Dry electrode sheet based on laser strengthening, processing method and equipment thereof
The laser channel is formed through laser processing technology and thinned in multi-stage rolling equipment, which solves the problem of low lateral tensile strength of the dry electrode sheet, and achieves the improvement of tensile strength and the improvement of production efficiency.
Patent Information
- Application Number
- CN202411221744.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The existing dry electrode sheet has a low tensile strength in the transverse direction and is prone to cracking during calendering or winding.
The intermediate film body is scanned vertically by laser processing technology to form a laser processing channel, thereby performing differential thinning in a multi-stage rolling equipment to enhance the tensile strength of the self-supporting film.
The tensile strength of the dry electrode plate in the transverse direction is effectively improved, the cracking problem is avoided, and the productivity is improved.
Smart Images

Figure CN118763184B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion battery manufacturing, and in particular to a dry electrode sheet based on laser strengthening, and a processing method and equipment thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density and long cycle life, and are widely used in new energy power and energy storage equipment.
[0003] At present, dry electrodes are a new technical direction for the development of lithium-ion batteries. The characteristic of dry electrodes is that the active material, binder and conductive agent are evenly mixed through a drying process under solvent-free conditions, and then pressed into electrodes of the desired shape. Dry electrodes have the advantages of low cost, uniform distribution of electrode components, and easy control of electrode thickness. Dry electrode pole pieces generally include a current collector and a self-supporting film disposed on the current collector. Since the self-supporting film is generally made by uniaxial stretching, the prepared self-supporting film has good tensile strength in the longitudinal direction, i.e., the machine direction (Machine Direction, MD), but low tensile strength in the transverse direction (Transverse Direction, TD), which makes the self-supporting film prone to damage and cracking during calendering or winding. Such as Figure 1 As shown, the dry electrode sheet prepared by the conventional method includes a current collector 1 and a self-supporting film 2. The self-supporting film 2 is prone to cracks 3 extending along the MD direction, indicating that the tensile strength of the self-supporting film 2 in the TD direction is relatively low. Summary of the invention
[0004] The main purpose of the present application is to provide a dry electrode plate based on laser strengthening, and its processing method and equipment, so as to solve the problem of low tensile strength in the TD direction and easy damage and cracking in the prior art.
[0005] One embodiment of the present application provides a dry electrode plate processing method based on laser strengthening, comprising the following steps:
[0006] Material mixing step: mixing and evenly dispersing the materials, the materials including: electrode main material, adhesive, conductive agent and dispersant, the mass percentage content of the adhesive is 0.5%-5%;
[0007] Fiberization step: subjecting the uniformly dispersed material to fiberization to obtain the fiberized material;
[0008] Pre-film forming step: placing the fiberized material into a multi-stage rolling device, and forming a film through a pair of rollers at differential speeds, thereby forming an intermediate film body;
[0009] Laser processing step: using laser processing equipment to perform laser scanning processing on the intermediate film body, the direction of the laser scanning processing is perpendicular to the movement direction of the intermediate film body, the laser power of the laser scanning processing is between 60W and 500W, the scanning speed of the laser scanning processing is between 1000mm / s and 5000mm / s, and the laser scanning processing process forms a plurality of laser processing grooves on the surface of the intermediate film body, and the laser processing grooves extend from one long side of the intermediate film body to the other long side of the intermediate film body;
[0010] Thinning step: subjecting the intermediate film body after the laser scanning process to differential thinning in the multi-stage rolling equipment to form a self-supporting film;
[0011] Composite step: pressing the self-supporting film and the current collector to obtain a dry electrode plate.
[0012] In one embodiment, the electrode main material includes a nickel-cobalt-manganese ternary material or a lithium iron phosphate material, the adhesive includes a polytetrafluoroethylene material, the conductive agent includes conductive carbon black or carbon nanotubes, and the dispersant includes styrene-butadiene rubber. Calculated by mass percentage, the contents of the electrode main material, the conductive agent, and the dispersant are:
[0013] The electrode main material: 92.5%-97.50%; the conductive agent: 1.5%-5%; the dispersant: 0.5%-5%.
[0014] In one embodiment, the laser processing device includes a YAG laser or a semiconductor laser;
[0015] The laser power of the YAG laser is between 60W and 100W, and the scanning speed of the YAG laser is between 1000mm / s and 5000mm / s;
[0016] The laser power of the semiconductor laser is between 200W and 500W, and the scanning speed of the semiconductor laser is between 1000mm / s and 5000mm / s.
[0017] In one embodiment, the multi-stage rolling equipment includes a first pressing roller, a second pressing roller, a third pressing roller and a fourth pressing roller, a first roller gap is formed between the first pressing roller and the second pressing roller, a second roller gap is formed between the second pressing roller and the third pressing roller, and a third roller gap is formed between the third pressing roller and the fourth pressing roller, and the fiberized material passes through the first roller gap and the second roller gap to form the intermediate film body.
[0018] In one of the embodiments, the first pressure roller, the second pressure roller, the third pressure roller and the fourth pressure roller are arranged along a first direction, and the rotation axis direction of the first pressure roller, the second pressure roller, the third pressure roller and the fourth pressure roller is a second direction perpendicular to the first direction. The laser processing equipment is arranged close to the third pressure roller to perform laser scanning processing on the intermediate film body formed after passing through the first roller gap and the second roller gap, and the scanning direction of the laser processing equipment is parallel to the second direction.
[0019] In one embodiment, the intermediate film body after the laser scanning process is subjected to a differential thinning process in the third roller gap to form the self-supporting film.
[0020] In one embodiment, the rotation speed of the first pressing roller, the second pressing roller, the third pressing roller and the fourth pressing roller ranges from 1.5 m / min to 100 m / min;
[0021] The speed ratio between two adjacent pressure rollers is between 1.1 and 10.
