Down jacket fabric with aerogel coating

Through the resurgence and heat treatment of silica airgel particles, combined with isoamyl alcohol vapor and high-pressure auxiliary conditions, the problem of low mechanical strength of the airgel coating is solved, and the warmth and wear resistance of down jacket fabrics are improved.

CN118756500AActive Publication Date: 2024-10-11GAOFAN (ZHEJIANG) INFORMATION TECH CO LTD

Patent Information

Application Number
CN202410752316.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-11
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

The existing airgel-coated down jacket fabrics have low mechanical strength and are easily scratched, damaged and worn, resulting in a decrease in thermal insulation performance and aesthetics.

Method used

Modified silica airgel particles that have undergone moisture resurgence treatment and heat treatment are used to achieve a moisture regain rate of 8-12%, and are heated to 800-850°C in a nitrogen atmosphere for heat treatment, transforming into crystals, and improving the mechanical strength, and uses isoamyl alcohol vapor and high-pressure auxiliary conditions during the moisture regain process to reduce the surface tension of the particles and improve compatibility.

Benefits of technology

The mechanical strength of the airgel coating is significantly improved to avoid scratches, pressure losses and abrasions, while maintaining the thermal insulation properties of the airgel and enhancing the wear resistance and aesthetics of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756500A_ABST
    Figure CN118756500A_ABST
Patent Text Reader

Abstract

The invention discloses a down jacket fabric with an aerogel coating, the down jacket fabric comprises a basic fabric and the aerogel coating coated on at least one surface of the basic fabric, the aerogel coating is prepared from the following raw materials: 40-80 wt% of a coating matrix, 10-25 wt% of modified silicon dioxide aerogel particles and 10-35 wt% of an auxiliary agent, the modified silicon dioxide aerogel particles are obtained by sequentially carrying out moisture regaining treatment and heat treatment on silicon dioxide aerogel particles. The modified silicon dioxide aerogel particles adopted by the invention are subjected to heat treatment, so that the aerogel particles can be converted from amorphous to crystal, the mechanical strength of the aerogel particles is remarkably improved, the coating is effectively prevented from being scratched, damaged by pressure or abraded, and the moisture regaining treatment can effectively reduce the phenomena of pore collapse and particle aggregation in the crystal conversion process; the porous skeleton structure of the aerogel is maintained, so that the advantage of the aerogel in thermal insulation performance is maintained, and heat treatment at the temperature of 800 DEG C or above can be adopted after moisture regaining treatment, so that the crystal transformation degree can be deepened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fabric preparation, and in particular to a down jacket fabric with an aerogel coating. Background Art

[0002] Aerogel is a nano-scale porous solid material. Covering the surface of down jacket fabric with aerogel coating can significantly improve the thermal insulation performance of down jackets, thereby appropriately reducing the amount of filling to make light down jackets. At the same time, the fabric can still maintain a soft feel, increasing wearing comfort.

[0003] However, as a special material, although aerogel has many unique advantages, it also has some obvious disadvantages. The most important disadvantage is that aerogel has low density and loose structure, which leads to its weak mechanical strength and can be easily crushed or damaged. Especially in situations where higher mechanical strength is required, the use of aerogel will have obvious limitations.

[0004] Therefore, the conventional process of covering the surface of down jacket fabric with aerogel coating produces an aerogel coating with poor durability, which is easily scratched, crushed and worn, reducing its thermal insulation performance and aesthetics. Summary of the invention

[0005] The object of the present invention is to provide a down jacket fabric with an aerogel coating, which solves the problems of low mechanical strength of the coating and easy scratching, crushing and abrasion in the existing down jacket fabric with aerogel coating.

[0006] The present invention achieves the above-mentioned purpose through the following technical solutions:

[0007] A down jacket fabric with an aerogel coating comprises a base fabric and an aerogel coating coated on at least one surface of the base fabric, wherein the raw materials for preparing the aerogel coating comprise 40-80wt% of a coating matrix, 10-25wt% of modified silica aerogel particles and 10-35wt% of an auxiliary agent, and the modified silica aerogel particles are obtained by sequentially subjecting silica aerogel particles to moisture reconditioning treatment and heat treatment.

[0008] A further improvement is that the base fabric is selected from one of natural fiber fabric, chemical fiber fabric, regenerated fiber fabric and blended fabric.

[0009] A further improvement is that the coating matrix is ​​selected from one or more of bisphenol A epoxy resin, hydroxyethyl methacrylate, acrylic emulsion, polyvinyl acetate emulsion, and melamine formaldehyde resin.

