Porous current collector and preparation method thereof, negative electrode sheet and battery

By using porous current collectors in the battery and using copper powder and zinc powder to construct a double gradient distribution of pore size and porosity, the problem of poor electrochemical performance caused by thick electrode plates is solved, and the rate performance and stability of the battery are significantly improved.

CN118763231BActive Publication Date: 2024-11-19JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411205979.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-19
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

In the process of increasing the energy density of existing batteries, thick electrode plates lead to low fast charging capacity and poor electrochemical performance. The widely used current collector materials lack pore structure, which limits the transmission of active ions and leads to poor rate performance.

Method used

Using a porous current collector, the first and second porous structural layers are arranged by laminating the material, including copper powder and zinc powder, to form a double gradient distribution of pore size and porosity, and to construct a capillary structure to improve the permeability of the electrolyte and active ions. And the bonding force is enhanced by heat treatment.

Benefits of technology

It significantly improves the rate performance of the battery and the stability of the electrode sheet, prevents powder loss, and improves the liquid retention capacity of the battery and the transmission efficiency of active ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763231B_ABST
    Figure CN118763231B_ABST
Patent Text Reader

Abstract

The embodiment of the present application relates to a porous current collector and a preparation method thereof, a negative electrode plate and a battery, wherein the porous current collector comprises: a first porous structure layer and a second porous structure layer which are stacked, wherein the materials of the first porous structure layer and the second porous structure layer both comprise copper powder, zinc powder and polyvinylidene fluoride; the pore size of the first porous structure layer is larger than the pore size of the second porous structure layer, and the porosity of the first porous structure layer is smaller than the porosity of the second porous structure layer. In this way, the rate performance of the battery can be significantly improved, and the bonding force between the porous current collector and the active material layer in the electrode plate can be greatly improved, thereby ensuring the stability of the electrode plate during the battery cycle and preventing the occurrence of powder falling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a porous current collector and a preparation method thereof, a negative electrode sheet and a battery. Background Art

[0002] For secondary batteries, in order to obtain higher energy density, a major technical means is to coat a thicker active material layer on the current collector to form a thick electrode plate, and to increase the energy density by increasing the load of active material per unit volume. Although this method can improve the energy density of the battery, it brings new challenges to the electrochemical performance of the battery. Because when the thickness of the active material layer in the electrode plate is too thick, the fast charging capability of the battery is low, the internal polarization of the battery cell increases, the diffusion path of active ions (such as lithium ions or sodium ions) and electrons increases, and the electrolyte has difficulty in infiltrating the active material layer, which will lead to poor rate performance of the battery. More importantly, the widely used current collector materials, such as aluminum foil or copper foil, do not have a porous structure, and the electrolyte is often difficult to penetrate directly, which limits the transmission of active ions between electrodes to only one side of the current collector, thereby further limiting the rate performance of thick electrode plates. Summary of the invention

[0003] In view of this, the embodiments of the present application provide a porous current collector and a preparation method thereof, a negative electrode plate and a battery to solve at least one problem existing in the background technology.

[0004] In a first aspect, an embodiment of the present application provides a porous current collector, comprising:

[0005] A first porous structure layer and a second porous structure layer are stacked, wherein the materials of the first porous structure layer and the second porous structure layer both include copper powder, zinc powder and polyvinylidene fluoride;

[0006] The pore size of the first porous structure layer is larger than the pore size of the second porous structure layer, and the porosity of the first porous structure layer is smaller than the porosity of the second porous structure layer.

[0007] In conjunction with the first aspect of the present application, in an optional embodiment, the porous current collector satisfies at least one of the following features (1) to (6):

[0008] (1) The pore size of the first porous structure layer is 2 μm to 5 μm;

[0009] (2) The pore size of the second porous structure layer is less than 2 μm;

[0010] (3) The porosity of the first porous structure layer is 10% to 20%;

[0011] (4) The porosity of the second porous structure layer is 25% to 35%;

[0012] (5) The thickness of the first porous structure layer is 10 μm to 20 μm;

[0013] (6) The thickness of the second porous structure layer is 5 μm to 10 μm.

[0014] In a second aspect, an embodiment of the present application provides a method for preparing a porous current collector, the method comprising the following steps:

[0015] S1: dissolving a first copper powder, a first zinc powder and a polyvinylidene fluoride powder in a first solvent, and mixing them uniformly to obtain a first mixture;

[0016] S2: coating the first mixture on a carrier and performing drying treatment to obtain a first porous structure layer;

[0017] S3: dissolving a second copper powder, a second zinc powder and a polyvinylidene fluoride powder in a second solvent, and mixing them uniformly to obtain a second mixture; the particle size of the first copper powder and the first zinc powder is different from the particle size of the second copper powder and the second zinc powder;

[0018] S4: coating the second mixture on the first porous structure layer and performing drying treatment to obtain a second porous structure layer stacked on the first porous structure layer; the pore size of the first porous structure layer is larger than the pore size of the second porous structure layer, and the porosity of the first porous structure layer is smaller than the porosity of the second porous structure layer.

[0019] In conjunction with the second aspect of the present application, in an optional implementation manner, step S1 satisfies at least one of the following features (1) to (3):

[0020] (1) The mass ratio of the first copper powder, the first zinc powder and the polyvinylidene fluoride powder is (80-90): (10-20): 0.1;

[0021] (2) The particle size of the first copper powder and the first zinc powder is 2 μm to 5 μm;

[0022] (3) The first solvent includes at least one of N-methylpyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide.

[0023] In conjunction with the second aspect of the present application, in an optional implementation manner, step S2 satisfies at least one of the following features (1) to (6):

[0024] (1) The coating thickness of the first mixture is 10 μm to 20 μm;

[0025] (2) The coating process of the first mixture is spraying;

[0026] (3) The drying process is vacuum drying at a temperature of 80°C to 100°C;

[0027] (4) The carrier comprises a quartz plate;

[0028] (5) The pore size of the first porous structure layer is 2 μm to 5 μm;

[0029] (6) The porosity of the first porous structure layer is 10% to 20%.

