodium gluconate, 15-20 parts of hexamethyltetramine, and 7-10 parts of zinc chloride.
[0010] Optionally, the preparation steps of the modified polyaspartic acid include:
[0011] The polysuccinimide intermediate is stirred for the first time in an alkaline environment, and then aminosulfonic acid and amino acid are dissolved in an alkaline solution, and then the polysuccinimide intermediate mixed solution is added and stirred for the second time to obtain the aminosulfonic acid and amino acid modified polyaspartic acid.
[0012] Optionally, the aminosulfonic acid is any one of 3-aminobenzenesulfonic acid, 3-amino-1-propanesulfonic acid, and 2-aminoethanesulfonic acid; the amino acid is any one of L-histidine, lysine, and tryptophan;
[0013] Preferably, the aminosulfonic acid is 2-aminoethanesulfonic acid, and the amino acid is tryptophan.
[0014] Optionally, the molar ratio of the polysuccinimide intermediate to aminosulfonic acid and amino acid is (6-10):(2-4):(1-3);
[0015] Preferably, the molar ratio of the polysuccinimide intermediate to aminosulfonic acid and amino acid is 8:3:2.
[0016] Optionally, the first stirring is stirring at 25-40°C for 30-60 min; and the second stirring is stirring at 25-40°C for 20-24 h.
[0017] Optionally, the preparation steps of the polysuccinimide intermediate include:
[0018] After mixing maleic anhydride and ammonium salt in an alkaline environment, N,N-dimethylformamide is added, stirred and filtered to obtain a polysuccinimide intermediate;
[0019] The molar ratio of maleic anhydride to ammonium salt is 1:(1.6-1.8), and the molar amount of ammonium salt is calculated based on ammonium ions; the ammonium salt is ammonium sulfate, ammonium chloride, ammonium nitrate, and ammonium carbonate.
[0020] Preferably, the modified polyaspartic acid is aminosulfonic acid and the chemical structure of amino acid modified polyaspartic acid is as shown in Formula I:
[0021] Formula I;
[0022] Wherein, n and mn are both positive integers, n:mn=(1-3):(1-5) The total molecular weight range of the modified polyaspartic acid is 3000-5000.
[0023] The present invention also provides a method for preparing a corrosion inhibitor for a storage tank wall in an alkaline liquid environment. The corrosion inhibitor is prepared by uniformly mixing the components according to the following mass fractions: 30-50 parts of modified polyaspartic acid, 18-28 parts of sodium tungstate, 2-8 parts of thiourea, 2-10 parts of sodium gluconate, 10-30 parts of hexamethyltetramine, and 5-13 parts of zinc chloride.
[0024] Preferably, the corrosion inhibitor is prepared by uniformly mixing the components according to the following mass parts: 35-45 parts of modified polyaspartic acid, 20-25 parts of sodium tungstate, 4-6 parts of thiourea, 4-8 parts of sodium gluconate, 15-20 parts of hexamethyltetramine, and 7-10 parts of zinc chloride.
[0025] The present invention also provides a corrosion inhibitor for the wall of a storage tank in an alkaline liquid environment and / or a method for preparing a corrosion inhibitor for the wall of a storage tank in an alkaline liquid environment as described in any of the above items, and its application in corrosion and scale inhibition of the wall of a marine storage tank.
[0026] The beneficial effects of this application include but are not limited to:
[0027] 1. The present invention provides a corrosion inhibitor for the tank wall in an alkaline liquid environment, which has excellent scale dispersing and corrosion inhibition performance, and prolongs the service life of the tank in the marine alkaline environment. Modified polyaspartic acid is used as the main agent of the composite corrosion inhibitor, and sodium tungstate, thiourea, sodium gluconate, hexamethyltetramine, and zinc chloride are selected to be compounded with it, wherein thiourea, hexamethyltetramine, and sodium gluconate are adsorption film type corrosion inhibitors, sodium tungstate is an oxidation film type corrosion inhibitor, and zinc chloride is a precipitation film type corrosion inhibitor. A synergistic reaction is formed between the composite corrosion inhibitors to improve the corrosion inhibition efficiency in the alkaline environment, inhibit the formation of scale such as calcium carbonate, improve the dispersibility of iron oxide, prolong the life of the tank in the marine alkaline environment, and reduce the economic losses caused by equipment failure. At the same time, the corrosion inhibitors used are all environmentally friendly corrosion inhibitors and will not pollute the environment.
[0028] 2. The present invention first introduces aminosulfonic acid groups with strong hydrophilic properties and amino acid groups with excellent corrosion inhibition properties into the polyaspartic acid molecular chain, which can increase the content of carboxyl and sulfonic acid groups in the side chains of the polyaspartic acid molecular chain. The introduced sulfonic acid groups have active sites that can adsorb electrons on the metal surface and form an adsorption film on the outermost layer of the metal, which can further improve the corrosion inhibition effect of the modified polyaspartic acid in an alkaline environment. In addition, in addition to the polar groups such as amino and carboxyl groups forming an adsorption film on the outermost layer of the metal, some non-polar groups are also included that can form a hydrophobic film on the outermost layer of the metal, thereby preventing the charge transfer associated with the corrosion reaction from occurring, isolating the alkaline medium solution from the metal surface, and further improving the corrosion inhibition effect on the metal surface.