[0010] A further improvement is that the auxiliary agent includes toluene, polyethylene glycol, sodium hexametaphosphate, polyvinyl alcohol and ethanol.

[0011] A further improvement is that the mass ratio of the auxiliary agents is toluene: polyethylene glycol: sodium hexametaphosphate: polyvinyl alcohol: ethanol = 1:1.2:0.5:1.5:2.

[0012] A further improvement is that the moisture regain treatment refers to placing the silica aerogel particles in a constant temperature and humidity chamber at a temperature of 40-50°C and a humidity of 80-90% for 2-5 hours, so that the moisture regain of the silica aerogel particles reaches 8-12%.

[0013] A further improvement is that during the rehumidification process, isoamyl alcohol vapor is introduced into the box and the air pressure in the box is controlled to be 300-320 kPa.

[0014] A further improvement is that the heat treatment refers to placing the silica aerogel particles in a crucible, heating the temperature from room temperature to 800-850°C at a heating rate of 10-12°C / min in a nitrogen atmosphere, and then keeping the temperature for 0.2-0.5h.

[0015] The beneficial effects of the present invention are as follows: the modified silica aerogel particles used in the present invention have been subjected to a rehydration treatment and a heat treatment, wherein the heat treatment can transform the aerogel particles from amorphous to crystalline, significantly improving their mechanical strength, thereby effectively avoiding the coating from being scratched, crushed or worn, and the rehydration treatment can effectively reduce the pore collapse and particle aggregation during the crystal transformation process, maintain the porous skeleton structure of the aerogel, thereby maintaining the advantage of the aerogel in thermal insulation performance, and after the rehydration treatment, a heat treatment of more than 800°C can be used, which helps to deepen the degree of crystal transformation. In addition, the auxiliary conditions of isoamyl alcohol vapor and high pressure are used in the rehydration treatment process, which can reduce the surface tension of the particles and improve the compatibility, thereby improving the rehydration effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is an electron microscope SEM image of the modified silica aerogel particles of Example 4;

[0017] Figure 2 This is an electron microscope SEM image of the modified silica aerogel particles of Comparative Example 1;

[0018] Figure 3 This is an electron microscope SEM image of the silica aerogel particles of Comparative Example 2; DETAILED DESCRIPTION

[0019] The present application is further described in detail below in conjunction with the accompanying drawings. It is necessary to point out here that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technical personnel in this field can make some non-essential improvements and adjustments to the present application based on the above application content.

[0020] 1. Main instruments and materials

[0021] Silica aerogel particles: Common commercially available hydrophilic silica aerogel particles are used, which are white and slightly transparent, with a particle size between 0.02-0.05mm and a density of 92.4kg / m 3 The porosity is calculated by Brunau-EmmettTeller (BET) model to be 96.5%.

[0022] Electron microscope: A scanning electron microscope (SEM) model S4800 from Hitachi, Japan was used.

[0023] 2. Implementation of the experiment

[0024] Example 1

[0025] A down jacket fabric with an aerogel coating comprises a base fabric and an aerogel coating coated on at least one surface of the base fabric, wherein the raw materials for preparing the aerogel coating comprise 40wt% of a coating matrix, 25wt% of modified silica aerogel particles and 35wt% of an auxiliary agent, and the modified silica aerogel particles are obtained by sequentially subjecting silica aerogel particles to a moisture reconditioning treatment and a heat treatment.

[0026] The moisture regain treatment refers to placing the silica aerogel particles in a constant temperature and humidity chamber at a temperature of 40°C and a humidity of 80% for 5 hours (normal pressure) to make the moisture regain of the silica aerogel particles reach 8%. The heat treatment refers to placing the silica aerogel particles in a crucible, heating the temperature from room temperature to 800°C at a heating rate of 10°C / min in a nitrogen atmosphere, and then keeping the temperature for 0.5 hours.

[0027] In addition, the base fabric is natural cotton fiber fabric; the coating matrix is ​​bisphenol A epoxy resin; the additives include toluene, polyethylene glycol, sodium hexametaphosphate, polyvinyl alcohol and ethanol, and the mass ratio of each additive is toluene: polyethylene glycol: sodium hexametaphosphate: polyvinyl alcohol: ethanol = 1:1.2:0.5:1.5:2.