[0030] In conjunction with the second aspect of the present application, in an optional implementation manner, step S3 satisfies at least one of the following features (1) to (3):

[0031] (1) The mass ratio of the second copper powder, the second zinc powder and the polyvinylidene fluoride powder is (80-90): (10-20): 0.1;

[0032] (2) The particle size of the second copper powder and the second zinc powder is 1 μm to 2 μm;

[0033] (3) The second solvent includes at least one of N-methylpyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide.

[0034] In conjunction with the second aspect of the present application, in an optional implementation manner, step S4 satisfies at least one of the following features (1) to (4):

[0035] (1) The coating thickness of the second mixture is 5 μm to 10 μm;

[0036] (2) The second mixture is applied by spraying;

[0037] (3) The pore size of the second porous structure layer is less than 2 μm;

[0038] (4) The porosity of the second porous structure layer is 25% to 35%.

[0039] In conjunction with the second aspect of the present application, in an optional implementation manner, the method further includes:

[0040] Place a pressing plate on the second porous structure layer, perform heat treatment on the first porous structure layer and the second porous structure layer under a protective gas atmosphere, take out the first porous structure layer and the second porous structure layer after cooling, wash and dry them; wherein the heat treatment has at least one of the following characteristics: a) the protective gas includes a reducing gas or includes a reducing gas and an inert gas; b) the temperature of the heat treatment is 400°C~500°C; c) the insulation time of the heat treatment is 2h~4h; d) the heating rate of the heat treatment is 5°C / min~10°C / min.

[0041] In a third aspect, an embodiment of the present application provides a negative electrode plate, which includes a porous current collector as described in any one of the first aspects or a porous current collector prepared by the preparation method as described in any one of the second aspects.

[0042] In a fourth aspect, an embodiment of the present application provides a battery, comprising the negative electrode plate as described in the third aspect.

[0043] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0044] The porous current collector and its preparation method, negative electrode plate and battery provided in the embodiment of the present application, the porous current collector includes: a first porous structure layer and a second porous structure layer arranged in a stacked manner, the materials of the first porous structure layer and the second porous structure layer both include copper and zinc; the pore size of the first porous structure layer is larger than the pore size of the second porous structure layer, and the porosity of the first porous structure layer is smaller than the porosity of the second porous structure layer. A double gradient distribution of pore size and porosity is formed by the first porous structure layer and the second porous structure layer, and a capillary structure is constructed in the porous current collector, so that the electrolyte can quickly penetrate into the active material layer through the porous current collector through capillary action, effectively improving the battery's liquid retention capacity, and the gradient distribution of pore size and porosity structure in the porous current collector can further induce the rapid passage of active ions, and the porous current collector allows the active ions to be transmitted through the porous current collector, which can shorten the distance of the active ions to the active material layer by half, thereby significantly improving the battery's rate performance. In addition, the porous current collector has a three-dimensional porous structure, which can greatly enhance the bonding strength between the porous current collector and the active material layer in the electrode plate, thereby ensuring the stability of the electrode plate during the battery cycle and preventing powder loss.

[0045] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0047] Figure 1 A schematic diagram of the cross-sectional structure of a porous current collector provided in an embodiment of the present application;

[0048] Figure 2 A schematic diagram of a process for preparing a porous current collector provided in an embodiment of the present application;

[0049] Figure 3 A schematic diagram of the cross-sectional structure of a negative electrode plate provided in an embodiment of the present application. DETAILED DESCRIPTION

[0050] In order to make the technical scheme and beneficial effects of the present invention more obvious and easy to understand, the following is described in detail by combining the accompanying drawings and listing specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on conventional experimental conditions. The reagents and raw materials used in the present invention are commercially available unless otherwise specified.

[0051] In the following description, a large number of specific details are given to provide a more thorough understanding of the present application. However, it is obvious to those skilled in the art that the present application can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present application, some technical features known in the art are not described; that is, all features of the actual embodiments are not described here, and well-known functions and steps are not described in detail.

[0052] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be limiting of the present application. When used herein, the singular forms "one", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0053] In order to thoroughly understand the present application, detailed steps and detailed structures will be presented in the following description to illustrate the technical solution of the present application. The preferred embodiments of the present application are described in detail below, but in addition to these detailed descriptions, the present application may also have other implementation methods.

[0054] Unless otherwise defined, technical and scientific terms used in this application have the same meanings as those in the technical field to which this application belongs.

[0055] If no specific techniques or conditions are specified in the following examples, the conventional techniques or conditions described in the literature in the art, or the conditions recommended by the product instructions and the manufacturer are generally used. The numerical ranges in the following examples all include the endpoint values.

[0056] In the related art, in order to improve the energy density of the battery, a thick active material layer is usually coated on the current collector to form a thick electrode plate. Since the thick electrode plate easily increases the diffusion path of active ions and electrons and makes it difficult for the electrolyte to infiltrate, the rate performance of the battery is poor. At present, porous current collectors are used in electrode plates to improve the above problems, because the porous current collector has a porous structure that allows active ions to pass through the current collector and the diaphragm at the same time, shortening the distance for the active ions to be transmitted to the active material layer, which can improve the rate performance. At the same time, the porous structure can improve the battery's liquid retention capacity and ensure that the electrolyte and the active material layer are in full contact during the battery cycle. However, as the thickness of the active material layer coated on the porous current collector increases, the effect of the currently used porous current collector on improving the above problems is still relatively limited.

[0057] Based on this, the present application embodiment provides a porous current collector. Figure 1 The porous current collector 100 includes: a first porous structure layer 101 and a second porous structure layer 102 which are stacked, and the materials of the first porous structure layer 101 and the second porous structure layer 102 both include copper powder, zinc powder and polyvinylidene fluoride; the pore size of the first porous structure layer 101 is larger than the pore size of the second porous structure layer 102, and the porosity of the first porous structure layer 101 is smaller than the porosity of the second porous structure layer 102.