[0029] 3. The modified polyaspartic acid in the present invention can destroy the lattice structure of calcium carbonate in the marine environment, and at the same time, the modified polyaspartic acid can be adsorbed to the active growth points of CaCO3 crystals and bind to CaCO3. 2+ Chelating reaction inhibits the lattice growth direction of CaCO3 crystals; on the other hand, some modified polyaspartic acid components will enter the lattice structure along with the growth of CaCO3 crystals, causing dislocation and offset in the growth process of CaCO3 lattice structure. This process can change the scaling process of subsequent growth of CaCO3 from hard scale to soft scale, which can be easily washed away by seawater; at the same time, modified polyaspartic acid further provides carboxyl, sulfonic acid, imine and other groups, which can react with CaCO3 in the alkaline environment of seawater. 2+ Mg 2+ etc. to form a stable water-soluble complex, further increasing the scaling compound Ca 2+ Mg 2+ The solubility of salt can be increased, thereby inhibiting the deposition of scale. In addition, the introduction of sulfonic acid groups can further improve the dispersion performance of iron oxide.
[0030] 4. The thiourea and hexamethyltetramine in the corrosion inhibitor of the present invention can be adsorbed between the surface of the storage tank and the alkaline seawater interface. The nitrogen and sulfur atoms have paired electrons, which can further react with metal ions to squeeze out the water molecules on the surface of the metal ions to form a corrosion inhibition layer attached to the metal surface. At the same time, there is an energy barrier between the interfaces to prevent electron migration between the metal surface and the solution interface, thereby further improving the corrosion inhibition effect. Zinc chloride can also provide zinc ions, which can form a stable chelate with modified polyaspartic acid to increase the firmness of the corrosion inhibition film. Sodium gluconate belongs to a precipitation film type inhibitor. The corrosive agent can form precipitation adsorption with metal ions in alkaline seawater, and cooperate with the carboxyl and sulfonic acid groups in modified polyaspartic acid to change the charge distribution on the tank wall surface, and can form a more stable and denser protective film on the tank wall surface to reduce corrosion. Sodium tungstate contains tungstate, which can form a passivation film on the metal surface in the presence of dissolved oxygen, and cooperate with modified polyaspartic acid to form a stable organic film to complement each other, thereby forming a protective layer between the metal surface and the alkaline seawater interface. Sodium tungstate also has a compression effect on polyaspartic acid molecules, which can increase its effective coverage area on the metal surface.
[0031] 5. The present invention can form a multi-layer protective structure on the metal surface in alkaline seawater through a composite system composed of modified polyaspartic acid, sodium tungstate, thiourea, sodium gluconate, hexamethyltetramine, and zinc chloride components. The above protective structures can be superimposed and supplemented with each other, and a more complete protective system can be constructed on the tank wall; secondly, the composite system can further inhibit the formation of scale in alkaline seawater through chelation and dispersion, and can reduce the scale formation conditions by adjusting the ion balance in the solution; the composite system changes the properties of the metal surface such as the charge distribution and hydrophilicity of the tank wall surface through adsorption and chemical reaction, reduces the interaction between the metal surface and the corrosive medium or scaling ions, can obtain a long-term corrosion inhibition effect, and achieves good scale inhibition and dispersion performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0033] Figure 1 Infrared spectra of polyaspartic acid and modified polyaspartic acid prepared for this application. DETAILED DESCRIPTION
[0034] In order to more clearly illustrate the overall concept of the present invention, a detailed description is given below by way of examples.
[0035] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0036] In the following, the corrosion inhibitor for the tank wall in an alkaline liquid environment and the preparation method thereof of the present invention will be described in detail in combination with exemplary embodiments. A good corrosion inhibition rate can be achieved in an alkaline liquid environment, and the corrosion and scaling problems faced by the tank in the marine environment can be solved, and a good protection for the tank can be formed.
[0037] Example 1
[0038] This embodiment adopts the above preparation method to prepare a corrosion inhibitor, and the specific steps are as follows:
[0039] (1) Preparation of polysuccinimide intermediates
[0040] 9.8g of maleic anhydride was added to 100mL of distilled water, stirred, and heated to 60°C until the maleic anhydride was completely dissolved, and then the temperature was further raised to 100°C, and 8g of ammonium carbonate was added to react for 60min. The temperature was further raised to 200°C for high-temperature polycondensation for 40min, and the obtained product was dissolved in 100mL of N,N-dimethylformamide solution, and stirred in a constant temperature water bath at 60°C for 4h, then dehydrated and purified, and anhydrous ethanol was added for precipitation for 30min, and the polysuccinimide intermediate was obtained by filtration, washing, and drying.
[0041] (2) Preparation of modified polyaspartic acid
[0042] 6 g of polysuccinimide intermediate was dissolved in 50 mL of 10% NaOH, and stirred for 60 min at 25°C to obtain a polysuccinimide intermediate mixed solution. 2 g of 2-aminoethanesulfonic acid and 1 g of tryptophan were dissolved in 50 mL of 10% NaOH, respectively, and after 50 min of reaction, the polysuccinimide intermediate mixed solution was added, and the reaction was continued at 40°C for 20 h to obtain a product solution. After the reaction was completed, the product solution was adjusted to neutral with 5 mol / L hydrochloric acid, and anhydrous ethanol was added to generate a precipitate, which was dried to obtain modified polyaspartic acid.
[0043] (3) Preparation of compound corrosion inhibitor
[0044] After mixing according to the following mass parts at a temperature of 25° C., a composite corrosion inhibitor is obtained, wherein: 45 parts of modified polyaspartic acid, 20 parts of sodium tungstate, 6 parts of thiourea, 8 parts of sodium gluconate, 15 parts of hexamethyltetramine, and 10 parts of zinc chloride.
