A bonded wafer and a method for forming the same

By forming a copper diffusion barrier layer and a bonding surface stack on the wafer surface and performing plasma activation treatment before bonding, the problem of reduced thin film density at the bonding interface is solved, and the reliability and stability of the device after bonding are improved.

CN118763091BActive Publication Date: 2024-11-29NEXCHIP SEMICON CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411245078.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-29
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

In the BSI fabrication process, the bonding interface between the pixel wafer and the logic circuit wafer is prone to a decrease in film density when the bonding energy is increased, which affects the reliability of the bonded device.

Method used

The design employs a copper diffusion barrier layer and a bonding surface stack, forming grooves on the wafer surface and filling them with copper material. Combined with plasma activation treatment, this ensures that the film quality of the copper diffusion barrier layer is not affected and prevents copper diffusion.

Benefits of technology

The reliability of the bonded device is improved by combining a copper diffusion barrier layer and plasma treatment, which ensures optimal bonding energy, prevents copper diffusion, and enhances the stability of the bonding interface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763091B_ABST
    Figure CN118763091B_ABST
Patent Text Reader

Abstract

The invention provides a bonding wafer and a forming method thereof. The forming method of the bonding wafer comprises the following steps: providing a first wafer and a second wafer both provided with a copper interconnection structure, forming an interface stack on a side close to the copper interconnection structure, the interface stack comprising a copper diffusion barrier layer and a bonding surface in order from bottom to top; forming a copper through hole on a side close to the interface stack; activating the bonding surface, and bonding the first wafer and the second wafer, with the bonding surface of the first wafer facing the bonding surface of the second wafer, so as to perform copper diffusion barrier on the copper interconnection layer through a special copper diffusion barrier layer, and when activating the bonding interface before bonding, the content of each component of the bonding surface is changed, and the plasma treatment process in the activation process does not affect the film quality of the copper diffusion barrier layer, so that the interface stack can prevent copper diffusion and ensure the optimal bonding energy at the same time, thereby improving the reliability of the device after bonding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor manufacturing, and in particular to a bonding wafer and a forming method thereof. Background Art

[0002] In the BSI (backside illumination) manufacturing process, the pixel wafer and the logic wafer need to be bonded. During the bonding process, the bonding effect between the pixel wafer and the logic wafer will affect the subsequent process and yield. In addition, SiO 2 and SICN as the bonding interface between pixel wafer and logic circuit wafer, but SiO 2 When SICN is activated during bonding, the density of the bonding interface film tends to decrease as the bonding energy increases, which affects the reliability of the device after bonding. Summary of the invention

[0003] The object of the present invention is to provide a bonding wafer and a method for forming the same, which can prevent the problem of a decrease in film density at the bonding interface as the bonding energy increases during bonding activation at the bonding interface.

[0004] In order to solve the above problems, the present invention provides a method for forming a bonded wafer, comprising the following steps:

[0005] Providing a first wafer and a second wafer, wherein a copper interconnection structure is disposed in the first wafer and the second wafer, and forming an interface stack on a side of the first wafer and the second wafer close to the copper interconnection structure, respectively, wherein the interface stack includes a copper diffusion barrier layer and a bonding surface in sequence from bottom to top;

[0006] A groove is formed on one side of the first wafer and the second wafer close to the interface stack, the groove passes through the interface stack and exposes the copper interconnect structure, and a copper material is filled in the groove to form a copper through hole;

[0007] The bonding surface of the first wafer and the bonding surface of the second wafer are activated, and the first wafer and the second wafer are bonded, wherein the bonding surface of the first wafer faces the bonding surface of the second wafer.

[0008] Optionally, the interface stack further includes an adhesion layer, wherein the adhesion layer is located between the copper diffusion barrier layer and the bonding surface.