[0058] In the embodiment of the present application, a dual gradient distribution of pore size and porosity is formed by the first porous structure layer 101 and the second porous structure layer 102, and a capillary structure is constructed in the porous current collector 100, so that the electrolyte can quickly penetrate into the active material layer through the porous current collector 100 through capillary action, effectively improving the battery's liquid retention capacity, and the gradient distribution of pore size and porosity structure in the porous current collector 100 can further induce active ions (such as lithium ions or sodium ions) to pass quickly, and the porous current collector 100 allows the active ions to be transmitted through the porous current collector 100, which can shorten the distance of the active ions to the active material layer by half, thereby significantly improving the battery's rate performance. At the same time, because the zinc element in the materials of the first porous structure layer 101 and the second porous structure layer 102 has lithium affinity, in lithium-ion batteries, it can further induce lithium ions to quickly pass through the porous current collector 100, thereby further improving the rate performance. In addition, the porous current collector 100 has a three-dimensional porous structure, which can greatly enhance the bonding force between the porous current collector 100 and the active material layer in the electrode plate, thereby ensuring the stability of the electrode plate during battery cycling and preventing powder loss.

[0059] It should be noted that the materials of the first porous structure layer 101 and the second porous structure layer 102 are both composite metal materials composed of copper and zinc. In actual preparation, the first porous structure layer 101 and the second porous structure layer 102 can be prepared by copper powder and zinc powder, for example.

[0060] In some embodiments, the pore size of the first porous structure layer 101 of the porous current collector 100 may be 2 μm to 5 μm. Controlling the pore size of the first porous structure layer 101 within the above range can make it easier to construct a capillary structure in the porous current collector 100, so as to further accelerate the penetration of the electrolyte and the transmission of active ions, thereby further improving the rate performance of the battery.

[0061] In some embodiments, the pore size of the second porous structure layer 102 may be less than 2 μm. Controlling the pore size of the second porous structure layer 102 within the above range can make it easier to construct a capillary structure in the porous current collector 100 to further accelerate the penetration of the electrolyte and the transmission of active ions, thereby further improving the rate performance of the battery.

[0062] In some embodiments, the porosity of the first porous structure layer 101 may be 10% to 20%. Controlling the porosity of the first porous structure layer 101 within the above range can make it easier to construct a capillary structure in the porous current collector 100, so as to further accelerate the penetration of the electrolyte and the transmission of active ions, and enhance the electrolyte retention capacity of the porous current collector 100, thereby further improving the rate performance of the battery.

[0063] In some embodiments, the porosity of the second porous structure layer 102 may be 25% to 35%. Controlling the porosity of the second porous structure layer 102 within the above range can make it easier to construct a capillary structure in the porous current collector 100, so as to further accelerate the penetration of the electrolyte and the transmission of active ions, and enhance the electrolyte retention capacity of the porous current collector 100, thereby further improving the rate performance of the battery.

[0064] It can be understood that for the four parameter ranges of the pore size of the first porous structure layer 101 being 2 μm to 5 μm, the pore size of the second porous structure layer 102 being less than 2 μm, the porosity of the first porous structure layer 101 being 10% to 20%, and the porosity of the second porous structure layer 102 being 25% to 35%, the first porous structure layer 101 and / or the second porous structure layer 102 of the porous current collector 100 in the embodiment of the present application satisfying any one of the parameter ranges can better improve the rate performance of the battery. Of course, if If the first porous structure layer 101 and / or the second porous structure layer 102 of the porous current collector 100 satisfy any two, any three or four of the above four parameter ranges, the rate performance of the battery can be more significantly improved, and the more parameter ranges are satisfied, the better the performance of the porous current collector 100. When the first porous structure layer 101 and the second porous structure layer 102 of the porous current collector 100 satisfy the above four parameter ranges at the same time, the effect of improving the rate performance of the battery can be optimized.

[0065] For example, the pore size of the first porous structure layer 101 can be controlled within the range of 2 μm to 5 μm, while the pore size of the second porous structure layer 102 can be controlled within the range of less than 2 μm; or the pore size of the first porous structure layer 101 can be controlled within the range of 2 μm to 5 μm, while the porosity of the first porous structure layer 101 can be controlled within the range of 10% to 20%; or the porosity of the first porous structure layer 101 can be controlled within the range of 10% to 20%, while the porosity of the second porous structure layer 102 can be controlled within the range of 25% to 35%; or the pore size of the second porous structure layer 102 can be controlled within the range of less than 2 μm, while the porosity of the second porous structure layer 102 can be controlled within the range of 25% to 35%; or the pore size of the first porous structure layer 101 can be controlled within the range of 2 μm to 5 μm, and the porosity can be controlled within the range of 10% to 20%, while the pore size of the second porous structure layer 102 can be controlled within the range of less than 2 μm. 2μm; or the pore size of the first porous structure layer 101 is controlled within 2μm~5μm, the porosity is controlled within 10%~20%, and the porosity of the second porous structure layer 102 is controlled within 25%~35%; or the pore size of the first porous structure layer 101 is controlled within 2μm~5μm, and the pore size of the second porous structure layer 102 is controlled within less than 2μm, and the porosity is controlled within 25%~35%; or While the porosity of the first porous structure layer 101 is controlled at 10%~20%, the pore size of the second porous structure layer 102 is controlled to be less than 2μm and the porosity is controlled to be 25%~35%; or while the pore size of the first porous structure layer 101 is controlled to be 2μm~5μm and the porosity is controlled to be 10%~20%, the pore size of the second porous structure layer 102 is controlled to be less than 2μm and the porosity is controlled to be 25%~35%.

[0066] In some embodiments, the thickness of the first porous structure layer 101 may be 10 μm to 20 μm. Controlling the thickness of the first porous structure layer 101 within the above range can effectively improve the energy density of the battery while allowing the electrolyte to fully penetrate into the porous current collector 100, and maintain a sufficient amount of electrolyte, and control the transmission path of active ions within a suitable range, thereby ensuring the rate performance of the battery.