[0045] Example 2
[0046] This embodiment adopts the above preparation method to prepare a corrosion inhibitor, and the specific steps are as follows:
[0047] (1) Preparation of polysuccinimide intermediates
[0048] 9.8g of maleic anhydride was added to 100mL of distilled water, stirred, and heated to 60°C until all the maleic anhydride was dissolved, and then the temperature was further raised to 100°C, and 16g of ammonium chloride was added to react for 60min. The temperature was further raised to 200°C for high-temperature polycondensation for 40min, and the obtained product was dissolved in 100mL of N,N-dimethylformamide solution, and stirred in a constant temperature water bath at 60°C for 4h, then dehydrated and purified, and anhydrous ethanol was added for precipitation for 30min, and the polysuccinimide intermediate was obtained by filtration, washing, and drying.
[0049] (2) Preparation of modified polyaspartic acid
[0050] 8 g of polysuccinimide intermediate was dissolved in 50 mL of 10% NaOH, and stirred for 40 min at 30°C to fully mix to obtain a polysuccinimide intermediate mixed solution. 3 g of 2-aminoethanesulfonic acid and 2 g of tryptophan were dissolved in 50 mL of 10% NaOH, respectively, and after 50 min of reaction, the polysuccinimide intermediate mixed solution was added, and the reaction was continued at 30°C for 22 h to obtain a product solution. After the reaction was completed, the product solution was adjusted to neutral with 5 mol / L hydrochloric acid, and anhydrous ethanol was added to generate a precipitate, which was dried to obtain modified polyaspartic acid.
[0051] (3) Preparation of compound corrosion inhibitor
[0052] After mixing according to the following mass parts at a temperature of 25° C., a composite corrosion inhibitor is obtained, wherein: 40 parts of modified polyaspartic acid, 23 parts of sodium tungstate, 5 parts of thiourea, 6 parts of sodium gluconate, 18 parts of hexamethyltetramine, and 8 parts of zinc chloride.
[0053] Example 3
[0054] This embodiment adopts the above preparation method to prepare a corrosion inhibitor, and the specific steps are as follows:
[0055] (1) Preparation of polysuccinimide intermediates
[0056] 9.8g of maleic anhydride was added to 100mL of distilled water, stirred, heated to 60°C until all maleic anhydride was dissolved, and then heated to 100°C, and 8g of ammonium sulfate was added to react for 60min. The temperature was further raised to 200°C for high-temperature polycondensation for 40min, and the obtained product was dissolved in 100mL of N,N-dimethylformamide solution, and stirred in a constant temperature water bath at 60°C for 4h, then dehydrated and purified, and anhydrous ethanol was added for precipitation for 30min, and the polysuccinimide intermediate was obtained by filtration, washing, and drying.
[0057] (2) Preparation of modified polyaspartic acid
[0058] 10 g of polysuccinimide intermediate was dissolved in 50 mL of 10% NaOH, and stirred at 40°C for 30 min to fully mix to obtain a polysuccinimide intermediate mixed solution. 4 g of 2-aminoethanesulfonic acid and 3 g of tryptophan were dissolved in 50 mL of 10% NaOH, respectively, and after 50 min of reaction, the polysuccinimide intermediate mixed solution was added, and the reaction was continued at 25°C for 24 h to obtain a product solution. After the reaction was completed, the product solution was adjusted to neutral with 5 mol / L hydrochloric acid, and anhydrous ethanol was added to generate a precipitate, which was dried to obtain modified polyaspartic acid.
[0059] (3) Preparation of compound corrosion inhibitor
[0060] After mixing according to the following mass parts at a temperature of 25° C., a composite corrosion inhibitor is obtained, wherein: 35 parts of modified polyaspartic acid, 25 parts of sodium tungstate, 4 parts of thiourea, 4 parts of sodium gluconate, 20 parts of hexamethyltetramine, and 7 parts of zinc chloride.
[0061] Example 4
[0062] This embodiment adopts the above preparation method to prepare a corrosion inhibitor, and the specific steps are as follows:
[0063] (1) Preparation of polysuccinimide intermediates
[0064] 9.8g of maleic anhydride was added to 100mL of distilled water, stirred, and heated to 60°C until the maleic anhydride was completely dissolved, and then the temperature was further raised to 100°C, and 16g of ammonium nitrate was added for reaction for 60min. The temperature was further raised to 200°C for high-temperature polycondensation for 40min, and the obtained product was dissolved in 100mL of N,N-dimethylformamide solution, and stirred in a constant temperature water bath at 60°C for 4h, then dehydrated and purified, and anhydrous ethanol was added for precipitation for 30min, and the polysuccinimide intermediate was obtained by filtration, washing, and drying.
[0065] (2) Preparation of modified polyaspartic acid
[0066] 7 g of polysuccinimide intermediate was dissolved in 50 mL of 10% NaOH, and stirred for 40 min at 30°C to fully mix to obtain a polysuccinimide intermediate mixed solution. 3 g of 3-aminobenzenesulfonic acid and 2 g of lysine were dissolved in 50 mL of 10% NaOH, respectively, and after 50 min of reaction, the polysuccinimide intermediate mixed solution was added, and the reaction was continued at 30°C for 24 h to obtain a product solution. After the reaction was completed, the product solution was adjusted to neutral with 5 mol / L hydrochloric acid, and anhydrous ethanol was added to generate a precipitate, which was dried to obtain modified polyaspartic acid.
[0067] (3) Preparation of compound corrosion inhibitor
[0068] After mixing according to the following mass parts at a temperature of 25° C., a composite corrosion inhibitor is obtained, wherein: 30 parts of modified polyaspartic acid, 28 parts of sodium tungstate, 2 parts of thiourea, 2 parts of sodium gluconate, 10 parts of hexamethyltetramine, and 13 parts of zinc chloride.