[0009] Further, the first wafer includes a front side and a back side, the front side is provided with pixel units distributed in an array, a first copper interconnection structure is provided in the first wafer near the back side, the first copper interconnection structure includes at least one first bottom copper interconnection layer and a first top copper interconnection layer located on one side of all the first bottom copper interconnection layers, and the back side exposes the first top copper interconnection layer;

[0010] The second wafer includes a first surface and a second surface, a logic circuit is arranged in the second wafer on a side close to the first surface, a second copper interconnect structure is arranged in the second wafer on a side close to the second surface, the second copper interconnect structure includes at least one second bottom copper interconnect layer and a second top copper interconnect layer located on one side of all the second bottom copper interconnect layers, and the second surface exposes the second top copper interconnect layer.

[0011] Furthermore, the method for forming the interface stack is specifically as follows:

[0012] forming a first initial copper diffusion barrier layer on the back side by a deposition process, and then forming a first initial oxide layer on the first initial copper diffusion barrier layer by a TEOS process; forming a second initial copper diffusion barrier layer on the second surface by a deposition process, and then forming a second initial oxide layer on the second initial copper diffusion barrier layer by a TEOS process;

[0013] A first copper diffusion barrier layer, a first adhesion layer and a first bonding surface are sequentially formed on the first initial oxide layer by a deposition process; and a second copper diffusion barrier layer, a second adhesion layer and a second bonding surface are sequentially formed on the second initial oxide layer by a deposition process.

[0014] Furthermore, the first copper diffusion barrier layer and the second copper diffusion barrier layer are both carbon-doped silicon nitride film layers, the first adhesion layer and the second adhesion layer are both oxide layers, and the first bonding surface and the second bonding surface are both silicon carbide layers.

[0015] Furthermore, the ratio of the carbon content to the silicon content in the first bonding surface is adjustable.

[0016] Furthermore, the ratio of carbon content to silicon content in the first bonding surface is 1:0.5 to 1:1.5.

[0017] Furthermore, the thickness of the first copper diffusion barrier layer and the second copper diffusion barrier layer is 500Å~1500Å, the thickness of the first adhesion layer and the second adhesion layer is 10Å~35Å, and the thickness of the first bonding surface and the second bonding surface is 40Å~70Å.

[0018] Furthermore, the method of bonding the first wafer and the second wafer is specifically as follows:

[0019] Performing plasma activation treatment on the first bonding surface and the second bonding surface respectively by nitrogen gas;

[0020] The first wafer and the second wafer are bonded, with the first bonding surface being disposed toward the second bonding surface.

[0021] On the other hand, the present invention also provides a bonding wafer, which is prepared by the bonding wafer forming method described above, wherein the bonding wafer includes a first wafer and a second wafer that are bonded together, wherein a copper interconnection structure is provided in the first wafer and the second wafer, and an interface stack is formed on the first wafer and the second wafer on a side close to the copper interconnection structure, respectively, wherein the interface stack includes a copper diffusion barrier layer and a bonding surface from bottom to top, and grooves are formed on the first wafer and the second wafer on a side close to the interface stack, wherein the grooves penetrate the interface stacks and expose the copper interconnection structure, and copper material is filled in the grooves to form copper through-holes, wherein the bonding surface of the first wafer faces the bonding surface of the second wafer.

[0022] Compared with the prior art, the present invention has the following unexpected technical effects:

[0023] The present invention provides a bonding wafer and a method for forming the bonding wafer. The method for forming the bonding wafer comprises the following steps: providing a first wafer and a second wafer, wherein a copper interconnection structure is provided in the first wafer and the second wafer, and an interface stack is formed on a side of the first wafer and the second wafer close to the copper interconnection structure, respectively, wherein the interface stack comprises a copper diffusion barrier layer and a bonding surface in sequence from bottom to top; forming a groove on a side of the first wafer and the second wafer close to the interface stack, wherein the groove passes through the interface stack and exposes the copper interconnection structure, and copper material is filled in the groove to form a copper through hole; activating the bonding surface of the first wafer and the bonding surface of the second wafer, and bonding the first wafer and the second wafer, wherein the bonding surface of the first wafer faces the bonding surface of the second wafer. The present invention has the following unexpected technical effects: copper diffusion is blocked for the copper interconnect layer by a special copper diffusion barrier layer, and when the bonding interface is activated before bonding, the content of each component on the bonding surface is changed, and the plasma treatment process during the activation process does not affect the film quality of the copper diffusion barrier layer, so that the interface stack can prevent copper diffusion while ensuring the optimal bonding energy, thereby improving the reliability of the device after bonding. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a schematic diagram of the structure of a current logic wafer or pixel wafer.