[0067] In some embodiments, the thickness of the second porous structure layer 102 may be 5 μm to 10 μm. Controlling the thickness of the second porous structure layer 102 within the above range can effectively improve the energy density of the battery while allowing the electrolyte to fully penetrate into the porous current collector 100, and maintain a sufficient amount of electrolyte, and control the transmission path of active ions within a suitable range, thereby ensuring the rate performance of the battery.

[0068] Based on this, the present application also provides a method for preparing a porous current collector. Figure 2The method for preparing the porous current collector provided in the embodiment of the present application comprises the following steps:

[0069] S1: dissolving a first copper powder, a first zinc powder and a polyvinylidene fluoride powder in a first solvent, and mixing them uniformly to obtain a first mixture;

[0070] S2: coating the first mixture on a carrier and performing drying treatment to obtain a first porous structure layer;

[0071] S3: dissolving the second copper powder, the second zinc powder and the polyvinylidene fluoride powder in a second solvent, and mixing them uniformly to obtain a second mixture; the particle size of the first copper powder and the first zinc powder is different from the particle size of the second copper powder and the second zinc powder;

[0072] S4: coating the second mixture on the first porous structure layer and drying it to obtain a second porous structure layer stacked on the first porous structure layer; the pore size of the first porous structure layer is larger than the pore size of the second porous structure layer, and the porosity of the first porous structure layer is smaller than the porosity of the second porous structure layer.

[0073] In the embodiment of the present application, a first porous structure layer is formed by a first mixture including a first copper powder and a first zinc powder, and a second porous structure layer is formed by a second mixture including a second copper powder and a second zinc powder. The copper powder and the zinc powder are stacked on each other under the action of a binder, polyvinylidene fluoride, and the pores formed between the particles constitute the pores in the first porous structure layer and the second porous structure layer. Since the particle size of the first copper powder and the first zinc powder is different from the particle size of the second copper powder and the second zinc powder, the pore size and porosity of the first porous structure layer and the second porous structure layer are different. At the same stacking density, the porous structure layer formed by the copper powder and the zinc powder with relatively larger particle size has a larger pore size and a lower porosity. The porous structure layer formed by the copper powder and zinc powder with relatively small particle size has a small pore size and a high porosity. In this way, by forming a dual gradient distribution of pore size and porosity in the first porous structure layer and the second porous structure layer, a capillary structure is constructed in the porous current collector, so that the electrolyte can quickly penetrate into the active material layer through the porous current collector through capillary action, effectively improving the battery's liquid retention capacity. The gradient distribution of pore size and porosity structure in the porous current collector can further induce the rapid passage of active ions, and the porous current collector allows the active ions to be transmitted through the porous current collector, which can shorten the distance of the active ions to the active material layer by half, so that the battery's rate performance can be significantly improved. At the same time, because the zinc element in the materials of the first porous structure layer and the second porous structure layer has lithium affinity, in lithium-ion batteries, it can further induce lithium ions to quickly pass through the porous current collector, thereby further improving the rate performance. In addition, the porous current collector has a three-dimensional porous structure, which can greatly enhance the bonding strength between the porous current collector and the active material layer in the electrode plate, ensure the stability of the electrode plate during battery cycling, and prevent powder loss.

[0074] In the above step S1, the mass ratio of the first copper powder, the first zinc powder and the polyvinylidene fluoride powder can be (80-90):(10-20):0.1, for example, it can be (80:20:0.1), (85:15:0.1), (90:10:0.1) or any other mass ratio within the above range.

[0075] In the embodiments of the present application, polyvinylidene fluoride powder can be used as a binder to enable the first copper powder and the first zinc powder to better form a first porous structure layer. Controlling the mass ratio of the first copper powder, the first zinc powder and the polyvinylidene fluoride powder within the above range can form a first porous structure layer with better quality and ensure that the first porous structure layer has better conductive properties.

[0076] In some specific embodiments, the particle size of the first copper powder and the first zinc powder can be 2μm~5μm, for example, 2μm, 3μm, 4μm, 5μm or any value between any two of the above numerical ranges. The particle sizes of the first copper powder and the first zinc powder can be the same or different. The pore size and porosity of the first porous structure layer can be controlled by controlling the particle sizes of the first copper powder and the first zinc powder. By controlling the particle sizes of the first copper powder and the first zinc powder within the above range, the pore size of the formed first porous structure layer can be 2μm~5μm and / or the porosity of the first porous structure layer can be 10%~20%. This makes it easier to construct a capillary structure in the porous current collector to further accelerate the penetration of the electrolyte and the transmission of active ions, thereby further improving the rate performance of the battery. In some more specific embodiments, the first copper powder and the first zinc powder have the same particle size, and it is easier to form suitable pore sizes and pores between the first copper powder and the first zinc powder with the same particle size, so that the pore size and pores of the formed first porous structure layer are better controllable, thereby facilitating the construction of a better capillary structure in the porous current collector.

[0077] The type of the first solvent in step S1 is not particularly limited, as long as it is a highly polar solvent that can dissolve polyvinylidene fluoride.

[0078] For example, the first solvent may include at least one of N-methylpyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide.

[0079] In the above step S2, the thickness of the first mixture coating can be 10 μm to 20 μm, for example, 10 μm, 12 μm, 15 μm, 17 μm, 18 μm, 20 μm or any value between any two of the above numerical ranges. By controlling the thickness of the first mixture coating within the above range, the thickness of the first porous structure layer formed can be controlled within 10 μm to 20 μm, so that while improving the energy density of the battery, the electrolyte can be fully infiltrated into the porous current collector, and a sufficient amount of electrolyte can be maintained, and the transmission path of the active ions can be controlled within a suitable range, thereby ensuring the rate performance of the battery.