[0022] Another embodiment of the present application provides a dry electrode plate processing device based on laser strengthening, including a material mixing device, a material fiberizing device, a multi-stage rolling device, a laser processing device and a composite processing device;
[0023] The mixing equipment is used to mix and evenly disperse the materials, the materials including: electrode main material, adhesive, conductive agent and dispersant, the mass percentage content of the adhesive is 0.5%-5%;
[0024] The material fiberizing device is used to perform fiberizing treatment on the uniformly dispersed material to obtain the fiberized material;
[0025] The multi-stage rolling equipment includes a pre-filming mechanism and a thinning mechanism;
[0026] The pre-filming mechanism is used to film the fiberized material through a pair of rollers at differential speeds, thereby forming an intermediate film body;
[0027] The laser processing device is arranged between the pre-filming mechanism and the thinning mechanism, and is used to perform laser scanning processing on the intermediate film body. The laser power of the laser scanning processing is between 60W and 500W, and the scanning speed of the laser scanning processing is between 1000mm / s and 5000mm / s. The laser scanning processing process forms a plurality of laser processing grooves on the surface of the intermediate film body, and the laser processing grooves extend from one long side of the intermediate film body to the other long side of the intermediate film body.
[0028] The thinning mechanism performs differential thinning on the intermediate film body after the laser scanning process to form a self-supporting film;
[0029] The composite processing equipment is used to press the self-supporting film and the current collector to obtain a dry electrode plate.
[0030] Yet another embodiment of the present application provides a dry electrode plate, which is manufactured by the dry electrode plate processing method as described in any one of the above embodiments.
[0031] In one embodiment, the dry electrode plate includes the current collector and the self-supporting film disposed on the current collector;
[0032] A plurality of laser-processed channels are arranged on the surface of the self-supporting film, and the laser-processed channels extend from one long side of the self-supporting film to the other long side of the self-supporting film.
[0033] Another embodiment of the present application provides a dry electrode sheet based on laser strengthening, comprising:
[0034] a current collector; and
[0035] A self-supporting film, arranged on the surface of the current collector, wherein the surface of the self-supporting film is provided with a plurality of laser-processed channels, and the laser-processed channels are arranged to extend in a lateral direction of the self-supporting film;
[0036] The width of the laser processed channel ranges from 0.1 mm to 1 mm;
[0037] The depth of the laser processed trench ranges from 10 μm to 10 mm.
[0038] The laser-enhanced dry electrode sheet processing method, equipment, and dry electrode sheet of the present application have the following advantages and beneficial effects:
[0039] 1. In the dry electrode plate processing method provided in the present application, a laser processing step is set between the pre-filming step and the thinning step, and in the laser processing step, the intermediate film body formed in the pre-filming step is subjected to laser scanning processing by a laser processing device, the direction of the laser scanning processing is perpendicular to the movement direction of the intermediate film body, the laser power of the laser scanning processing is between 60W and 500W, and the scanning speed of the laser scanning processing is between 1000mm / s and 5000mm / s. The laser scanning processing process forms a plurality of laser processing grooves on the surface of the intermediate film body, and the laser processing grooves extend from one of the long sides of the intermediate film body to the other long side of the intermediate film body. In this embodiment, the adhesive or dispersant in the intermediate film body will produce a burning and solidifying effect under the action of the laser, thereby playing a role in improving the strength of the intermediate film body. In addition, since the direction of the laser scanning process is perpendicular to the movement direction of the intermediate film body, after the laser scanning process, a number of laser processing channels will be formed on the intermediate film body, and the laser processing channels extend from one of the long sides of the self-supporting film to the other long side of the self-supporting film. Therefore, the laser processing channels will enhance the tensile strength of the intermediate film body in the TD direction, thereby further enhancing the tensile strength of the subsequent dry electrode sheet in the TD direction. The above laser processing method can effectively avoid the problem of damage and cracking of the dry electrode sheet during the calendering and winding process, and improve the production yield of the dry electrode sheet.
[0040] 2. In one embodiment, the adhesive includes polytetrafluoroethylene material, and its mass percentage content is 0.5%-5%; the dispersant includes styrene-butadiene rubber, and its mass percentage content is 0.5%-5%. Since polytetrafluoroethylene material and styrene-butadiene rubber are both polymer materials with low melting points, under the action of laser, polytetrafluoroethylene material or styrene-butadiene rubber and other materials will be burned, melted and solidified, thereby improving the tensile strength of the intermediate film in the TD direction.
[0041] 3. In one embodiment, the laser processing equipment includes a YAG laser or a semiconductor laser. The laser power of the YAG laser is between 60W and 100W, and the scanning speed of the YAG laser is between 1000mm / s and 5000mm / s. The laser power of the semiconductor laser is between 200W and 500W, and the scanning speed of the semiconductor laser is between 1000mm / s and 5000mm / s. When a YAG laser is used, the laser power of the YAG laser is set between 60W and 100W, and the scanning speed of the YAG laser is set between 1000mm / s and 5000mm / s. The YAG laser can effectively burn, melt and solidify the polymer materials such as the adhesive or dispersant in the intermediate film body, thereby achieving the effect of improving the tensile strength of the intermediate film body in the TD direction. Similarly, when a semiconductor laser is used, the laser power of the semiconductor laser is set between 200W and 500W, and the scanning speed of the semiconductor laser is set between 1000mm / s and 5000mm / s. The semiconductor laser can effectively burn, melt and solidify the polymer materials such as the adhesive or dispersant in the intermediate film body, thereby achieving the effect of improving the tensile strength of the intermediate film body in the TD direction.
[0042] 4. In one embodiment, the multi-stage rolling device is configured to include a first roller, a second roller, a third roller and a fourth roller. A first roller gap is formed between the first roller and the second roller, and a second roller gap is formed between the second roller and the third roller. The fiberized material passes through the first roller gap and the second roller gap to form the intermediate film body. After the rolling process of the first roller gap and the second roller gap, the intermediate film body can be roughly formed, which is convenient for subsequent laser scanning processing operations.
[0043] 5. In one embodiment, the laser processing device is arranged close to the third pressure roller to perform laser scanning processing on the intermediate film body formed after passing through the first roller gap and the second roller gap. On the one hand, after the rolling process of the first roller gap and the second roller gap, the intermediate film body can be roughly formed, which is convenient for the subsequent laser scanning processing operation. On the other hand, since the intermediate film body has been roughly formed, when the intermediate film body after the laser scanning processing continues to be thinned, the traces formed by the laser scanning processing on the intermediate film body will not change too much, so that the intermediate film body after the laser scanning processing can still maintain its high tensile strength in the TD direction after the thinning processing.