[0025] Figure 2A schematic diagram of the structure of forming copper through-holes in current logic wafers or pixel wafers.

[0026] Figure 3 This is a schematic diagram of the structure after the logic wafer and pixel wafer are bonded.

[0027] Figure 4 A schematic flow chart of a method for forming a bonded wafer provided in one embodiment of the present invention.

[0028] Figure 5 A schematic structural diagram of a first wafer provided in accordance with an embodiment of the present invention.

[0029] Figure 6 A schematic structural diagram of a second wafer provided in accordance with an embodiment of the present invention.

[0030] Figure 7 It is a schematic structural diagram of forming a first bonding stack according to an embodiment of the present invention.

[0031] Figure 8 It is a schematic structural diagram of forming a second bonding stack according to an embodiment of the present invention.

[0032] Fig. 9 It is a schematic structural diagram of forming a first groove according to an embodiment of the present invention.

[0033] Fig.10 It is a schematic structural diagram of forming a second groove according to an embodiment of the present invention.

[0034] Fig.11 This is a schematic diagram of the structure of an embodiment of the present invention after the first groove is filled.

[0035] Fig.12 This is a schematic diagram of the structure after the second groove is filled according to an embodiment of the present invention.

[0036] Fig.13 It is a schematic structural diagram of a first groove filled with a material after a grinding process according to an embodiment of the present invention.

[0037] Fig.14 It is a schematic structural diagram of a second groove filled with a material after a grinding process according to an embodiment of the present invention.

[0038] Fig.15 This is a schematic diagram of the structure after the first wafer and the second wafer are bonded together according to an embodiment of the present invention.

[0039] Description of reference numerals:

[0040] 1-logic wafer; 2-pixel wafer; 11-copper interconnect layer; 21-NDC layer; 22-oxide film layer; 23-copper via;

[0041] 100-first wafer; 100a-front side; 100b-back side; 101-first top copper interconnect layer; 110-first initial copper diffusion barrier layer; 120-first initial oxide layer; 130-first interface stack; 131-first copper diffusion barrier layer; 132-first adhesion layer; 133-first bonding surface; 140-first oxide layer; 151-first groove; 152-first trench; 161-first copper via; 162-first virtual pattern metal block;

[0042] 200-second wafer; 200a-first surface; 200b-second surface; 201-second top copper interconnect layer; 210-second initial copper diffusion barrier layer; 220-second initial oxide layer; 230-second interface stack; 231-second copper diffusion barrier layer; 232-second adhesion layer; 233-second bonding surface; 240-second oxide layer; 251-second groove; 252-second trench; 261-second copper through hole; 262-second virtual graphic metal block. DETAILED DESCRIPTION

[0043] A bonded wafer and a method for forming the same of the present invention will be described in further detail below. The present invention will be described in more detail below with reference to the accompanying drawings, in which preferred embodiments of the present invention are shown, and it should be understood that those skilled in the art may modify the present invention described herein and still achieve the beneficial effects of the present invention. Therefore, the following description should be understood as being broadly known to those skilled in the art and not as a limitation of the present invention.