[0080] In step S2, the coating process of the first mixture may include at least one of spray coating, scraper coating, roller coating, etc. In a specific embodiment, the coating process of the first mixture may be spray coating, so that the formed first porous structure layer can be smoother, more uniform in thickness, and the overall quality of the first porous structure layer is higher.

[0081] There is no particular limitation on the carrier in step S2 as long as it has a relatively flat surface.

[0082] Exemplarily, the carrier may include a quartz plate, the surface of which is flat and smooth, which facilitates uniform adhesion of the first mixture on the one hand, and enables the formed first porous structure layer to have a flatter and more uniform structure, and the quality of the first porous structure layer is higher on the other hand.

[0083] The drying process in step S2 can be vacuum drying, and the drying temperature can be 80°C to 100°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C or any value between any two of the above ranges. Drying under vacuum can protect the copper powder and the zinc powder from being oxidized, etc., and controlling the drying temperature within the above range can form a first porous structure layer with better quality.

[0084] In actual preparation, the first mixture can be first placed in a spraying device, then coated on a smooth quartz plate by spraying, and then placed in a vacuum oven for drying, thereby obtaining a first porous structure layer.

[0085] In the above step S3, the mass ratio of the second copper powder, the second zinc powder and the polyvinylidene fluoride powder can be (80-90): (10-20): 0.1, for example, it can be (80:20:0.1), (85:15:0.1), (90:10:0.1) or any other mass ratio within the above range.

[0086] In the embodiments of the present application, polyvinylidene fluoride powder can be used as a binder to enable the second copper powder and the second zinc powder to better form a second porous structure layer. Controlling the mass ratio of the second copper powder, the second zinc powder and the polyvinylidene fluoride powder within the above range can form a second porous structure layer with better quality and ensure that the second porous structure layer has better conductive properties.

[0087] In some specific embodiments, the particle size of the second copper powder and the second zinc powder can be 1 μm to 2 μm, for example, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2 μm or any value between any two of the above numerical ranges. The particle size of the second copper powder and the second zinc powder can be the same or different. The pore size and porosity of the second porous structure layer can be controlled by controlling the particle size of the second copper powder and the second zinc powder. By controlling the particle size of the second copper powder and the second zinc powder within the above range, the pore size of the formed second porous structure layer can be less than 2 μm and / or the porosity of the second porous structure layer can be 25% to 35%. In this way, it is easier to construct a capillary structure in the porous current collector to further accelerate the penetration of the electrolyte and the transmission of active ions, thereby further improving the rate performance of the battery. In some more specific embodiments, the second copper powder and the second zinc powder have the same particle size, and it is easier to form suitable pore sizes and pores between the second copper powder and the second zinc powder with the same particle size, so that the pore size and pores of the formed second porous structure layer are better controllable, thereby facilitating the construction of a better capillary structure in the porous current collector.

[0088] The type of the second solvent in step S3 is not particularly limited, as long as it is a highly polar solvent that can dissolve polyvinylidene fluoride.

[0089] For example, the second solvent may include at least one of N-methylpyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide.

[0090] In the above step S4, the thickness of the second mixture coating can be 5μm~10μm, for example, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm or any value between any two of the above numerical ranges. Controlling the thickness of the second mixture coating within the above range can control the thickness of the formed second porous structure layer to 5μm~10μm, so that the energy density of the battery can be effectively improved while allowing the electrolyte to fully penetrate into the porous current collector, and maintaining a sufficient amount of electrolyte, and controlling the transmission path of the active ions within a suitable range, thereby ensuring the rate performance of the battery.

[0091] In step S4, the coating process of the second mixture may include at least one of spraying, scraping, rolling, etc. In a specific embodiment, the coating process of the second mixture may be spraying, so that the formed second porous structure layer can be smoother, more uniform in thickness, and higher in overall quality.

[0092] In actual preparation, the second mixture can be first placed in a spraying device, then coated on the first porous structure layer by spraying, and dried to obtain a second porous structure layer stacked on the first porous structure layer. The first porous structure layer and the second porous structure layer together constitute a porous current collector.

[0093] The specific process of the drying treatment in step S4 can be understood by referring to the process of the drying treatment in the above step S2, and will not be repeated here.

[0094] In some embodiments, the method for preparing the porous current collector may also include: placing a pressing plate on the second porous structure layer, heat treating the first porous structure layer and the second porous structure layer under a protective gas atmosphere, and after cooling, taking out the first porous structure layer and the second porous structure layer, washing and drying them.

[0095] In the embodiment of the present application, placing the pressing plate on the second porous structure layer can make the finally formed porous current collector have a smoother surface and uniform thickness, thereby improving the quality of the porous current collector and enhancing the practicality of the porous current collector; heat treating the first porous structure layer and the second porous structure layer can enhance the binding effect of the particles in the first porous structure layer and the second porous structure layer, reduce the stress inside the first porous structure layer and the second porous structure layer and between the first porous structure layer and the second porous structure layer, and enhance the strength of the porous current collector, thereby obtaining a higher quality porous current collector; washing and drying the first porous structure layer and the second porous structure layer (porous current collector) after cooling can remove impurities on the surface of the porous current collector, thereby further improving the quality of the porous current collector, which is beneficial to further improve the rate performance of the battery.

[0096] For example, the press plate may be a quartz plate, because the quartz plate has a smooth and flat surface, which can make the processed porous current collector have a more flat surface.

[0097] In some specific embodiments, the protective gas may include a reducing gas or a reducing gas and an inert gas. For example, the protective gas may be H2 or CO, or the protective gas may be a mixed gas of H2 and Ar, etc. In this way, the porous current collector can be protected from oxidation during heat treatment, thereby avoiding adverse effects on the performance of the porous current collector.

[0098] In actual preparation, first, a smooth quartz plate can be placed on the second porous structure layer without applying external force, and then the porous current collector is placed in a tubular furnace, and a protective gas is introduced. After being kept at a set temperature for a set time, the porous current collector is taken out, and then the taken out porous current collector is naturally cooled and washed with ethanol and deionized water.