[0044] 6. In one embodiment, the rotation speed range of the first pressing roller, the second pressing roller, the third pressing roller and the fourth pressing roller is between 1.5 m / min and 100 m / min; the speed ratio between two adjacent pressing rollers is between 1.1 and 10. The difference in rotation speed between the first pressing roller and the second pressing roller, and the difference in rotation speed between the second pressing roller and the third pressing roller, can effectively form the intermediate film body after the fiberized material passes through the first roller gap and the second roller gap, and roughly shape the intermediate film body. At the same time, the rotation speed of the third pressing roller and the laser scanning speed of the laser processing equipment also jointly determine the shape of the laser processing trace formed by the laser processing equipment on the intermediate film body. Therefore, setting the rotation speed of the third pressing roller to between 1.5 m / min and 100 m / min can make the shape of the laser processing trace formed on the intermediate film body more effectively improve the tensile strength of the intermediate film body in the TD direction.
[0045] 7. In one embodiment, the dry electrode plate includes the current collector and the self-supporting film disposed on the current collector. The surface of the self-supporting film is provided with a plurality of laser-processed channels, and the laser-processed channels extend from one of the long sides of the self-supporting film to the other long side of the self-supporting film. As mentioned above, the laser-processed channels are formed by the adhesive or dispersant in the intermediate film body under the action of laser, thereby playing a role in improving the strength of the intermediate film body. In addition, since the laser-processed channels extend from one of the long sides of the self-supporting film to the other long side of the self-supporting film, the laser-processed channels will play a role in improving the tensile strength of the intermediate film body in the TD direction, thereby further improving the tensile strength of the dry electrode plate in the TD direction.
[0046] 8. In one embodiment, the surface of the self-supporting film is provided with a plurality of laser-processed grooves, and the laser-processed grooves are arranged along the lateral extension of the self-supporting film. Since the width of the laser-processed grooves ranges from 0.1 mm to 1 mm, and the depth of the laser-processed grooves ranges from 10 μm to 10 mm, the adhesive or dispersant in the self-supporting film will be burned and solidified under the action of the laser, thereby improving the tensile strength of the self-supporting film. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0048] Figure 1 A schematic diagram of a self-supporting film in a dry electrode sheet in the prior art being broken;
[0049] Figure 2 A schematic diagram of the steps of a dry electrode sheet processing method disclosed in one of the embodiments of the present application;
[0050] Figure 3 for Figure 2 A schematic diagram of the structure of a multi-stage rolling equipment;
[0051] Figure 4 for Figure 3 Schematic diagram of the structure of the middle film layer after laser scanning processing;
[0052] Figure 5 for Figure 4 A schematic top view of the intermediate film layer in FIG.
[0053] Figure 6 for Figure 4 A schematic top view of another embodiment of the intermediate film layer in FIG.
[0054] Figure 7 This is a surface SEM photo of a dry electrode sheet that has not been laser treated.
[0055] Figure 8 This is a surface SEM photo of a dry electrode sheet made by laser treatment;
[0056] Fig. 9 This is a cross-sectional picture of a dry electrode piece made by laser scanning using a YAG laser;
[0057] Fig.10 This is a cross-sectional picture of a dry electrode piece made by laser scanning using a semiconductor laser;
[0058] Fig.11 The 400-cycle capacity retention test data of the dry electrode sheet without laser treatment and the dry electrode sheet after laser treatment after being made into lithium-ion batteries;
[0059] Fig.12 A schematic structural diagram of a dry electrode sheet processing device provided in another embodiment of the present application;
[0060] Fig.13 A schematic structural diagram of a dry electrode plate provided in yet another embodiment of the present application. DETAILED DESCRIPTION
[0061] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0062] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0063] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values of the parts and steps set forth in these embodiments do not limit the scope of the application. Meanwhile, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to actual proportional relationships. The technology, methods and equipment known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology, methods and equipment should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, and therefore, once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.
[0064] See also Figures 2 to 5 One embodiment of the present application provides a dry electrode plate processing method based on laser strengthening. The dry electrode plate processing method comprises the following steps:
[0065] Material mixing step: Mix and evenly disperse the materials, the materials including: electrode main material, adhesive, conductive agent and dispersant, the mass percentage of the adhesive is 0.5%-5%. In this embodiment, the electrode main material, the adhesive, the conductive agent and the dispersant are mechanically mixed to form a uniform dry powder mixture. The equipment used for mechanical mixing can be a high-speed high-power mixer or a ball mill.
[0066] Fiberization step: The uniformly dispersed material is subjected to fiberization treatment to obtain the fiberized material. In this embodiment, the fiberization process is to process the adhesive into a form with a fibrous structure, so that it is easier to combine with the electrode main material, the conductive agent and other components during the dry mixing process. This step is also called the fibrillation step (Fibrillation). The adhesive is processed into a form with a fibrous structure mainly to enable the adhesive to fully exert its bonding effect in a dry state, thereby enhancing the adhesion and mechanical strength of the mixture. Through the fiberization step, the adhesive can firmly combine the electrode main material and the conductive agent and other components. In one embodiment, the fiberization process is mainly to apply high shear force to the mixed material, so that the adhesive is fiberized and then bonded to the electrode main material and the conductive agent and other materials to form the fiberized material.
[0067] Pre-film forming step: the fiberized material is placed in a multi-stage rolling device, and the film is formed by differential speed of the rollers to form an intermediate film body 10. As needed, the fiberized material can be granulated before being placed in the multi-stage rolling device. The granulation process can make the fiberized material into granules through a mechanical granulation process. After the granulation process, the granules have good fluidity and handling characteristics, so that they are suitable for the subsequent film forming step. Generally speaking, during the granulation process, the density and shape of the particles should be consistent, and have sufficient mechanical strength so that the particles will not break or pulverize during the processing.
[0068] Laser processing step: The intermediate film body 10 is subjected to laser scanning processing by using a laser processing device. The direction of the laser scanning processing is perpendicular to the movement direction of the intermediate film body 10. The laser power of the laser scanning processing is between 60W and 500W. The scanning speed of the laser scanning processing is between 1000mm / s and 5000mm / s. The laser scanning processing process forms a plurality of laser processing grooves 11 on the surface of the intermediate film body 10. The laser processing grooves 11 extend from one long side of the intermediate film body 10 to the other long side of the intermediate film body 10. Please refer to Figure 5 In this embodiment, a plurality of laser-processed channels 11 are connected end to end to form a multi-segment bending shape. It can be understood that the shape of the plurality of laser-processed channels 11 is not limited to the above embodiment. Figure 6 In another embodiment, a plurality of laser processing channels 11 are arranged in parallel to each other to form a plurality of parallel line segments. As required, the laser processing device may also be provided with a plurality of laser heads, which perform laser scanning processing simultaneously to form a plurality of laser processing channels.