[0069] Example 5
[0070] This embodiment adopts the above preparation method to prepare a corrosion inhibitor, and the specific steps are as follows:
[0071] (1) Preparation of polysuccinimide intermediates
[0072] 9.8g of maleic anhydride was added to 100mL of distilled water, stirred, and heated to 60°C until the maleic anhydride was completely dissolved, and then the temperature was further raised to 100°C, and 8g of ammonium carbonate was added to react for 60min. The temperature was further raised to 200°C for high-temperature polycondensation for 40min, and the obtained product was dissolved in 100mL of N,N-dimethylformamide solution, and stirred in a constant temperature water bath at 60°C for 4h, then dehydrated and purified, and anhydrous ethanol was added for precipitation for 30min, and the polysuccinimide intermediate was obtained by filtration, washing, and drying.
[0073] (2) Preparation of modified polyaspartic acid
[0074] 6 g of polysuccinimide intermediate was dissolved in 50 mL of 10% NaOH, and stirred for 30 min at 25°C to obtain a polysuccinimide intermediate mixed solution. 2 g of 3-amino-1-propane sulfonic acid and 1 g of L-histidine were dissolved in 50 mL of 10% NaOH, respectively, and after 50 min of reaction, the polysuccinimide intermediate mixed solution was added, and the reaction was continued at 40°C for 24 h to obtain a product solution. After the reaction was completed, the product solution was adjusted to neutral with 5 mol / L hydrochloric acid, and anhydrous ethanol was added to generate a precipitate, which was dried to obtain modified polyaspartic acid.
[0075] (3) Preparation of compound corrosion inhibitor
[0076] After mixing according to the following mass parts at a temperature of 25° C., a composite corrosion inhibitor is obtained, wherein: 50 parts of modified polyaspartic acid, 18 parts of sodium tungstate, 8 parts of thiourea, 10 parts of sodium gluconate, 30 parts of hexamethyltetramine, and 5 parts of zinc chloride.
[0077] Comparative Example 1
[0078] In this comparative example, a comparative composite corrosion inhibitor was prepared by the same preparation method as in Example 2. The difference from Example 2 is that in step (2), 2-aminoethanesulfonic acid and tryptophan are not added to modify the polyaspartic acid to obtain an unmodified polyaspartic acid product, thereby obtaining a composite corrosion inhibitor.
[0079] Comparative Example 2
[0080] In this comparative example, a comparative composite corrosion inhibitor was prepared by the same preparation method as in Example 2. The difference from Example 2 is that in step (2), 2-aminoethanesulfonic acid and tryptophan are not added to modify the polyaspartic acid, but 3 g of diethyl malonate dissolved in 50 mL of 10% NaOH is added to modify the polyaspartic acid to prepare a diethyl malonate-modified polyaspartic acid product, which is then compounded to obtain the final corrosion inhibitor.
[0081] Comparative Example 3
[0082] In this comparative example, a comparative composite corrosion inhibitor was prepared by the same preparation method as in Example 2. The difference from Example 2 is that in step (2), 2-aminoethanesulfonic acid and tryptophan are not added to modify the polyaspartic acid, but 2 g of aminomethanesulfonic acid is added and dissolved in 50 mL of 10% NaOH to modify the polyaspartic acid, thereby preparing an aminomethanesulfonic acid-modified polyaspartic acid product, which is then compounded to obtain the final corrosion inhibitor.
[0083] Comparative Example 4
[0084] In this comparative example, a comparative composite corrosion inhibitor was prepared by the same preparation method as in Example 2. The difference from Example 2 is that hexamethyltetramine and thiourea components were not added to the composite corrosion inhibitor.
[0085] Comparative Example 5
[0086] In this comparative example, a comparative compound corrosion inhibitor is prepared by the same preparation method as in Example 2. The difference from Example 2 is that no sodium tungstate component is added to the compound corrosion inhibitor.
[0087] Comparative Example 6
[0088] In this comparative example, a comparative composite corrosion inhibitor was prepared by the same preparation method as in Example 2. The difference from Example 2 is that no zinc chloride component was added to the composite corrosion inhibitor.
[0089] Comparative Example 7
[0090] In this comparative example, a comparative compound corrosion inhibitor was prepared by the same preparation method as in Example 2. The difference from Example 2 is that no sodium gluconate component was added to the compound corrosion inhibitor.
[0091] Comparative Example 8
[0092] In this comparative example, a comparative compound corrosion inhibitor was prepared by the same preparation method as in Example 2. The difference from Example 2 is that the mass fractions of the compound corrosion inhibitor are: 20 parts of modified polyaspartic acid, 10 parts of sodium tungstate, 20 parts of thiourea, 15 parts of sodium gluconate, 35 parts of hexamethyltetramine, and 20 parts of zinc chloride.
[0093] Comparative Example 9
[0094] In this comparative example, a comparative compound corrosion inhibitor was prepared by the same preparation method as in Example 2. The difference from Example 2 is that the mass components of the compound corrosion inhibitor are: 60 parts of modified polyaspartic acid, 13 parts of sodium tungstate, 1 part of thiourea, 1 part of sodium gluconate, 5 parts of hexamethyltetramine, and 20 parts of zinc chloride.
[0095] Experiment 1. Infrared Characterization of Modified Polyaspartic Acid
[0096] The unmodified polyaspartic acid prepared in Comparative Example 1 and the modified polyaspartic acid prepared in Example 2 were prepared by the KBR tableting method and then scanned by an infrared scanner with a scanning range of 4000-500 cm -1 , where the horizontal axis is the wave number (cm -1 ), the vertical axis is the transmittance (%). The scanning results are as follows Figure 1 As shown, 1 is the infrared spectrum of unmodified polyaspartic acid, and 2 is the infrared spectrum of polyaspartic acid modified with 2-aminoethanesulfonic acid and tryptophan.