[0099] Placing a smooth quartz plate on the second porous structure layer without applying external force can avoid deformation of the porous current collector, especially uneven deformation, caused by applying a large external force or an uneven external force, thereby ensuring that the performance of the porous current collector is not affected.

[0100] It can be understood that when the temperature of the heat treatment is low, it is not possible to improve the bonding effect of the particles in the first porous structure layer and the second porous structure layer, reduce the stress inside the first porous structure layer and the second porous structure layer, and between the first porous structure layer and the second porous structure layer. When the temperature of the heat treatment is high, it is easy to over-treat the first porous structure layer and the second porous structure layer, resulting in uncontrollable changes in the pore size and porosity of the first porous structure layer and the second porous structure layer, thereby affecting the performance of the porous current collector. Therefore, in some specific embodiments, the temperature of the heat treatment can be 400°C to 500°C, for example, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C or any value between any two of the above numerical ranges. In this way, a high-quality porous current collector can be prepared, thereby better improving the electrochemical performance of the battery.

[0101] The holding time of the heat treatment is closely related to the effect of the heat treatment. Therefore, in some embodiments, the holding time of the heat treatment can be 2h~4h, for example, 2h, 2.5h, 3h, 3.5h, 4h or any value between any two of the above ranges. Controlling the holding time within the above range can further improve the quality of the prepared porous current collector.

[0102] The heating rate of the heat treatment is closely related to the effect of the heat treatment. Therefore, in some embodiments, the heating rate of the heat treatment can be 5°C / min to 10°C / min, for example, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min or any value between any two of the above ranges. Controlling the heating rate within the above range can further improve the quality of the prepared porous current collector.

[0103] Based on this, the embodiment of the present application also provides a negative electrode sheet, such as Figure 3 As shown, the negative electrode plate 200 includes the porous current collector 100 described in any of the above embodiments or includes a porous current collector prepared by the method for preparing the porous current collector described in any of the above embodiments.

[0104] It should be understood that since the negative electrode plate 200 in the embodiment of the present application includes the porous current collector 100 described in any of the above embodiments or includes a porous current collector prepared by the preparation method of the porous current collector described in any of the above embodiments, the beneficial effects of the porous current collector 100 described in any of the above embodiments are applicable to the negative electrode plate 200.

[0105] In some embodiments, Figure 3 As shown, the negative electrode sheet 200 may include a porous current collector 100 and a negative electrode active material layer 201 disposed on at least one surface of the porous current collector 100. As an example, the porous current collector 100 has two surfaces opposite to each other in its own thickness direction, and the negative electrode active material layer 201 is disposed on any one or both of the two opposite surfaces of the porous current collector 100. Figure 3 The negative electrode active material layer 201 is shown as being disposed on one surface of the porous current collector 100. When the negative electrode active material layer 201 is disposed on one surface of the porous current collector 100, it is a better solution to dispose the negative electrode active material layer 201 on the surface of the second porous structure layer 102, that is, to dispose the negative electrode active material layer 201 on the surface of the porous structure layer with a smaller pore size, so that the electrolyte can pass through the porous current collector 100 more quickly, thereby accelerating the infiltration of the negative electrode active material layer 201. Of course, the embodiment of the present application does not exclude the case where the negative electrode active material layer 201 is disposed on the surface of the first porous structure layer 101.

[0106] The preparation method of the negative electrode sheet 200 may include: first, mixing the negative electrode active material, conductive carbon, binder and thickener in deionized water to obtain a negative electrode slurry, wherein the mass fraction of the negative electrode active material can be 96.7%~98.2%, the mass fraction of the conductive carbon can be 0%~1%, the mass fraction of the binder can be 1%~1.5%, and the mass fraction of the thickener can be 0.5%~0.8%, and then the negative electrode slurry is coated on the porous current collector 100, and the negative electrode sheet 200 is formed by drying and rolling.

[0107] Exemplarily, the negative electrode active material may include at least one of graphite, silicon-based negative electrode material, hard carbon negative electrode material, etc.; the conductive agent may include at least one of carbon black, carbon nanotubes, carbon fiber, graphene, etc.; the binder may include styrene-butadiene rubber and / or polyvinylidene fluoride; the thickener may include polyvinylidene fluoride and / or carboxymethyl cellulose.

[0108] Based on this, an embodiment of the present application also provides a battery, comprising the negative electrode plate described in the above embodiment.

[0109] In some embodiments, the battery may be a secondary battery, and the secondary battery may be a lithium-ion secondary battery or a sodium-ion secondary battery. Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery charge and discharge process, active ions are embedded and extracted back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is disposed between the positive electrode sheet and the negative electrode sheet, and mainly plays the role of preventing the positive and negative electrodes from short-circuiting, while allowing ions to pass through.

[0110] The technical solution of the present application is further described below in combination with a plurality of embodiments and comparative examples. Example 1

[0111] The preparation of the porous current collector in this embodiment includes the following steps:

[0112] Step S101: copper powder with a particle size of 5 μm, zinc powder with a particle size of 5 μm, and polyvinylidene fluoride powder are uniformly mixed in N-methylpyrrolidone (NMP) at a mass ratio of 80:20:0.1 to obtain a first mixture;

[0113] Step S102: putting the first mixture obtained in step S101 into a sprayer, preparing a clean and smooth quartz plate, spraying the first mixture on the quartz plate, controlling the spraying thickness to 10 μm, and then putting the quartz plate into a vacuum drying oven at 80° C. to dry, to obtain a first porous structure layer with a thickness of 10 μm;

[0114] Step S103: mixing copper powder with a particle size of 2 μm, zinc powder with a particle size of 2 μm, and polyvinylidene fluoride powder in NMP at a mass ratio of 80:20:0.1 to obtain a second mixture;

[0115] Step S104: putting the second mixture obtained in step S103 into a sprayer, spraying the second mixture on the first porous structure layer, and controlling the spraying thickness to be 5 μm to obtain a second porous structure layer with a thickness of 5 μm;

[0116] Step S105: First, place another smooth quartz plate on the second porous structure layer obtained in step S104 without applying external force. Then, put the sample into a tubular furnace and introduce a mixed gas of Ar and H2. Next, heat it to 450°C at a heating rate of 5°C / min. Take out the sample after heat treatment for 2 hours, cool it naturally, wash it with deionized water and ethanol, and dry it to obtain the final porous current collector. Example 2

[0117] The preparation of the porous current collector in this embodiment is basically the same as that in Embodiment 1, except that the particle size of the copper powder and the zinc powder in step S103 is both 1 μm.