[0069] Thinning step: The intermediate film body 10 after the laser scanning process is subjected to differential thinning in the multi-stage rolling equipment to form a self-supporting film. In this embodiment, the thinning step can reduce the thickness and increase the density of the intermediate film body 10 to enhance its electrode performance, thereby forming a final self-supporting film. The thickness of the self-supporting film is generally between 40μm and 150μm. The self-supporting film has good compaction to ensure good conductivity and mechanical strength. In this embodiment, after the laser-processed channel 11 is processed by the thinning step, its width ranges from 0.1-1mm and its depth ranges from 10μm-10 mm.
[0070] Composite step: Press the self-supporting film and the current collector to obtain a dry electrode plate. In this embodiment, the current collector can be a copper foil or an aluminum foil. In the process of combining the self-supporting film and the current collector, a hot press or rolling press device can be used to firmly combine the self-supporting film and the current collector. As needed, before the self-supporting film is combined with the current collector, the current collector can be surface treated to enhance the adhesion of the current collector, so that the self-supporting film and the current collector can be more firmly combined to obtain the dry electrode plate.
[0071] In the dry electrode plate processing method provided in the above embodiment, a laser processing step is provided between the pre-filming step and the thinning step, and in the laser processing step, the intermediate film body 10 formed in the pre-filming step is subjected to laser scanning processing by a laser processing device, the direction of the laser scanning processing is perpendicular to the movement direction of the intermediate film body 10, the laser power of the laser scanning processing is between 60W and 500W, and the scanning speed of the laser scanning processing is between 1000mm / s and 5000mm / s. The laser scanning processing process forms a plurality of laser processing grooves 11 on the surface of the intermediate film body 10, and the laser processing grooves 11 extend from one of the long sides of the intermediate film body 10 to the other long side of the intermediate film body 10. In this embodiment, the adhesive or dispersant in the intermediate film body 10 will produce a burning and solidifying effect under the action of the laser, thereby playing a role in improving the strength of the intermediate film body 10. In addition, since the direction of the laser scanning process is perpendicular to the movement direction of the intermediate film body 10, after the laser scanning process, the intermediate film body 10 will form a number of laser processing channels, and the laser processing channels extend from one of the long sides of the self-supporting film to the other long side of the self-supporting film. Therefore, the laser processing channels will enhance the tensile strength of the intermediate film body 10 in the TD direction, thereby further enhancing the tensile strength of the subsequent dry electrode sheet in the TD direction. The above laser processing method can effectively avoid the problem of damage and cracking of the dry electrode sheet during the calendering and winding process, and improve the production yield of the dry electrode sheet.
[0072] In practice, in the conventional production process of dry electrode plates, the self-supporting film is generally made by uniaxial stretching. Therefore, the prepared self-supporting film has good tensile strength in the MD direction and low tensile strength in the TD direction, which makes the self-supporting film prone to cracks extending along the MD direction. In the dry electrode plate processing method provided in this embodiment, the intermediate film body 10 formed by the pre-filming step is laser scanned by a laser processing device, and the direction of the laser scanning processing is perpendicular to the movement direction of the intermediate film body 10. At this time, during the laser processing process, the adhesive or dispersant in the intermediate film body 10 will produce a burning and solidification effect under the action of the laser, thereby forming a number of laser processing channels 11. The laser processing channel 11 extends from one of the long sides of the intermediate film body 10 to the other long side of the intermediate film body 10, thereby playing a role in improving the tensile strength of the intermediate film body 10 in the TD direction.
[0073] In one embodiment, the electrode main material includes a nickel-cobalt-manganese ternary material or a lithium iron phosphate material, the adhesive includes a polytetrafluoroethylene material, the conductive agent includes conductive carbon black or carbon nanotubes, and the dispersant includes styrene-butadiene rubber. Calculated by mass percentage, the mass percentage contents of the electrode main material, the conductive agent, and the dispersant are respectively:
[0074] The electrode main material: 92.5%-97.50%; the conductive agent: 1.5%-5%; the dispersant: 0.5%-5%.
[0075] In this embodiment, the adhesive includes polytetrafluoroethylene material, and its mass percentage content is 0.5%-5%; the dispersant includes styrene-butadiene rubber, and its mass percentage content is 0.5%-5%. Since polytetrafluoroethylene material and styrene-butadiene rubber are both polymer materials with low melting points, under the action of laser, polytetrafluoroethylene material or styrene-butadiene rubber and other materials will be burned, melted and solidified, thereby improving the tensile strength of the intermediate film body 10 in the TD direction. In fact, since the laser-processed channel 11 is mainly formed by the adhesive in the intermediate film body 10 being burned and solidified under the action of laser, it plays a role in improving the tensile strength of the intermediate film body 10. Therefore, the content of the adhesive has a relatively large impact on the tensile strength of the intermediate film body 10. The higher the content of the adhesive, the greater its effect on improving the tensile strength after laser scanning. The lower the content of the adhesive, the smaller its effect on improving the tensile strength after laser scanning. However, since the content of the adhesive also affects the characteristics of the self-supporting film, such as compaction density and porosity, generally speaking, the mass percentage of the adhesive is selected to be up to 5%.
[0076] In one embodiment, the laser processing equipment includes a YAG laser or a semiconductor laser.
[0077] The laser power of the YAG laser is between 60W and 100W, and the scanning speed of the YAG laser is between 1000mm / s and 5000mm / s.
[0078] The laser power of the semiconductor laser is between 200W and 500W, and the scanning speed of the semiconductor laser is between 1000mm / s and 5000mm / s.
[0079] In this embodiment, when a YAG laser is used, the laser power of the YAG laser is set between 60W and 100W, and the scanning speed of the YAG laser is set between 1000mm / s and 5000mm / s, and the YAG laser can effectively burn, melt and solidify the polymer materials such as the adhesive or dispersant in the intermediate film body 10, thereby achieving the effect of improving the tensile strength in the TD direction of the intermediate film body 10. Similarly, when a semiconductor laser is used, the laser power of the semiconductor laser is set between 200W and 500W, and the scanning speed of the semiconductor laser is set between 1000mm / s and 5000mm / s, and the semiconductor laser can effectively burn, melt and solidify the polymer materials such as the adhesive or dispersant in the intermediate film body 10, thereby achieving the effect of improving the tensile strength in the TD direction of the intermediate film body 10.