[0044] For the sake of clarity, not all features of the actual embodiments are described. In the following description, well-known functions and structures are not described in detail because they would clutter the invention with unnecessary detail. It should be recognized that in the development of any actual embodiment, a large number of implementation details must be made to achieve the developer's specific goals, such as changing from one embodiment to another according to the limitations of the relevant system or the relevant business. In addition, it should be recognized that such development work may be complex and time-consuming, but it is just a routine task for those skilled in the art.

[0045] In order to make the purpose and features of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are further described below in conjunction with the accompanying drawings. It should be noted that the accompanying drawings are all in a very simplified form and use inaccurate ratios, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0046] When bonding the current logic wafer and the pixel wafer, a hybrid bonding interface needs to be formed on the bonding side surfaces of the logic wafer and the pixel wafer, respectively. The method for forming the hybrid bonding interface is as follows:

[0047] like Figure 1As shown, a logic wafer 1 and a pixel wafer 2 are provided, and an NDC (carbon-doped silicon nitride film, Nitride Doped Silicon Carbide) layer 21 and an oxide film layer 22 are formed on one side of the logic wafer 1 and one side of the pixel wafer 2, respectively, wherein a copper interconnect layer 11 is provided in both the logic wafer 1 and the pixel wafer 2; Figure 2 As shown, in the logic wafer 1 or the pixel wafer 2, the oxide film layer 22 and the NDC layer 21 are sequentially etched to expose the copper interconnect layer 11 to form a groove, and the groove is filled with copper material; finally, the copper material is polished and planarized and the oxide film layer 22 is removed to expose the NDC layer 21 and form a copper through hole 23, and the NDC layer 21 and the copper through hole 23 constitute a mixed interface. Figure 3 As shown, finally, the mixed interface of the logic wafer 1 and the mixed interface of the pixel wafer 2 are activated, and the logic wafer 1 and the pixel wafer 2 are bonded, wherein the mixed interface of the logic wafer 1 is arranged toward the mixed interface of the pixel wafer 2. The NDC layer 21 can prevent the diffusion of copper in the copper interconnect layer 11, and as one of the mixed interfaces, the bonding energy of the material silicon nitride used in the NDC layer 21 is better than other bonding interface materials (such as silicon oxide). During the activation process of the mixed interface, nitrogen plasma treatment needs to be introduced into the mixed interface to break the Si-O, CO, and Si-C covalent bonds in the NDC layer. The formed dangling bonds play a very important role in the bonding energy. As the ratio of carbon to nitrogen in the NDC layer 21 increases, the bonding energy of the NDC layer 21 gradually increases, but as the carbon content increases, the film density of the NDC layer 21 will decrease, that is, the film quality of the NDC layer deteriorates, resulting in a deterioration in the effect of blocking the diffusion of copper in the copper interconnect layer, thereby affecting the reliability of the device after bonding.

[0048] Based on this, Figure 4 As shown, the core idea of ​​the present invention is to provide a method for forming a bonded wafer, comprising the following steps:

[0049] Step S1: providing a first wafer and a second wafer, wherein a copper interconnection structure is disposed in the first wafer and the second wafer, and forming an interface stack on a side of the first wafer and the second wafer close to the copper interconnection structure, respectively, wherein the interface stack includes a copper diffusion barrier layer and a bonding surface in sequence from bottom to top;

[0050] Step S2: forming grooves on one side of the first wafer and the second wafer close to the interface stack, the grooves penetrating the interface stack and exposing the copper interconnect structure, and filling the grooves with copper material to form copper through-holes;

[0051] Step S3: activating the bonding surface of the first wafer and the bonding surface of the second wafer, and bonding the first wafer and the second wafer, with the bonding surface of the first wafer facing the bonding surface of the second wafer.

[0052] A method for forming a bonded wafer in this embodiment uses a special copper diffusion barrier layer to block the copper diffusion of the copper interconnect layer, and when the bonding interface is activated before bonding, the content of each component on the bonding surface changes, and the plasma treatment process during the activation process does not affect the film quality of the copper diffusion barrier layer, so that the interface stack can prevent copper diffusion while ensuring the optimal bonding energy, thereby improving the reliability of the device after bonding.