[0028] Example 2

[0029] A down jacket fabric with an aerogel coating comprises a base fabric and an aerogel coating coated on at least one surface of the base fabric, wherein the raw materials for preparing the aerogel coating comprise 60wt% of a coating matrix, 20wt% of modified silica aerogel particles and 20wt% of an auxiliary agent, and the modified silica aerogel particles are obtained by sequentially subjecting silica aerogel particles to a moisture reconditioning treatment and a heat treatment.

[0030] The moisture regain treatment refers to placing the silica aerogel particles in a constant temperature and humidity chamber at a temperature of 45°C and a humidity of 85% for 3 hours (normal pressure) to make the moisture regain of the silica aerogel particles reach 10%. The heat treatment refers to placing the silica aerogel particles in a crucible, heating the temperature from room temperature to 820°C at a heating rate of 11°C / min in a nitrogen atmosphere, and then keeping the temperature for 0.4 hours.

[0031] In addition, the base fabric is polyester fiber fabric; the coating matrix is ​​acrylic emulsion and polyvinyl acetate emulsion (mass ratio 1:1); the auxiliary agents include toluene, polyethylene glycol, sodium hexametaphosphate, polyvinyl alcohol and ethanol, and the mass ratio of each auxiliary agent is toluene: polyethylene glycol: sodium hexametaphosphate: polyvinyl alcohol: ethanol = 1:1.2:0.5:1.5:2.

[0032] Example 3

[0033] A down jacket fabric with an aerogel coating comprises a base fabric and an aerogel coating coated on at least one surface of the base fabric, wherein the raw materials for preparing the aerogel coating comprise 80wt% of a coating matrix, 10wt% of modified silica aerogel particles and 10wt% of an auxiliary agent, and the modified silica aerogel particles are obtained by sequentially subjecting silica aerogel particles to a moisture reconditioning treatment and a heat treatment.

[0034] The moisture regain treatment refers to placing the silica aerogel particles in a constant temperature and humidity chamber at a temperature of 50°C and a humidity of 90% for 2 hours (normal pressure) to make the moisture regain of the silica aerogel particles reach 12%. The heat treatment refers to placing the silica aerogel particles in a crucible, heating the temperature from room temperature to 850°C at a heating rate of 12°C / min in a nitrogen atmosphere, and then keeping the temperature for 0.2 hours.

[0035] In addition, the base fabric is modal fiber fabric; the coating matrix is ​​melamine formaldehyde resin; the additives include toluene, polyethylene glycol, sodium hexametaphosphate, polyvinyl alcohol and ethanol, and the mass ratio of each additive is toluene: polyethylene glycol: sodium hexametaphosphate: polyvinyl alcohol: ethanol = 1:1.2:0.5:1.5:2.

[0036] Example 4

[0037] A down jacket fabric with an aerogel coating comprises a base fabric and an aerogel coating coated on at least one surface of the base fabric, wherein the raw materials for preparing the aerogel coating comprise 60wt% of a coating matrix, 20wt% of modified silica aerogel particles and 20wt% of an auxiliary agent, and the modified silica aerogel particles are obtained by sequentially subjecting silica aerogel particles to a moisture reconditioning treatment and a heat treatment.

[0038] The rehydration treatment refers to placing the silica aerogel particles in a constant temperature and humidity chamber at a temperature of 45°C and a humidity of 85% for 3 hours, so that the moisture regain of the silica aerogel particles reaches 10%; and during the rehydration treatment, isoamyl alcohol vapor is introduced into the chamber and the air pressure in the chamber is controlled to be 300kPa. The heat treatment refers to placing the silica aerogel particles in a crucible, heating the temperature from room temperature to 820°C at a heating rate of 11°C / min in a nitrogen atmosphere, and then keeping the temperature for 0.4h.

[0039] The electron microscope SEM image of the obtained modified silica aerogel particles is as follows: Figure 1 As shown, it can be seen that crystallization has occurred, but the microscopic pore structure is rarely destroyed, and the pore collapse and particle aggregation phenomena are not obvious.

[0040] In addition, the base fabric is polyester fiber fabric; the coating matrix is ​​acrylic emulsion and polyvinyl acetate emulsion (mass ratio 1:1); the auxiliary agents include toluene, polyethylene glycol, sodium hexametaphosphate, polyvinyl alcohol and ethanol, and the mass ratio of each auxiliary agent is toluene: polyethylene glycol: sodium hexametaphosphate: polyvinyl alcohol: ethanol = 1:1.2:0.5:1.5:2.