[0080] In fact, since the laser-processed channel 11 is mainly formed by the adhesive and the like in the intermediate film body 10 being burned and solidified under the action of the laser, the lower the power of the laser, the lower its burning ability for materials such as adhesives, so that the effect of strengthening the tensile strength of the intermediate film body 10 is worse. Similarly, the higher the power of the laser, the stronger its burning ability for materials such as adhesives, so that the effect of strengthening the tensile strength of the intermediate film body 10 is better. Similarly, the higher the scanning speed of the laser, the lower its burning ability for materials such as adhesives, so that the effect of strengthening the tensile strength of the intermediate film body 10 is worse. The lower the scanning speed of the laser, the stronger its burning ability for materials such as adhesives, so that the effect of strengthening the tensile strength of the intermediate film body 10 is better.
[0081] Table 1 shows the effects of laser power, scanning speed, and adhesive content on the tensile strength of dry electrode sheets.
[0082]
[0083] For dry-process electrode sheets that have not been treated with lasers, when the content of the adhesive is 0.5% (wt), the tensile strength is 0.2MPa. The dry-process electrode sheets produced have cracks along the MD direction during the winding process, indicating that the tensile strength in the TD direction is relatively low. For dry-process electrode sheets that have not been treated with lasers, when the content of the adhesive is 5% (wt), the tensile strength is 0.55MPa. The dry-process electrode sheets produced have no cracks in the MD direction during the winding process.
[0084] 1. Using YAG laser:
[0085] When using a YAG laser, the YAG laser power is selected as 50W, 60W, 65W, and 100W. The lower the laser power, the lower the burning ability and the worse the strengthening effect. The higher the laser power, the stronger the burning ability and the better the strengthening effect. The scanning speed of the laser is set to 5000mm / s and 1000mm / s. The higher the scanning rate, the lower the burning ability and the worse the strengthening effect. The lower the scanning rate, the stronger the burning ability and the better the strengthening effect. The content of the adhesive is selected as 0.5% (wt) and 5% (wt). The lower the content of the adhesive, the worse the strengthening effect after laser treatment. The higher the content of the adhesive, the better the strengthening effect after laser treatment.
[0086] Using a 50W YAG laser, a scanning speed of 5000mm / s, and a binder content of 0.5% (wt), the tensile strength of the dry electrode sheet is 0.35MPa, and the MD direction of the dry electrode sheet is damaged during the winding process. Using a 50W YAG laser, a scanning speed of 5000mm / s, and a binder content of 5% (wt), the tensile strength of the dry electrode sheet is 0.85MPa, and the MD direction of the dry electrode sheet is not damaged during the winding process.
[0087] Using a 60W YAG laser, a scanning speed of 5000mm / s, and a binder content of 0.5% (wt), the tensile strength of the dry electrode sheet is 0.55MPa, and no damage or cracking occurs in the MD direction of the dry electrode sheet during the winding process.
[0088] Using a 65W YAG laser, a scanning speed of 5000mm / s, and a binder content of 0.5% (wt), the tensile strength of the dry electrode sheet is 0.60MPa, and no damage or cracking occurs in the MD direction of the dry electrode sheet during the winding process.
[0089] Using a 100W YAG laser, a scanning speed of 1000mm / s, and a binder content of 0.5% (wt), the tensile strength of the dry electrode sheet is 0.65MPa, and the dry electrode sheet has no damage or cracking in the MD direction. Using a 100W YAG laser, a scanning speed of 1000mm / s, and a binder content of 5% (wt), the tensile strength of the dry electrode sheet is 1.25MPa, and the dry electrode sheet has no damage or cracking in the MD direction.
[0090] The above data show that by adjusting the laser power, scanning speed and binder content of the YAG laser, the strength of the dry electrode in the TD direction can be improved, which can effectively prevent the dry electrode from producing cracks extending along the MD direction. In addition, when the binder content is 0.5% - 5% (wt), the laser power of the YAG laser is selected between 60W and 100W, so that the dry electrode will not be damaged during the winding process. At the same time, compared with the dry electrode that has not been laser treated, the tensile strength of the dry electrode treated by the YAG laser is significantly improved when the binder content is the same.
[0091] 2. Using semiconductor laser:
[0092] When a semiconductor laser is used, the laser power of the semiconductor laser is set to 200W and 500W. The lower the laser power, the lower the burning ability and the worse the strengthening effect. The higher the laser power, the stronger the burning ability and the better the strengthening effect. The scanning speed of the semiconductor laser is set to 5000mm / s and 1000mm / s. The higher the scanning rate, the lower the burning ability and the worse the strengthening effect. The lower the scanning rate, the stronger the burning ability and the better the strengthening effect. The content of the adhesive is selected as 0.5% (wt) and 5% (wt). The lower the content of the adhesive, the worse the strengthening effect after laser treatment. The higher the content of the adhesive, the better the strengthening effect after laser treatment.
[0093] Using a 200W semiconductor laser, a scanning speed of 5000mm / s, a binder content of 0.5% (wt), the tensile strength of the dry electrode sheet is 0.55MPa. The MD direction of the dry electrode sheet did not show any damage or cracking during the winding process. Using a 200W semiconductor laser, a scanning speed of 5000mm / s, a binder content of 5% (wt), the tensile strength of the dry electrode sheet is 1.05MPa, and the MD direction of the dry electrode sheet did not show any damage or cracking during the winding process.
[0094] Using a 500W semiconductor laser, a scanning speed of 1000mm / s, and a binder content of 0.5% (wt), the tensile strength of the dry electrode sheet is 1.05MPa, and no damage or cracking occurs in the MD direction of the dry electrode sheet. Using a 500W semiconductor laser, a scanning speed of 1000mm / s, and a binder content of 5% (wt), the tensile strength of the dry electrode sheet is 1.45MPa, and no damage or cracking occurs in the MD direction of the dry electrode sheet.
[0095] The above data show that by adjusting the power of the semiconductor laser, the scanning speed, and the binder content, the tensile strength of the dry electrode pole piece in the TD direction can be improved, and the dry electrode pole piece can be effectively prevented from cracking along the MD direction. In addition, since the laser power of the semiconductor laser is higher than that of the YAG laser, the process window of the semiconductor laser is wider, and the effect of preventing the dry electrode pole piece from being damaged in the MD direction is better. Moreover, compared with the dry electrode pole piece that has not been laser-treated, the tensile strength of the dry electrode pole piece that has been laser-treated by the semiconductor laser is significantly improved when the adhesive content is the same. Moreover, the dry electrode pole piece that has been laser-treated by the semiconductor laser did not show any damage or cracking during the winding process.