[0053] The following is combined with Figure 5-Figure 15 A method for forming a bonded wafer provided in this embodiment is described in detail.

[0054] First, step S1 is performed to provide a first wafer 100 and a second wafer 200, wherein a copper interconnection structure is disposed in the first wafer 100 and the second wafer 200, and an interface stack is formed on a side of the first wafer 100 and the second wafer 200 close to the copper interconnection structure, respectively, and the interface stack includes a copper diffusion barrier layer and a bonding surface from bottom to top.

[0055] This step specifically includes the following steps:

[0056] First, if Figure 5 As shown, a first wafer 100 is provided, wherein the first wafer 100 includes a front side 100a and a back side 100b, wherein the front side 100a is provided with array-distributed pixel units, and a first copper interconnection structure is provided in the first wafer 100 close to the back side 100b, wherein the first copper interconnection structure includes at least one first bottom copper interconnection layer and a first top copper interconnection layer 101 located on one side of all the first bottom copper interconnection layers, and the back side 100b exposes the first top copper interconnection layer 101.

[0057] like Figure 6 As shown, a second wafer 200 is provided, the second wafer 200 includes a first surface 200a and a second surface 200b, a logic circuit is arranged in the second wafer 200 on the side close to the first surface 200a, a second copper interconnect structure is arranged in the second wafer 200 on the side close to the second surface 200b, the second copper interconnect structure includes at least one second bottom copper interconnect layer and a second top copper interconnect layer 201 located on one side of all the second bottom copper interconnect layers, and the second surface 200b exposes the second top copper interconnect layer 201.

[0058] Next, please continue reading Figure 5A first initial copper diffusion barrier layer 110 is formed on the back surface 100b by a deposition process, and a first initial oxide layer 120 is formed on the first initial copper diffusion barrier layer 110 by a TEOS process. Figure 6 , a second initial copper diffusion barrier layer 210 is formed on the second surface 200 b by a deposition process, and then a second initial oxide layer 220 is formed on the second initial copper diffusion barrier layer 210 by a TEOS process.

[0059] The first initial copper diffusion barrier layer 110 and the second initial copper diffusion barrier layer 210 may be NDC layers, the first initial oxide layer 120 and the second initial oxide layer 220 may be TEOS (tetraethyl silicon oxide) layers, and the first initial copper diffusion barrier layer 110 and the first initial oxide layer 120 are used to form a first dummy pattern metal block 162, and the second initial copper diffusion barrier layer 210 and the second initial oxide layer 220 are used to form a second dummy pattern metal block 262.

[0060] Then, if Figure 7 As shown, a first interface stack 130 and a first oxide layer 140 are formed on the first initial oxide layer 120. In detail, a first copper diffusion barrier layer 131, a first adhesion layer 132 and a first bonding surface 133 are sequentially formed on the first initial oxide layer 120 by a deposition process.

[0061] like Figure 8 As shown, a second interface stack 230 and a second oxide layer 240 are formed on the second initial oxide layer 220. In detail, a second copper diffusion barrier layer 231, a second adhesion layer 232 and a second bonding surface 233 are sequentially formed on the second initial oxide layer 220 by a deposition process.

[0062] The first copper diffusion barrier layer 131 and the second copper diffusion barrier layer 231 are both carbon-doped silicon nitride film layers, the first adhesion layer 132 and the second adhesion layer 232 are both oxide layers (such as silicon oxide layers), the first bonding surface 133 and the second bonding surface 233 are both silicon carbide layers, and the ratio of carbon content to silicon content in the first bonding surface 133 is adjustable. Further, the ratio of carbon content to silicon content in the first bonding surface 133 is 1:1, and preferably, the ratio of carbon content to silicon content in the first bonding surface 133 is 1:0.5~1:1.5. The thickness of the first copper diffusion barrier layer 131 and the second copper diffusion barrier layer 231 may be 500Å~1500Å, the thickness of the first adhesion layer 132 and the second adhesion layer 232 may be 10Å~35Å, and the thickness of the first bonding surface 133 and the second bonding surface 233 may be 40Å~70Å.