[0097] From the infrared spectrum of polyaspartic acid, we can see that at 3435cm -1 The vicinity is the stretching vibration of NH in -CONH-, and 1621cm -1 The absorption peak at 1395cm is the stretching vibration of the C=O bond in the amide. -1 The absorption peaks at are the NH bending vibration in -CONH- and the stretching vibration of CN, indicating that polyaspartic acid was successfully synthesized.
[0098] The infrared spectra of 2-aminoethanesulfonic acid and tryptophan-modified polyaspartic acid have three peaks in addition to the above three peaks, and another peak at 1045 cm -1 and 647cm -1 The absorption peaks of -S=O and CS in the sulfonic acid group are at 3403cm -1 The strong peak at 867cm is the absorption peak of NH in the amide group, which is offset compared with the absorption peak of NH in the amide group of polyaspartic acid. -1 The absorption peak of the benzene ring is at , indicating that tryptophan is successfully grafted onto the side chain of polyaspartic acid; the above data prove that the synthesis of 2-aminoethanesulfonic acid and tryptophan-modified polyaspartic acid is successful.
[0099] Test 2. Corrosion inhibition rate test
[0100] 2.1 Test method: The corrosion inhibition efficiency was determined by the coupon weight loss method.
[0101] A steel sheet (50 mm × 25 mm × 2 mm) made of 907A steel was selected, washed with anhydrous ethanol, dried and weighed; the weighed steel sheet was immersed in natural seawater for 10 days and then taken out for rinsing (the pH value of natural seawater was about 8.5); the corrosion inhibitors prepared in Examples 1-5 and Comparative Examples 1-9 were respectively formulated into 12 mg / L rinsing liquid, and the steel sheet rinsed after immersion was placed in 300 mL of rinsing liquid and soaked for 15 minutes; then placed in a salt spray box and hung for 30 days (temperature 25°C, humidity 85RH%); after placement, a steel sheet was taken out on the 10th day, 20th day and 30th day, and rinsed and dehydrated with 10% hydrochloric acid lotion, tap water and anhydrous ethanol in turn, and weighed after drying and the corrosion inhibition rate was calculated; the steel sheet not immersed in the rinsing liquid was the control steel sheet;
[0102] Corrosion inhibition rate = (mass loss of control steel sheet - mass loss of experimental group steel sheet) / mass loss of control steel sheet x 100%.
[0103] 2.2 Test results:
[0104] Table 1 Corrosion inhibition rate of the corrosion inhibitors obtained in Examples 1-5 and Comparative Examples 1-9
[0105] sample 10-day corrosion inhibition rate (%) 20-day corrosion inhibition rate (%) 30-day corrosion inhibition rate (%) Example 1 90.21 88.38 82.49 Example 2 93.85 92.96 89.53 Example 3 89.86 88.21 83.56 Example 4 88.79 85.78 82.77 Example 5 89.37 86.1 81.83 Comparative Example 1 65.57 52.68 36.79 Comparative Example 2 73.38 62.85 49.32 Comparative Example 3 70.79 59.13 45.47 Comparative Example 4 80.25 74.93 67.61 Comparative Example 5 81.37 76.16 68.95 Comparative Example 6 81.36 76.19 69.02 Comparative Example 7 81.59 76.03 67.47 Comparative Example 8 76.81 70.29 63.76 Comparative Example 9 82.97 78.58 73.19
[0106] From the vertical comparison in Table 1, it can be seen that the corrosion inhibition efficiency of the corrosion inhibitors prepared in Examples 1-3 is relatively close, and is higher than the corrosion inhibition rate of the corrosion inhibitors prepared from the other components, indicating that the corrosion inhibition effect of the modified polyaspartic acid in the alkaline seawater environment is better than that of the other components, especially the unmodified polyaspartic acid component; the corrosion inhibition efficiency of the corrosion inhibitors prepared in Examples 4-5 is higher than that of the comparative example components, indicating that modified polyaspartic acid is used as the compounding main agent, and sodium tungstate, thiourea, sodium gluconate, hexamethyltetramine, and zinc chloride components are selected and compounded in a certain mass fraction, which can fully improve the corrosion inhibition efficiency of marine storage tanks in an alkaline seawater environment. Comparative Example 1 is a composite corrosion inhibitor of unmodified polyaspartic acid, and Comparative Examples 2 and 3 are composite corrosion inhibitors prepared by using only one of aminosulfonic acid and amino acid as a modifier as the main agent. The corrosion inhibition efficiency of the above Comparative Examples 1-3 is far lower than that of Example 2, indicating that the polyaspartic acid is not modified or the polyaspartic acid is modified by using one of diethyl malonate and aminomethanesulfonic acid, and the prepared composite corrosion inhibitor has limited improvement in the corrosion inhibition efficiency of the corrosion inhibitor for marine storage tanks; this is because, on the one hand, the molecular chain side chains of the modified polyaspartic acid contain carboxyl and sulfonic acid groups at the same time, which have active sites that can adsorb electrons on the metal surface, forming an adsorption film on the outermost layer of the metal, thereby reducing the corrosion rate; in addition, some non-polar groups adsorbed on the metal surface can form a hydrophobic film on the outermost layer of the metal, organize the electron migration related to the corrosion reaction, isolate the alkaline seawater solution from the metal surface, and slow down the corrosion rate of the metal surface.