[0096] Please also see Figure 3 In one embodiment, the multi-stage rolling device includes a first roller 110, a second roller 120, a third roller 130 and a fourth roller 140. A first roller gap 111 is formed between the first roller 110 and the second roller 120. A second roller gap 121 is formed between the second roller 120 and the third roller 130. A third roller gap 131 is formed between the third roller 130 and the fourth roller 140. The fiberized material passes through the first roller gap 111 and the second roller gap 112 to form the intermediate film body 10.
[0097] In this embodiment, the fiberized material passes through the first roller gap 111 and the second roller gap 121 to form the intermediate film body 10. After the rolling process of the first roller gap 111 and the second roller gap 121, the intermediate film body 10 can be roughly formed, which is convenient for subsequent laser scanning processing operations.
[0098] In one embodiment, the first pressing roller 110, the second pressing roller 120, the third pressing roller 130 and the fourth pressing roller 140 are arranged along the first direction. In this embodiment, the first direction is the MD direction of the dry electrode sheet, or the movement direction of the dry electrode sheet. The rotation axis direction of the first pressing roller 110, the second pressing roller 120, the third pressing roller 130 and the fourth pressing roller 140 is a second direction perpendicular to the first direction. In this embodiment, the second direction is the TD direction of the dry electrode sheet, or the lateral direction of the dry electrode sheet. The laser processing equipment 20 is arranged close to the third pressing roller 130 to perform laser scanning processing on the intermediate film body 10 formed after passing through the first roller gap 111 and the second roller gap 121. The scanning direction of the laser processing equipment 20 is parallel to the second direction.
[0099] In this embodiment, the laser processing device 20 is arranged close to the third pressing roller 130 to perform laser scanning processing on the intermediate film body 10 formed after passing through the first roller gap 111 and the second roller gap 121. On the one hand, after the rolling process of the first roller gap 111 and the second roller gap 121, the intermediate film body 10 can be roughly formed, which is convenient for the subsequent laser scanning processing operation. On the other hand, since the intermediate film body 10 has been roughly formed, when the intermediate film body 10 after the laser scanning processing continues to be thinned, the traces formed by the laser scanning processing on the intermediate film body 10 will not change too much, so that the intermediate film body 10 after the laser scanning processing can still maintain its high tensile strength in the TD direction after the thinning processing.
[0100] In this embodiment, the intermediate film body 10 after the laser scanning process is subjected to differential thinning process in the third roller gap 131 to form the self-supporting film. As required, the multi-stage rolling equipment can further increase the number of rollers to adjust the thickness and compaction density of the dry electrode sheet. In one embodiment, the multi-stage rolling equipment includes 10 or more rollers.
[0101] In one embodiment, the rotation speed of the first pressing roller, the second pressing roller, the third pressing roller and the fourth pressing roller ranges from 1.5 m / min to 100 m / min.
[0102] The speed ratio between two adjacent pressure rollers is between 1.1 and 10.
[0103] In this embodiment, the speed ratio between the first pressing roller 110 and the second pressing roller 120 is set between 1.1 and 10, and the speed ratio between the second pressing roller 120 and the third pressing roller 130 is set between 1.1 and 10, so that the fiberized material can effectively form the intermediate film body 10 after passing through the first roller gap 111 and the second roller gap 121, and the intermediate film body 10 can be roughly formed. At the same time, the rotation speed of the third pressing roller 130 and the laser scanning speed of the laser processing device 20 also jointly determine the shape of the laser processing trace formed by the laser processing device 20 on the intermediate film body 10. Therefore, setting the rotation speed range of the third pressing roller 130 between 1.5 m / min and 100 m / min can make the shape of the laser processing trace formed on the intermediate film body 10 more effectively improve the tensile strength of the intermediate film body 10 in the TD direction.
[0104] Figure 7 The surface SEM (scanning electron microscope) photograph of the dry electrode sheet made without laser treatment is given. Figure 8 The surface SEM (scanning electron microscope) photos of the dry electrode sheet made by laser treatment are given. It can be clearly seen from the figure that compared with the dry electrode sheet made without laser treatment, the dry electrode sheet made by laser treatment has its adhesive burned, melted and solidified under the action of laser after laser scanning, and its fiberization effect is more obvious, which can effectively improve the tensile strength of the dry electrode sheet in the TD direction.
[0105] Fig. 9 The cross-sectional picture of the dry electrode piece made by laser scanning with YAG laser is given. Fig.10 The cross-sectional image of the dry electrode piece made by laser scanning with a semiconductor laser is given. Fig. 9 In the experiment, the laser power of the YAG laser was 50W, the scanning speed was 5000mm / s, and the content of the adhesive was 0.5% (wt). Fig.10 The laser power of the semiconductor laser is 200W, the scanning speed is 5000mm / s, and the content of the adhesive is 0.5% (wt). Fig. 9 It can be seen that the laser processing channel formed by the YAG laser is narrow in width and shallow in depth, so it cannot effectively improve the tensile strength of the dry electrode sheet in the TD direction. The test data also proves that the tensile strength of the dry electrode sheet produced in this way is 0.35MPa, and the dry electrode sheet produces cracks along the MD direction during the winding process. Fig.10 It can be seen that the laser-processed channel formed by the semiconductor laser is wider and deeper, which can effectively improve the tensile strength of the dry electrode sheet in the TD direction. The test data also proves that the tensile strength of the dry electrode sheet produced in this way is 0.55MPa. There is no damage or cracking in the MD direction of the dry electrode sheet during the winding process.
[0106] Table 2 shows the test results of the 7-day 55°C capacity retention rate (5.5Ah) of the dry electrode sheet made without laser treatment after being made into a lithium-ion battery. Among them, the 7-day 55°C capacity retention rate refers to the ability of the battery to maintain its capacity after being placed in an environment of 55°C for 7 days. Table 3 shows the test results of the 7-day 55°C capacity retention rate (5.5Ah) of the dry electrode sheet made by laser treatment after being made into a lithium-ion battery. A total of 10 samples were tested in each table, and their average values were calculated.