[0063] In this embodiment, the first oxide layer 140 is used to increase the adhesion between the first copper diffusion barrier layer 131 and the first bonding surface 133 , and the second oxide is used to increase the adhesion between the second copper diffusion barrier layer 231 and the second bonding surface 233 .

[0064] Then, step S2 is performed to form grooves on one side of the first wafer 100 and the second wafer 200 close to the interface stack, wherein the grooves penetrate the interface stack and expose the copper interconnect structure, and copper material is filled in the grooves to form copper through holes.

[0065] This step specifically includes the following steps:

[0066] First, if Fig. 9 As shown, the first oxide layer 140, the first bonding surface 133, the first adhesion layer 132, the first copper diffusion barrier layer 131, the first initial oxide layer 120 and the first initial copper diffusion barrier layer 110 are etched in sequence to expose the first top copper interconnect layer 101 and form a first groove 151. At the same time, first grooves 152 are formed on both sides of the first groove 151. The first grooves 152 penetrate the first oxide layer 140, the first bonding surface 133, the first adhesion layer 132, the first copper diffusion barrier layer 131 and the first initial oxide layer 120.

[0067] like Fig.10 As shown, the second oxide layer 240, the second bonding surface 233, the second adhesion layer 232, the second copper diffusion barrier layer 231, the second initial oxide layer 220 and the second initial copper diffusion barrier layer 210 are etched in sequence to expose the second top copper interconnect layer 201 and form a second groove 251. At the same time, second grooves 252 are formed on both sides of the second groove 251. The second grooves 252 penetrate the second oxide layer 240, the second bonding surface 233, the second adhesion layer 232, the second copper diffusion barrier layer 231 and the second initial oxide layer 220.

[0068] Then, if Fig.11 As shown, copper material is filled in the first groove 151 and the first trench 152 by electroplating process; Fig.12 As shown, copper material is filled in the second groove 251 and the second trench 252 by an electroplating process.

[0069] Then, if Fig.13As shown, the copper material filled in the first groove 151 and the first trench 152 is planarized by a chemical mechanical polishing process, and the first oxide layer 140 is removed to expose the first bonding surface 133, and at the same time, a first copper through hole 161 is formed in the first groove 151, and a first virtual pattern metal block 162 is formed in the first trench 152, and the surface of the first copper through hole 161 and the surface of the first virtual pattern metal block 162 are both flush with the first bonding surface 133.

[0070] like Fig.14 As shown, the copper material filled in the second groove 251 and the second groove 252 is planarized by a chemical mechanical polishing process, and the second oxide layer 240 is removed to expose the second bonding surface 233. At the same time, a second copper through hole 261 is formed in the second groove 251, and a second virtual pattern metal block 262 is formed in the second groove 252. The surface of the second copper through hole 261 and the surface of the second virtual pattern metal block 262 are both flush with the second bonding surface 233.

[0071] like Fig.15 As shown, step S3 is then performed to activate the bonding surface of the first wafer 100 and the bonding surface of the second wafer 200, and bond the first wafer 100 and the second wafer 200, with the bonding surface of the first wafer 100 facing the bonding surface of the second wafer 200.

[0072] This step specifically includes the following steps:

[0073] Firstly, in order to optimize the bonding between the first bonding surface 133 and the second bonding surface 233, the first bonding surface 133 and the second bonding surface 233 are respectively subjected to plasma activation treatment by nitrogen to form dangling bonds of silicon and carbon at the first bonding surface 133 and simultaneously to form dangling bonds of silicon and carbon at the second bonding surface 233, thereby maximizing the dangling bond density of the first bonding surface 133 and the dangling bond density of the second bonding surface 233, and the activation process does not affect the carbon content in the first copper diffusion barrier layer 131 and the second copper diffusion barrier layer 231, thereby avoiding the influence of the bonding activation process on the film quality of the first copper diffusion barrier layer 131 and the second copper diffusion barrier layer 231.