[0107] The corrosion inhibition efficiency of the corrosion inhibitor for marine storage tanks obtained in Comparative Examples 4-7 is lower than that of the corrosion inhibition efficiency of the corrosion inhibitor obtained in Example 2, indicating that the corrosion inhibition efficiency of the compound corrosion inhibitor will be reduced in the absence of any component of sodium tungstate, thiourea, sodium gluconate, hexamethyltetramine, and zinc chloride, and the compound corrosion inhibitors have not formed a good synergistic effect. Among them, sodium tungstate, when compounded with modified polyaspartic acid, can effectively compress the modified polyaspartic acid molecules, increase the effective coverage area, and generate a passivation film in the presence of dissolved oxygen. At the same time, compounding with thiourea further changes the charge distribution on the metal surface and promotes the formation of a passivation film; sodium gluconate can form a dense and stable protective film on the metal surface to prevent corrosion from occurring; hexamethyltetramine can be adsorbed on the metal surface with thiourea to prevent electrons from transferring between the metal surface and seawater, thereby reducing the corrosion rate; zinc chloride can form a stable chelate with modified polyaspartic acid to increase the firmness of the corrosion inhibition film.
[0108] The corrosion inhibition efficiency of the corrosion inhibitor for marine storage tanks prepared in Comparative Examples 8-9 is lower than that of the corrosion inhibition efficiency of the corrosion inhibitor prepared in Example 2, indicating that when the content of the modified polyaspartic acid component is too much, it will cause supersaturated adsorption of the modified polyaspartic acid on the metal surface, and will not continue to increase the corrosion inhibition efficiency. At the same time, it will also affect the adsorption capacity of thiourea, hexamethyltetramine or sodium gluconate on the metal surface, and will compete with the remaining components for adsorption sites, resulting in other effective corrosion inhibitor components cannot be fully adsorbed on the metal surface, affecting the corrosion inhibition efficiency; when the content of the modified polyaspartic acid component is too low, it will affect the film-forming ability, making the protective film incomplete or weak, resulting in an increase in the contact area between the metal and the corrosive medium, and the corrosive medium can more easily penetrate into the metal surface, reducing the corrosion inhibition efficiency.
[0109] A horizontal comparison of the corrosion inhibition rates of the compound corrosion inhibitors at the 10th, 20th and 30th days shows that the rate of decrease in the corrosion inhibition rate of the corrosion inhibitors for marine storage tanks prepared in Examples 1-3 is much lower than that of the corrosion inhibitors prepared in the comparative examples, indicating that the modified polyaspartic acid can maintain a longer stability when used in combination with the various components, thereby further extending the protection life of the marine storage tanks.
[0110] Test 3. Scale inhibition and dispersibility test
[0111] 3.1 Test method:
[0112] 3.1.1 Test for calcium carbonate scale inhibition performance: Take 14 500mL flasks as reagent bottles, and prepare 100mL of salt solution in each reagent bottle according to the test solution preparation steps, where Ca 2+ The concentration is 500 mg / L, HCO 3- The concentration was 1000 mg / L, and 100 mL of the corrosion inhibitor prepared in Example 1-5 was added to bottles 1-5, with a concentration of 12 mg / L, and 100 mL of the corrosion inhibitor prepared in Comparative Example 1-9 was added to bottles 6-14, with a concentration of 12 mg / L. After adjusting the pH to 9 and keeping the mixture in a constant temperature water bath at 80°C for 10 hours, the filtrate was taken and Ca was determined by ion chromatography. 2+ Concentration, calculate the calcium carbonate scale inhibition rate.
[0113] 3.1.2 Calcium sulfate scale inhibition performance test: Take 14 500mL flasks as reagent bottles, and prepare 100mL of salt solution in each reagent bottle according to the test solution preparation steps, including Ca 2+ Concentration is 500mg / L, SO4 2-The concentration was 500 mg / L, and 100 mL of the corrosion inhibitor prepared in Example 1-5 was added to bottles 1-5, with a concentration of 12 mg / L, and 100 mL of the corrosion inhibitor prepared in Comparative Example 1-9 was added to bottles 6-14, with a concentration of 12 mg / L. After adjusting the pH to 9 and keeping the mixture in a constant temperature water bath at 80°C for 10 hours, the filtrate was taken and Ca was determined by ion chromatography. 2+ Concentration, calculate the calcium sulfate scale inhibition rate.
[0114] 3.1.3 Dispersible iron oxide performance test: Take 14 500mL flasks as reagent bottles, and prepare 100mL of salt solution in each reagent bottle according to the test solution preparation steps, including Ca 2+ The concentration is 200 mg / L, Fe 2+ The concentration is 30 mg / L, and 100 mL of the corrosion inhibitor prepared in Example 1-5 is added to bottles 1-5, with a concentration of 12 mg / L, and 100 mL of the corrosion inhibitor prepared in Comparative Example 1-9 is added to bottles 6-14, with a concentration of 12 mg / L. The pH is adjusted to 9, and the mixture is placed at a constant temperature of 60°C for 5 hours. The transmittance is measured by spectrophotometry. The smaller the transmittance, the better the dispersion effect.