[0118] Comparative Example 1

[0119] The preparation of the porous current collector in this comparative example is basically the same as that in Example 1, except that the particle sizes of the copper powder and the zinc powder in step S101 are both 2 μm.

[0120] Comparative Example 2

[0121] The preparation of the porous current collector in this comparative example is basically the same as that in Example 1, except that the particle size of the copper powder and the zinc powder in step S103 is 5 μm.

[0122] The pore size and porosity of the porous current collectors obtained in the above embodiments and comparative examples were tested:

[0123] The test method is:

[0124] (1) Pore size test: The pore size distribution of the first porous structure layer and the second porous structure layer is measured by the mercury intrusion method. The mercury intrusion amount of the first porous structure layer and the second porous structure layer at each pressure point is measured respectively, so as to obtain the distribution range of the pore size of the first porous structure layer and the second porous structure layer.

[0125] (2) Porosity test: The porosity is tested by the immersion method. Specifically, first, the first porous structure layer is cut into samples of 10 cm × 6 cm in size, and its mass is accurately weighed to 0.00001 g. Then, the cut sample is placed in a container filled with hexadecane and soaked for 60 min to allow the pores in the sample to be filled with hexadecane. Next, the sample is placed between two pieces of oil-absorbing paper and repeatedly squeezed 10 times with a pressure roller, with one round trip as one time. The oil-absorbing paper is replaced 10 times to allow the hexadecane on the surface of the sample to be absorbed as much as possible. The mass of the sample filled with hexadecane is weighed to 0.00001 g. The porosity of the first porous structure layer is calculated using the following formula. P = (M1-M0) / (ρ × L × W × d) × 100%, where P is the porosity of the sample, M1 is the mass of the sample after fully absorbing hexadecane (in g), M0 is the mass of the sample before absorbing hexadecane (in g), and ρ is the density of hexadecane (in g / cm 3 ); L is the length of the sample (in cm), W is the width of the sample (in cm), and d is the thickness of the sample (in cm). The porosity of the porous current collector is measured using the same method as above, and the porosity of the second porous structure layer is obtained by subtracting the porosity of the first porous structure layer from the porosity of the porous current collector.

[0126] The test results are shown in Table 1.

[0127] Table 1

[0128]

[0129] It can be seen from the results of Example 1 and Example 2 in Table 1 that in the present application, since the particle sizes of the copper powder and zinc powder used to prepare the first porous structure layer are larger than the particle sizes of the copper powder and zinc powder used to prepare the second porous structure layer, the pore size of the obtained first porous structure layer is larger than the pore size of the second porous structure layer, and the porosity of the first porous structure layer is smaller than the porosity of the second porous structure layer. It can be seen from the results of Comparative Examples 1 and Comparative Examples 2 in Table 1 that when the particle sizes of the copper powder and zinc powder used to prepare the first porous structure layer and the particle sizes of the copper powder and zinc powder used to prepare the second porous structure layer are the same, the pore size of the first porous structure layer is slightly different from the pore size of the second porous structure layer, and is basically in the same numerical range, and an pore size gradient cannot be formed, and the pore size of the first porous structure layer is slightly different from the porosity of the second porous structure layer, and is basically in the same numerical range, and a porosity gradient cannot be formed.

[0130] From the above, it can be seen that in the present application, by controlling the particle size of copper powder and zinc powder, the pore size of the first porous structure layer can be made larger than the pore size of the second porous structure layer, and the porosity of the first porous structure layer is smaller than the porosity of the second porous structure layer, so that the obtained porous current collector presents a porous structure with a dual gradient distribution.

[0131] The porous current collectors obtained in the above embodiments and comparative examples are prepared into negative electrode sheets. The preparation method of the negative electrode sheets is as follows: first, artificial graphite, conductive carbon, sodium carboxymethyl cellulose and styrene-butadiene rubber are added to deionized water in a mass fraction ratio of 96.7%: 1%: 0.8%: 1.5% and mixed evenly to obtain negative electrode slurry; secondly, the negative electrode slurry is applied to the porous current collectors prepared in the above embodiments and comparative examples, and placed in an oven for drying to obtain an active material layer composited on the porous current collector; further, the dried sample is roller-pressed to obtain a negative electrode sheet.

[0132] It should be noted that, based on the above-mentioned Comparative Examples 1 and 2, Comparative Example 3 is added when preparing the negative electrode sheet, wherein the current collector in Comparative Example 3 is a non-porous copper foil. In addition, the method for preparing the negative electrode sheet using Comparative Example 3 is the same as the method for preparing the negative electrode sheet using the porous current collector obtained in Example 1 and Example 2 and Comparative Examples 1 and 2.

[0133] The peel strength and film resistance of the prepared negative electrode sheet were tested, and the test results are shown in Table 2.

[0134] In this application, peel strength is a well-known term in the art and can be measured using methods known in the art. For example, the peel strength test can be performed with reference to the standard GB / T2791-1995 method. The sheet resistance of the negative electrode sheet is a well-known term in the art and can be measured using instruments and methods known in the art. For example, several sheets with an area of ​​154.02 mm can be punched out. 2 The negative electrode sheet sample is tested by a diaphragm resistance tester, and the average diaphragm resistance of 10 parallel samples is taken as the diaphragm resistance value of the negative electrode sheet.