[0074] Next, the first wafer 100 and the second wafer 200 are bonded, with the first bonding surface 133 disposed toward the second bonding surface 233 .

[0075] See also Figure 5-Figure 15The present embodiment also provides a bonding wafer, the bonding wafer comprising a first wafer 100 and a second wafer 200 which are bonded together, a copper interconnection structure being arranged in the first wafer 100 and the second wafer 200, an interface stack being formed on the first wafer 100 and the second wafer 200 on the side close to the copper interconnection structure, the interface stack comprising a copper diffusion barrier layer and a bonding surface from bottom to top, a groove being formed on the first wafer 100 and the second wafer 200 on the side close to the interface stack, the groove penetrating the interface stack and exposing the copper interconnection structure, and a copper material being filled in the groove to form a copper through hole, the bonding surface of the first wafer 100 facing the bonding surface of the second wafer 200.

[0076] In summary, the present invention provides a bonded wafer and a method for forming the same, the method for forming the bonded wafer comprising the following steps: providing a first wafer and a second wafer, wherein a copper interconnection structure is disposed in the first wafer and the second wafer, and interface stacks are respectively formed on a side of the first wafer and the second wafer close to the copper interconnection structure, wherein the interface stacks include a copper diffusion barrier layer and a bonding surface from bottom to top; forming grooves on a side of the first wafer and the second wafer close to the interface stack, wherein the grooves penetrate the interface stacks and expose the copper interconnection structure, and copper material is filled in the grooves to form copper through-holes; activating the bonding surface of the first wafer and the bonding surface of the second wafer, and bonding the first wafer and the second wafer, wherein the bonding surface of the first wafer faces the bonding surface of the second wafer. The present invention has the following unexpected technical effects: copper diffusion is blocked for the copper interconnect layer by a special copper diffusion barrier layer, and when the bonding interface is activated before bonding, the content of each component on the bonding surface is changed, and the plasma treatment process during the activation process does not affect the film quality of the copper diffusion barrier layer, so that the interface stack can prevent copper diffusion while ensuring the optimal bonding energy, thereby improving the reliability of the device after bonding.

[0077] In addition, it should be noted that, unless otherwise specified or indicated, the terms "first" and "second" in the specification are only used to distinguish the various components, elements, steps, etc. in the specification, and are not used to indicate the logical relationship or sequential relationship between the various components, elements, steps, etc.

[0078] It is to be understood that, although the present invention has been disclosed as a preferred embodiment, the above embodiment is not intended to limit the present invention. For any person skilled in the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments of equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of protection of the technical solution of the present invention.

Claims

1. A method for forming a bonded wafer, It is characterized in that The following steps are involved: A first wafer and a second wafer are provided, wherein the first wafer includes a front side and a back side, and the second wafer includes a first surface and a second surface, a copper interconnection structure is disposed on the back side of the first wafer and the second surface side of the second wafer, and an interface stack is formed on the back side of the first wafer and the second surface of the second wafer, respectively, and the interface stack includes a copper diffusion barrier layer, an adhesion layer and a bonding surface in order from bottom to top; A groove is formed on one side of the first wafer and the second wafer close to the interface stack, the groove passes through the interface stack and exposes the copper interconnect structure, and a copper material is filled in the groove to form a copper through hole; activating a bonding surface of the first wafer and a bonding surface of the second wafer, and bonding the first wafer to the second wafer, wherein the bonding surface of the first wafer faces the bonding surface of the second wafer; The method for forming the interface stack is specifically as follows: forming a first initial copper diffusion barrier layer on the back side by a deposition process, and then forming a first initial oxide layer on the first initial copper diffusion barrier layer by a TEOS process; forming a second initial copper diffusion barrier layer on the second surface by a deposition process, and then forming a second initial oxide layer on the second initial copper diffusion barrier layer by a TEOS process; A first copper diffusion barrier layer, a first adhesion layer and a first bonding surface are sequentially formed on the first initial oxide layer by a deposition process; and a second copper diffusion barrier layer, a second adhesion layer and a second bonding surface are sequentially formed on the second initial oxide layer by a deposition process.