[0115] 3.2 Test results:
[0116] Table 2 Scale inhibition and dispersion performance of the corrosion inhibitors prepared in Examples 1-5 and Comparative Examples 1-9
[0117] sample Calcium carbonate scale inhibition rate% Calcium sulfate scale inhibition rate% Transmittance% Example 1 94.4 90.3 36.9 Example 2 97.5 93.5 34.6 Example 3 94.1 90.7 36.7 Example 4 93.8 89.6 38.3 Example 5 93.7 89.3 38.5 Comparative Example 1 57.7 54.1 71.3 Comparative Example 2 68.7 64.4 60.8 Comparative Example 3 67.6 63.3 61.5 Comparative Example 4 85.3 79.9 53.6 Comparative Example 5 86.9 81.4 50.3 Comparative Example 6 86.6 81.1 51.2 Comparative Example 7 85.7 80.3 52.9 Comparative Example 8 90.6 84.9 45.1 Comparative Example 9 91.3 86.5 40.3
[0118] Analysis of calcium carbonate scale inhibition rate: The above test was performed on the compound corrosion inhibitor samples prepared by Examples 1-5 and Comparative Examples 1-9, and the results are shown in Table 2. As can be seen from Table 2, Examples 1-5 can all achieve a relatively high calcium carbonate scale inhibition rate, indicating that the corrosion inhibitor obtained by modifying polyaspartic acid and compounding the present invention has good scale inhibition performance. Compared with Example 2, the scale inhibition performance of Comparative Example 1-3 is significantly reduced. This is because the modified polyaspartic acid has more carboxyl groups and sulfonic acid groups in the structure, and the formation of CaCO3 scale is essentially a heterogeneous nucleation crystallization process at the interface between metal and alkaline seawater. After the modified polyaspartic acid containing carboxylic acid groups and sulfonic acid groups is adsorbed during the crystallization process, a double electric layer will be formed on the surface of the crystal particles, changing the charge state of the crystal particles surface, preventing the particles from continuing to grow and deposit on the metal surface after collision, and at the same time causing the CaCO3 lattice structure growth process to shift, destroying the crystal orientation of the CaCO3 crystal during the growth process, and further promoting its solubility in water. Compared with Example 2, the scale inhibition performance of Example 4 is significantly reduced, indicating that hexamethyltetramine and thiourea components can improve the scale inhibition performance of CaCO3 to a certain extent; compared with Example 2, the scale inhibition performance of Example 5 is significantly reduced, indicating that the sodium tungstate component can improve the scale inhibition performance of CaCO3 to a certain extent; compared with Example 2, the scale inhibition performance of Example 6 is significantly reduced, indicating that the zinc chloride component can improve the scale inhibition performance of CaCO3 to a certain extent; compared with Example 2, the scale inhibition performance of Example 7 is significantly reduced, indicating that the sodium gluconate component can improve the scale inhibition performance of CaCO3 to a certain extent. Compared with Example 2, the scale inhibition performance of CaCO3 in Examples 8-9 is also reduced. When the amount of the modified polyaspartic acid component is too much, it will lead to the formation of too many adsorption layers or the complex will occupy too many crystal growth sites to affect the overall scale inhibition effect. When the amount of the modified polyaspartic acid component is too little, the inhibitory effect on CaCO3 scale will be reduced, and calcium ions are more likely to combine with carbonate to form scale.
[0119] Analysis of calcium sulfate scale inhibition rate: The above test was performed on the compound corrosion inhibitor samples prepared by Examples 1-5 and Comparative Examples 1-9, and the results are shown in Table 2. As can be seen from Table 2, Examples 1-5 can all achieve a relatively high calcium sulfate scale inhibition rate, indicating that the corrosion inhibitor prepared by the present invention has good scale inhibition performance. Compared with Example 2, the scale inhibition performance of Comparative Example 1-3 is significantly reduced, indicating that the modified polyaspartic acid can effectively improve the scale inhibition performance for calcium sulfate, and the single modified polyaspartic acid has a certain improvement in the scale inhibition performance for calcium sulfate; Compared with Example 2, the scale inhibition performance of Comparative Example 4 is significantly reduced, indicating that hexamethyltetramine and thiourea components can have a certain improvement in the scale inhibition performance of calcium sulfate; Compared with Example 2, the scale inhibition performance of Comparative Example 5 is significantly reduced, indicating that the sodium tungstate component can improve the scale inhibition performance of calcium sulfate. can be improved to a certain extent; compared with Example 2, the scale inhibition performance of Example 6 is significantly reduced in Example 6, indicating that the zinc chloride component can improve the scale inhibition performance of calcium sulfate to a certain extent; compared with Example 2, the scale inhibition performance of Example 7 is significantly reduced in Example 7, indicating that the sodium gluconate component can improve the scale inhibition performance of calcium sulfate to a certain extent; compared with Example 2, the scale inhibition performance of Examples 8-9 is significantly reduced in Examples 8-9, indicating that the reasonable mass fraction ratio between modified polyaspartic acid and each component can achieve good scale inhibition performance for calcium sulfate.