[0107]
[0108]
[0109] As can be seen from Table 2 and Table 3, in the 7-day 55°C capacity retention rate (5.5Ah) test results, the dry electrode plate made without laser treatment has a capacity retention rate of 98.19% and a capacity recovery rate of 99.24% after being made into a lithium-ion battery; while the dry electrode plate made with laser treatment has a capacity retention rate of 98.54% and a capacity recovery rate of 99.62% after being made into a lithium-ion battery. That is, compared with the dry electrode plate made without laser treatment, the dry electrode plate made with laser treatment has improved capacity retention rate and capacity recovery rate after being made into a lithium-ion battery.
[0110] Fig.11 The 400-cycle capacity retention rate test data of dry electrode sheets made without laser treatment and dry electrode sheets made with laser treatment after being made into lithium-ion batteries are given. Among them, the 400-cycle capacity retention rate refers to the ability of the battery to maintain its capacity after 400 cycles. Fig.11 It can be seen that the dry electrode sheet without laser treatment has a 400-week capacity retention rate of 80.11% after being made into a lithium-ion battery. The dry electrode sheet with laser treatment has a 400-week capacity retention rate of 80.31% after being made into a lithium-ion battery. Similarly, compared with the dry electrode sheet without laser treatment, the dry electrode sheet with laser treatment has a higher 400-week capacity retention rate after being made into a lithium-ion battery.
[0111] Table 4 shows the K value test data of the dry electrode plate made by laser treatment after being made into a lithium-ion battery. Table 5 shows the K value test data of the dry electrode plate made without laser treatment after being made into a lithium-ion battery. The K value is an important indicator to measure the self-discharge degree of lithium-ion batteries. It refers to the voltage drop of lithium-ion batteries per unit time. K=△OCT / △t, OCV refers to the open circuit voltage, t is the storage time. The unit of K value is mV / d, which is related to the performance of the battery itself, the test conditions, the positive and negative electrode materials, and the length of storage time.
[0112]
[0113]
[0114] As can be seen from Table 4 and Table 5, in terms of the K value test results, the dry electrode plates made without laser treatment have an average K value of 0.02 and an average yield of 98.97% after being made into lithium-ion batteries; while the dry electrode plates made with laser treatment have an average K value of 0.01 and an average yield of 99.19% after being made into lithium-ion batteries. That is, compared with the dry electrode plates made without laser treatment, the dry electrode plates made with laser treatment have improved K value and yield after being made into lithium-ion batteries.
[0115] See also Fig.12 Another embodiment of the present application provides a dry electrode plate processing device 200, including a mixing device 210, a material fiberization device 220, a multi-stage rolling device 230, a laser processing device 240 and a composite processing device 250.
[0116] The mixing device 210 is used to mix and evenly disperse the materials, which include: electrode main material, adhesive, conductive agent and dispersant. The mass percentage content of the adhesive is 0.5%-5%.
[0117] The material fiberizing device 220 is used to perform fiberizing treatment on the uniformly dispersed material to obtain the fiberized material.
[0118] The multi-stage rolling device 230 includes a pre-film forming mechanism 231 and a thinning mechanism 232 .
[0119] The pre-filming mechanism 231 is used to film the fiberized material through a pair of rollers at differential speeds, thereby forming an intermediate film body.
[0120] The laser processing device 240 is arranged between the pre-film forming mechanism 231 and the thinning mechanism 232. The laser processing device 240 is used to perform laser scanning processing on the intermediate film body. The laser power of the laser scanning processing is between 60W and 500W, and the scanning speed of the laser scanning processing is between 1000mm / s and 5000mm / s. The process of the laser scanning processing forms a plurality of laser processing grooves on the surface of the intermediate film body. The laser processing grooves extend from one long side of the intermediate film body to the other long side of the intermediate film body.
[0121] The thinning mechanism 232 performs differential thinning on the intermediate film after the laser scanning process to form a self-supporting film.
[0122] The composite processing equipment 250 is used to press the self-supporting film and the current collector to obtain a dry electrode plate.
[0123] See also Fig.13Another embodiment of the present application provides a dry electrode plate 300 based on laser strengthening, and the dry electrode plate 300 is manufactured by the dry electrode plate processing method as described in any of the above embodiments.
[0124] In one embodiment, the dry electrode plate 300 includes the current collector 310 and the self-supporting film 320 disposed on the current collector 310 .
[0125] A plurality of laser-processed channels 321 are disposed on the surface of the self-supporting film 320 . The laser-processed channels 321 extend from one long side of the self-supporting film 320 to the other long side of the self-supporting film 320 .
[0126] In this embodiment, the dry electrode plate 300 includes the current collector 310 and the self-supporting film 320 disposed on the current collector 310. The surface of the self-supporting film 320 is provided with a plurality of laser-processed channels 321, and the laser-processed channels 321 extend from one of the long sides of the self-supporting film 320 to the other long side of the self-supporting film 320. As mentioned above, the laser-processed channels are formed by the adhesive or dispersant in the intermediate film body under the action of laser, thereby playing a role in improving the strength of the intermediate film body. In addition, since the laser-processed channels 321 extend from one of the long sides of the self-supporting film 320 to the other long side of the self-supporting film 320, the laser-processed channels 321 will play a role in improving the tensile strength of the intermediate film body in the TD direction, thereby further improving the tensile strength of the dry electrode plate 300 in the TD direction.
[0127] Another embodiment of the present application provides a dry electrode sheet based on laser strengthening, comprising:
[0128] a current collector; and
[0129] A self-supporting film, arranged on the surface of the current collector, wherein the surface of the self-supporting film is provided with a plurality of laser-processed channels, and the laser-processed channels are arranged to extend in a lateral direction of the self-supporting film;
[0130] The width of the laser processed channel ranges from 0.1 mm to 1 mm;
[0131] The depth of the laser processed trench ranges from 10 μm to 10 mm.
[0132] In this embodiment, a plurality of laser-processed grooves are arranged on the surface of the self-supporting film, and the laser-processed grooves are arranged along the lateral extension of the self-supporting film. Since the width of the laser-processed grooves ranges from 0.1 mm to 1 mm, and the depth of the laser-processed grooves ranges from 10 μm to 10 mm, the adhesive or dispersant in the self-supporting film will be burned and solidified under the action of the laser, thereby improving the tensile strength of the self-supporting film. In this embodiment, the depth of the laser-processed grooves does not exceed the thickness of the self-supporting film.