2. The method for forming a bonded wafer according to claim 1, It is characterized in that The front side is provided with pixel units distributed in an array, a first copper interconnection structure is provided in the first wafer close to the back side, the first copper interconnection structure includes at least one first bottom copper interconnection layer and a first top copper interconnection layer located on one side of all the first bottom copper interconnection layers, and the back side exposes the first top copper interconnection layer; A logic circuit is arranged in the second wafer on the side close to the first surface, and a second copper interconnection structure is arranged in the second wafer on the side close to the second surface, the second copper interconnection structure includes at least one second bottom copper interconnection layer and a second top copper interconnection layer located on one side of all the second bottom copper interconnection layers, and the second surface exposes the second top copper interconnection layer.

3. The method for forming a bonded wafer according to claim 1, It is characterized in that The first copper diffusion barrier layer and the second copper diffusion barrier layer are both carbon-doped silicon nitride film layers, the first adhesion layer and the second adhesion layer are both oxide layers, and the first bonding surface and the second bonding surface are both silicon carbide layers.

4. The method for forming a bonded wafer according to claim 3, It is characterized in that The ratio of the carbon content to the silicon content in the first bonding surface is adjustable.

5. The method for forming a bonded wafer according to claim 4, It is characterized in that The ratio of carbon content to silicon content in the first bonding surface is 1:0.5 to 1:1.

5.

6. The method for forming a bonded wafer according to claim 1, It is characterized in that The thickness of the first copper diffusion barrier layer and the second copper diffusion barrier layer is 500Å~1500Å, the thickness of the first adhesion layer and the second adhesion layer is 10Å~35Å, and the thickness of the first bonding surface and the second bonding surface is 40Å~70Å.

7. The method for forming a bonded wafer according to claim 1, It is characterized in that The method of bonding the first wafer and the second wafer is specifically as follows: Performing plasma activation treatment on the first bonding surface and the second bonding surface respectively by nitrogen gas; The first wafer and the second wafer are bonded, with the first bonding surface being disposed toward the second bonding surface.

8. A bonded wafer, prepared by the method for forming a bonded wafer according to any one of claims 1 to 7, It is characterized in that The bonded wafer comprises a first wafer and a second wafer which are bonded, the first wafer comprises a front side and a back side, the second wafer comprises a first surface and a second surface, a copper interconnection structure is arranged on the back side of the first wafer and the second surface side of the second wafer, an interface stack is formed on the back side of the first wafer and the second surface of the second wafer respectively, the interface stack comprises a copper diffusion barrier layer, an adhesion layer and a bonding surface in sequence from bottom to top, grooves are formed on the first wafer and the second wafer on one side close to the interface stack, the grooves penetrate the interface stack and expose the copper interconnection structure, and copper material is filled in the grooves to form copper through holes, wherein the bonding surface of the first wafer faces the bonding surface of the second wafer; A first initial copper diffusion barrier layer and a first initial oxide layer are arranged on the back side, a first copper diffusion barrier layer, a first adhesion layer and a first bonding surface are arranged on the first initial oxide layer; a second initial copper diffusion barrier layer and a second initial oxide layer are arranged on the second surface, a second copper diffusion barrier layer, a second adhesion layer and a second bonding surface are arranged on the second initial oxide layer.

Citation Information

Patent Citations

  • Bonding structure and manufacturing method thereof

    CN111244057A