[0041] Comparative Example 1

[0042] A down jacket fabric with an aerogel coating comprises a base fabric and an aerogel coating coated on at least one surface of the base fabric, wherein the raw materials for preparing the aerogel coating comprise 60wt% of a coating matrix, 20wt% of modified silica aerogel particles and 20wt% of an auxiliary agent, and the modified silica aerogel particles are obtained by sequentially subjecting silica aerogel particles to heat treatment.

[0043] The heat treatment refers to placing the silica aerogel particles in a crucible, heating the crucible from room temperature to 820° C. at a heating rate of 11° C. / min in a nitrogen atmosphere, and then keeping the temperature for 0.4 h.

[0044] The electron microscope SEM image of the obtained modified silica aerogel particles is as follows: Figure 2 As shown, it can be seen that it is completely crystallized, the microscopic pore structure is completely destroyed, and the particles become larger and aggregated together.

[0045] In addition, the base fabric is polyester fiber fabric; the coating matrix is ​​acrylic emulsion and polyvinyl acetate emulsion (mass ratio 1:1); the auxiliary agents include toluene, polyethylene glycol, sodium hexametaphosphate, polyvinyl alcohol and ethanol, and the mass ratio of each auxiliary agent is toluene: polyethylene glycol: sodium hexametaphosphate: polyvinyl alcohol: ethanol = 1:1.2:0.5:1.5:2.

[0046] Comparative Example 2

[0047] A down jacket fabric with an aerogel coating comprises a base fabric and an aerogel coating coated on at least one surface of the base fabric, wherein the raw materials for preparing the aerogel coating comprise 60wt% of a coating matrix, 20wt% of silicon dioxide aerogel particles and 20wt% of an auxiliary agent.

[0048] The electron microscope SEM image of silica aerogel particles is shown in Figure 3 As shown, it can be seen that its porous structure is obvious and the particles are dispersed.

[0049] The base fabric is polyester fiber fabric; the coating matrix is ​​acrylic emulsion and polyvinyl acetate emulsion (mass ratio 1:1); the auxiliary agents include toluene, polyethylene glycol, sodium hexametaphosphate, polyvinyl alcohol and ethanol, and the mass ratio between the auxiliary agents is toluene: polyethylene glycol: sodium hexametaphosphate: polyvinyl alcohol: ethanol = 1:1.2:0.5:1.5:2.

[0050] The preparation methods of the above embodiments and comparative examples are the same, specifically: first, all the raw materials of the aerogel coating are mixed evenly in proportion to obtain a coating, and then the coating is evenly coated on the surface of the woven base fabric. Here, a single-sided coating method is adopted, and the coating thickness is controlled at 0.6 mm.

[0051] 3. Performance Test

[0052] The down jacket fabric samples with aerogel coatings prepared in Examples 1-4 and Comparative Examples 1-2 were taken and the following performance tests were performed on them:

[0053] (1) Thermal insulation performance: Six groups of sealable glass bottles filled with 90°C water (5 bottles in each group) were taken, and each group was wrapped with the fabric samples prepared in the above Examples 1-4 and Comparative Examples 1-2 on the side. After wrapping, they were placed in a room temperature environment, and the water temperature in the glass bottles was recorded after 2 hours. The average temperature loss rate of each group was calculated using the calculation formula: temperature loss rate = (initial temperature - temperature after 2 hours) / initial temperature * 100%. The calculation results are statistically obtained in Table 1 below.

[0054] (2) Wear resistance: Referring to GB / T21196.2-2007 "Determination of the abrasion resistance of textile fabrics by the Martindale method", abrasion resistance tests were carried out on down jacket fabric samples in their initial state and after folding 10,000 times, and their wear resistance index Ai (average mass loss per friction) was tested. The statistical results are shown in Table 2 below.

[0055] 4. Results Analysis

[0056] (1) Thermal insulation performance.

[0057] Table 1: Temperature loss rate results of various embodiments and comparative examples

[0058] Group Initial temperature Temperature after 2h Average temperature loss rate / % Example 1 90.0℃ 49.3℃ 45.2% Example 2 90.0℃ 52.9℃ 41.2% Example 3 90.0℃ 51.7℃ 42.6% Example 4 90.0℃ 60.6℃ 32.6% Comparative Example 1 90.0℃ 38.5℃ 57.2% Comparative Example 2 90.0℃ 62.1℃ 31.0%

[0059] (2) Wear resistance.