[0120] Transmittance analysis: The above test was performed on the compound corrosion inhibitor samples prepared by Examples 1-5 and Comparative Examples 1-9, and the results are shown in Table 2. As can be seen from Table 2, Examples 1-5 can all achieve lower transmittances, indicating that the corrosion inhibitor prepared by the present invention has good dispersion transmittance, especially the corrosion inhibitor prepared by Example 2 has the best dispersion transmittance. Compared with Example 2, Comparative Examples 1-3 have increased transmittance and reduced dispersion ability. This is because a double electric layer will be formed on the surface of the small crystal particles adsorbing the corrosion inhibitor, thereby changing the surface charge state of the particles, and the charge of the modified polyaspartic acid is more than that of the unmodified polyaspartic acid. Under the action of electrostatics, the particles repel each other, which can better avoid the particles from colliding and growing and then depositing, and the particles are better dispersed in water. Compared with the system modified by only diethyl malonate and aminomethanesulfonic acid single groups, the introduction of aminosulfonic acid and amino acid groups in the molecular structure of polyaspartic acid can better improve the ability to disperse iron oxide. Compared with Example 2, the transmittance of Comparative Example 4 is significantly increased, and the dispersion rate is reduced, indicating that the addition of hexamethyltetramine and thiourea components in the system can improve the dispersion performance of iron oxide by surface adsorption or complexation; Compared with Example 2, the transmittance of Comparative Example 5 is significantly increased, and the dispersion rate is reduced. No sodium tungstate component is added to the system of Comparative Example 5, and tungstate ions can form a stable adsorption layer for iron oxide particles, improving the dispersion effect. In addition, sodium tungstate, thiourea, and hexamethyltetramine work together to oxidize iron to form a stable dispersion system; Compared with Example 2, the transmittance of Comparative Example 6 is significantly increased, and the dispersion rate is reduced. No sodium gluconate component is added to the components of Comparative Example 6. Sodium gluconate has a carboxyl group that can react with iron oxide. The surface metal ions act to form an adsorption layer, reduce the agglomeration between particles, and improve the dispersibility of iron oxide; compared with Example 2, the transmittance of Comparative Example 7 is significantly increased, and the dispersion rate is reduced. No zinc chloride component is added to the components of Comparative Example 7. The zinc ions can form coordination bonds with the oxygen atoms in the iron oxide, change the surface charge state and polarity, and help to disperse; tungstate ions can form a stable adsorption layer for the iron oxide particles and improve the dispersion effect. In addition, sodium tungstate, thiourea, and hexamethyltetramine work together to oxidize iron to form a stable dispersion system; compared with Example 2, the transmittance of Comparative Examples 8-9 is significantly increased, that is, the dispersion rate is reduced, indicating that the reasonable ratio between the modified polyaspartic acid and each component can achieve good dispersion performance of iron oxide.
[0121] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.
Claims
1. A corrosion inhibitor for the wall of a storage tank in an alkaline liquid environment, characterized in that: The corrosion inhibitor comprises the following components in parts by mass: 30-50 parts of modified polyaspartic acid, 18-28 parts of sodium tungstate, 2-8 parts of thiourea, 2-10 parts of sodium gluconate, 10-30 parts of hexamethyltetramine, and 5-13 parts of zinc chloride; The modified polyaspartic acid is aminosulfonic acid and amino acid modified polyaspartic acid; The preparation steps of the modified polyaspartic acid include: The polysuccinimide intermediate is stirred for the first time in an alkaline environment, and then the aminosulfonic acid and the amino acid are dissolved in the alkaline solution, and then the polysuccinimide intermediate mixed solution is added and stirred for the second time to obtain the aminosulfonic acid and amino acid modified polyaspartic acid; The aminosulfonic acid is any one of 3-aminobenzenesulfonic acid, 3-amino-1-propanesulfonic acid, and 2-aminoethanesulfonic acid; the amino acid is any one of L-histidine, lysine, and tryptophan; The molar ratio of the polysuccinimide intermediate to aminosulfonic acid and amino acid is (6-10): (2-4): (1-3).
2. The corrosion inhibitor according to claim 1, characterized in that The corrosion inhibitor comprises the following components in parts by mass: 35-45 parts of modified polyaspartic acid, 20-25 parts of sodium tungstate, 4-6 parts of thiourea, 4-8 parts of sodium gluconate, 15-20 parts of hexamethyltetramine, and 7-10 parts of zinc chloride.
3. A corrosion inhibitor as claimed in claim 1, characterized in that: The aminosulfonic acid is 2-aminoethanesulfonic acid, and the amino acid is tryptophan.
4. A corrosion inhibitor as claimed in claim 1, characterized in that: The molar ratio of the polysuccinimide intermediate to aminosulfonic acid and amino acid is 8:3:
2.
5. A corrosion inhibitor as claimed in claim 1, characterized in that: The first stirring is specifically stirring at 25-40° C. for 30-60 min; the second stirring is specifically stirring at 25-40° C. for 20-24 h.
6. A corrosion inhibitor as claimed in claim 1, characterized in that: The preparation steps of the polysuccinimide intermediate include: After mixing maleic anhydride and ammonium salt in an alkaline environment, N,N-dimethylformamide is added, stirred and filtered to obtain a polysuccinimide intermediate; The molar ratio of maleic anhydride to ammonium salt is 1:(1.6-1.8), and the molar amount of ammonium salt is calculated based on ammonium ions; the ammonium salt is any one of ammonium sulfate, ammonium chloride, ammonium nitrate and ammonium carbonate.
7. A corrosion inhibitor as claimed in claim 1, characterized in that: The modified polyaspartic acid is aminosulfonic acid and the chemical structural formula of amino acid modified polyaspartic acid is shown in Formula I: Formula I; Wherein, n and mn are both positive integers, n:mn=(1-3):(1-5), and the total molecular weight of the modified polyaspartic acid is in the range of 3000-5000.
8. A method for preparing a corrosion inhibitor for a storage tank wall in an alkaline liquid environment, characterized in that: The corrosion inhibitor is prepared by uniformly mixing the components according to the following mass parts, wherein the modified polyaspartic acid is 30-50 parts, sodium tungstate is 18-28 parts, thiourea is 2-8 parts, sodium gluconate is 2-10 parts, hexamethyltetramine is 10-30 parts, and zinc chloride is 5-13 parts.
9. Application of the corrosion inhibitor for the wall of a storage tank in an alkaline liquid environment as described in any one of claims 1 to 7 and / or the corrosion inhibitor prepared by the preparation method of the corrosion inhibitor for the wall of a storage tank in an alkaline liquid environment as described in claim 8 in corrosion inhibition and scale prevention of the wall of a marine storage tank.
Citation Information
Cited By
An immobilized lipase and its application in catalytic preparation of monoglyceride and diglyceride
CN119265161B