[0133] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used herein to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" may include both "above" and "below". The device may also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used herein are interpreted accordingly.
[0134] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of this application.
[0135] The above are only preferred embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A dry electrode processing method based on laser strengthening, It is characterized in that The following steps are involved: Material mixing step: mixing and evenly dispersing the materials, the materials include: electrode main material, adhesive, conductive agent and dispersant, the mass percentage content of the adhesive is 0.5%-5%; calculated by mass percentage, the content of the electrode main material, the conductive agent and the dispersant is: the electrode main material: 92.5%-97.50%; the conductive agent: 1.5%-5%; the dispersant: 0.5%-5%; Fiberization step: subjecting the uniformly dispersed material to fiberization to obtain the fiberized material; Pre-film forming step: placing the fiberized material into a multi-stage rolling device, and forming a film through a pair of rollers at differential speeds, thereby forming an intermediate film body; Laser processing step: using laser processing equipment to perform laser scanning processing on the intermediate film body, the direction of the laser scanning processing is perpendicular to the movement direction of the intermediate film body, the laser power of the laser scanning processing is between 60W and 500W, the scanning speed of the laser scanning processing is between 1000mm / s and 5000mm / s, and the laser scanning processing process forms a plurality of laser processing grooves on the surface of the intermediate film body, and the laser processing grooves extend from one long side of the intermediate film body to the other long side of the intermediate film body; Thinning step: subjecting the intermediate film body after the laser scanning process to differential thinning in the multi-stage rolling equipment to form a self-supporting film; Composite step: pressing the self-supporting film and the current collector to obtain a dry electrode sheet; Wherein, the laser processing equipment includes a YAG laser or a semiconductor laser; the laser power of the YAG laser is between 60W and 100W, and the scanning speed of the YAG laser is between 1000mm / s and 5000mm / s; the laser power of the semiconductor laser is between 200W and 500W, and the scanning speed of the semiconductor laser is between 1000mm / s and 5000mm / s; The adhesive or the dispersant in the intermediate film body will be burned and solidified under the action of the laser, thereby improving the strength of the intermediate film body.
2. The method for processing a dry electrode sheet based on laser strengthening according to claim 1, It is characterized in that The electrode main material includes nickel-cobalt-manganese ternary material or lithium iron phosphate material, the adhesive includes polytetrafluoroethylene material, the conductive agent includes conductive carbon black or carbon nanotubes, and the dispersant includes styrene-butadiene rubber.
3. The dry electrode plate processing method based on laser strengthening according to claim 2, It is characterized in that The multi-stage rolling equipment includes a first pressing roller, a second pressing roller, a third pressing roller and a fourth pressing roller. A first roller gap is formed between the first pressing roller and the second pressing roller, a second roller gap is formed between the second pressing roller and the third pressing roller, and a third roller gap is formed between the third pressing roller and the fourth pressing roller. The fiberized material passes through the first roller gap and the second roller gap to form the intermediate film body.
4. The dry electrode sheet processing method according to claim 3, It is characterized in that The first pressing roller, the second pressing roller, the third pressing roller and the fourth pressing roller are arranged along a first direction, and the rotation axis direction of the first pressing roller, the second pressing roller, the third pressing roller and the fourth pressing roller is a second direction perpendicular to the first direction. The laser processing equipment is arranged close to the third pressing roller to perform laser scanning processing on the intermediate film body formed after passing through the first roller gap and the second roller gap, and the scanning direction of the laser processing equipment is parallel to the second direction.
5. The method for processing a dry electrode sheet based on laser strengthening according to claim 3, It is characterized in that The intermediate film body after the laser scanning process is subjected to a differential speed thinning process in the third roller gap to form the self-supporting film.
6. The method for processing a dry electrode sheet based on laser strengthening according to claim 4, It is characterized in that The rotation speeds of the first pressing roller, the second pressing roller, the third pressing roller and the fourth pressing roller are in a range of 1.5 m / min to 100 m / min; The speed ratio between two adjacent pressure rollers is between 1.1 and 10.
7. A dry electrode plate processing device based on laser strengthening, used to perform the dry electrode plate processing method based on laser strengthening according to any one of claims 1 to 6, It is characterized in that Including mixing equipment, material fiberization equipment, multi-stage rolling equipment, laser processing equipment and composite processing equipment; The mixing equipment is used to mix and evenly disperse the materials, the materials including: electrode main material, adhesive, conductive agent and dispersant, the mass percentage content of the adhesive is 0.5%-5%; The material fiberizing device is used to perform fiberizing treatment on the uniformly dispersed material to obtain the fiberized material; The multi-stage rolling equipment includes a pre-filming mechanism and a thinning mechanism; The pre-filming mechanism is used to film the fiberized material through a pair of rollers at differential speeds, thereby forming an intermediate film body; The laser processing device is arranged between the pre-filming mechanism and the thinning mechanism, and is used to perform laser scanning processing on the intermediate film body. The laser power of the laser scanning processing is between 60W and 500W, and the scanning speed of the laser scanning processing is between 1000mm / s and 5000mm / s. The laser scanning processing process forms a plurality of laser processing grooves on the surface of the intermediate film body, and the laser processing grooves extend from one long side of the intermediate film body to the other long side of the intermediate film body. The thinning mechanism performs differential thinning on the intermediate film body after the laser scanning process to form a self-supporting film; The composite processing equipment is used to press the self-supporting film and the current collector to obtain a dry electrode plate.
8. A dry electrode sheet based on laser strengthening, It is characterized in that The dry electrode plate is manufactured by the dry electrode plate processing method as described in any one of claims 1-6.
9. The dry electrode sheet based on laser strengthening according to claim 8, It is characterized in that comprising the current collector and the self-supporting film disposed on the current collector; A plurality of laser-processed channels are arranged on the surface of the self-supporting film, and the laser-processed channels extend from one long side of the self-supporting film to the other long side of the self-supporting film.
10. A laser-enhanced dry electrode sheet, manufactured by the laser-enhanced dry electrode sheet processing method according to any one of claims 1 to 6, It is characterized in that include: current collector; as well as A self-supporting film, arranged on the surface of the current collector, wherein the surface of the self-supporting film is provided with a plurality of laser-processed channels, and the laser-processed channels are arranged to extend in a lateral direction of the self-supporting film; The width of the laser processed channel ranges from 0.1 mm to 1 mm; The depth of the laser processed trench ranges from 10 μm to 10 mm.