[0060] Table 2: Wear resistance index Ai results of various embodiments and comparative examples

[0061]

[0062] Analysis: It can be seen from Table 1 and Table 2 above that Examples 1-3 of the present invention use modified silica aerogel particles that have been subjected to moisture recovery treatment and heat treatment, and their overall thermal insulation performance is good, which is significantly improved compared to Comparative Example 1 (without moisture recovery treatment). The wear resistance of Examples 1-3 is also good, close to the level of Comparative Example 1, and significantly better than Comparative Example 2 (ordinary silica aerogel particle coating); Based on Example 2, Example 4 of the present invention adds auxiliary conditions of isoamyl alcohol vapor and high pressure during the moisture recovery treatment, so that the thermal insulation performance is further improved, which is equivalent to Comparative Example 2; In addition, the silica aerogel particles of Comparative Example 1 have only been heat-treated, and although their wear resistance is the best, their thermal insulation performance is the worst; Comparative Example 2 uses ordinary silica aerogel particles, which have the best thermal insulation performance, but the worst wear resistance.

[0063] In summary, the present invention uses modified silica aerogel particles that have been subjected to moisture regain treatment and heat treatment, effectively reducing pore collapse and particle aggregation during crystal transformation, maintaining the porous skeleton structure of aerogel, thereby maintaining the advantage of aerogel in thermal insulation performance, so that the fabric has both thermal insulation and mechanical strength. And after moisture regain treatment, a heat treatment of more than 800°C can be used (generally, a heat treatment of more than 700°C will basically completely destroy the aerogel structure and make it lose its function), which helps to deepen the degree of crystal transformation. In addition, the auxiliary conditions of isoamyl alcohol vapor and high pressure are used during the moisture regain treatment process, which can reduce the surface tension of the particles and improve compatibility, thereby improving the moisture regain effect, and ultimately reflected in the further improvement of thermal insulation performance.

[0064] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A down jacket fabric with an aerogel coating, comprising a base fabric and an aerogel coating coated on at least one surface of the base fabric, It is characterized in that The raw materials for preparing the aerogel coating include 40-80wt% of a coating matrix, 10-25wt% of modified silica aerogel particles and 10-35wt% of an auxiliary agent. The modified silica aerogel particles are obtained by sequentially subjecting silica aerogel particles to moisture reconditioning and heat treatment.

2. A down jacket fabric with an aerogel coating according to claim 1, It is characterized in that The basic fabric is selected from one of natural fiber fabric, chemical fiber fabric, regenerated fiber fabric and blended fabric.

3. A down jacket fabric with an aerogel coating according to claim 1, It is characterized in that The coating matrix is ​​selected from one or more of bisphenol A epoxy resin, hydroxyethyl methacrylate, acrylic emulsion, polyvinyl acetate emulsion, and melamine formaldehyde resin.

4. A down jacket fabric with an aerogel coating according to claim 1, It is characterized in that The auxiliary agent comprises toluene, polyethylene glycol, sodium hexametaphosphate, polyvinyl alcohol and ethanol.

5. A down jacket fabric with aerogel coating according to claim 4, It is characterized in that The mass ratio of each auxiliary agent is toluene: polyethylene glycol: sodium hexametaphosphate: polyvinyl alcohol: ethanol = 1:1.2:0.5:1.5:

2.

6. A down jacket fabric with an aerogel coating according to claim 1, It is characterized in that The moisture regain treatment refers to placing the silica aerogel particles in a constant temperature and humidity chamber at a temperature of 40-50° C. and a humidity of 80-90% for 2-5 hours, so that the moisture regain of the silica aerogel particles reaches 8-12%.

7. A down jacket fabric with aerogel coating according to claim 6, It is characterized in that During the rehumidification process, isoamyl alcohol vapor is introduced into the box and the air pressure in the box is controlled at 300-320 kPa.

8. The down jacket fabric with aerogel coating according to claim 1, It is characterized in that The heat treatment refers to placing the silica aerogel particles in a crucible, heating the temperature from room temperature to 800-850° C. at a heating rate of 10-12° C. / min in a nitrogen atmosphere, and then keeping the temperature for 0.2-0.5 h.

Citation Information

Patent Citations

  • Oil-proof coating of down jacket and production method of oil-proof coating

    CN114717852A

  • Thermal insulation tent fabric and preparation method thereof

    CN116043568A

  • Methods for manufacturing insulating fabric for clothes containing aerogel

    KR102113292B1

Cited By

  • Antibacterial down jacket fabric with aerogel coating and preparation method thereof

    CN120099799A

  • Integrally-woven cold-spot-free convection-proof down jacket fabric and preparation method thereof

    CN120836840A