[0135] Table 2

[0136]

[0137] It can be seen from the results of Example 1 and Example 2 in Table 2 that the porous current collector prepared in the present application has a three-dimensional porous structure, which can greatly improve the bonding force between the porous current collector and the active material layer in the negative electrode sheet, so that the peel strength of the negative electrode sheet is significantly greater than the peel strength of the negative electrode sheet prepared by the current collector in Comparative Example 3. Although the negative electrode sheet prepared by the porous current collectors prepared in Comparative Examples 1 and 2 also has a three-dimensional porous structure, so that the peel strength of the negative electrode sheet is relatively greater than the peel strength of the negative electrode sheet prepared by the current collector in Comparative Example 3, it can be seen from the results in Table 2 that the membrane resistance of the negative electrode sheet prepared by the porous current collectors prepared in Examples 1 and 2 is less than the membrane resistance of the negative electrode sheet corresponding to Comparative Examples 1 to Comparative Examples 3, especially the membrane resistance of the negative electrode sheet corresponding to Example 1 is significantly smaller, which shows that the porous current collector with a gradient distributed porous structure in the present application has a smaller transmission resistance for active ions, can better promote the rapid transmission of active ions, and improve the rate performance of the battery. The diaphragm resistance of the negative electrode sheet corresponding to Example 2 is slightly larger than the diaphragm resistance of the negative electrode sheet corresponding to Example 1, indicating that the pore size of the second porous structure layer is too small, which weakens the effect of promoting the transport of active ions. Therefore, in the present application, the pore size of the second porous structure layer is between 1μm and 2μm, which is a better solution.

[0138] A lithium-ion battery was prepared and its electrochemical performance was tested. The preparation method of the lithium-ion battery was as follows: the negative electrode sheets prepared by the current collectors of the above-mentioned embodiments and comparative examples were assembled, a lithium metal sheet was used as a counter electrode, glass fiber was used as a separator, and 1 mol / L LiPF6 / DME (i.e., a solution formed by dissolving LiPF6 in ethylene glycol dimethyl ether) was used as the electrolyte to assemble a button-type lithium-ion half-cell. The performance test of the battery was as follows:

[0139] (1) Capacity retention rate test: Discharge to 0V at a constant current density of 1C, let stand for 10 minutes, charge to 2V at 0.5C current, let stand for 10 minutes, and then repeat 10 times in sequence to calculate the 1C capacity retention rate, 1C capacity retention rate = 1C charging capacity / 0.5C charging capacity. Then use the same method to test at 2C and 5C in sequence to obtain the 2C capacity retention rate and 5C capacity retention rate.

[0140] (2) Internal resistance (impedance) test: DC internal resistance ACR test: discharge the battery at a constant current of 0.05C to 0V, let it stand for 10 minutes, and then charge it at a constant current of 0.05C for 10 hours until it reaches 50% SOC (State of Charge). Use a DC internal resistance meter to test the DC internal resistance of the battery.

[0141] (3) Specific capacity test: The test instrument is a blue dot test cabinet, and the test voltage range is 0V-2V. First, discharge to 0V at a constant current of 0.05C, let it stand for 5 minutes, and then charge to 2V at a constant current of 0.1C, let it stand for 2 minutes to obtain the charge specific capacity.

[0142] The test results are shown in Table 3.

[0143] Table 3

[0144]

[0145] From the results of Example 1 and Example 2 in Table 3, it can be seen that compared with the comparative example, the specific capacity of the lithium ion battery comprising the porous current collector in the present application is relatively high, and the capacity retention rate of the lithium ion battery after 10 cycles at current densities of 1C, 2C and 5C is significantly higher than the specific capacity of the lithium ion battery comprising the current collector in the comparative example. The lithium ion battery comprising the porous current collector in the present application exhibits a better capacity retention rate after high rate (5C) cycling, and the electrochemical impedance after cycling is also lower, which shows that the porous current collector in the present application has a significant effect on improving the rate performance of the battery. The capacity retention rate of the lithium ion battery corresponding to Example 2 after cycling at a high rate of 5C is slightly worse than the capacity retention rate of the lithium ion battery corresponding to Example 1 after cycling at a high rate of 5C, indicating that the pore size of the second porous structure layer is too small, which weakens the effect of promoting the transport of active ions. Therefore, the pore size of the second porous structure layer in the present application is between 1μm and 2μm, which is a better solution. In Comparative Examples 1 to 3, since there is no pore structure with a gradient distribution in the current collector, the rate performance of the corresponding prepared batteries is poor, and the electrochemical impedance after cycling at a high rate of 5C is large.

[0146] The process for preparing the porous current collector in the present application is simple, controllable, and easy to operate, and the thickness of the porous current collector can be flexibly adjusted according to the design requirements. The self-supporting dual-gradient porous current collector has a gradient-distributed pore structure inside. The lower layer is a first porous structure layer with a large pore size and a small porosity, and the upper layer is a second porous structure layer with a small pore size and a large porosity. By constructing a capillary structure in the porous current collector, the electrolyte can quickly penetrate into the current collector through capillary action, which helps to improve the liquid retention capacity of the battery cell and ensure that the battery is fully infiltrated with the electrolyte during the cycle. At the same time, the gradient-distributed porous structure in the porous current collector and the lithium affinity of the zinc element can induce the active ions to quickly reach the active material layer, thereby significantly improving the transmission rate of active ions, especially lithium ions, and thus greatly improving the rate performance of the battery. In addition, the three-dimensional porous structure of the porous current collector enhances the bonding force between the active material layer and the porous current collector, which can ensure the stability of the pole piece during the battery cycle and prevent the phenomenon of powder falling.

[0147] It should be noted that the porous current collector embodiment, the porous current collector preparation method embodiment, the negative electrode plate embodiment and the battery embodiment provided in the present application belong to the same concept; the technical features in the technical solutions recorded in each embodiment can be arbitrarily combined without conflict.

[0148] It should be understood that the above embodiments are exemplary and are not intended to include all possible implementations included in the claims. Various modifications and changes may be made on the basis of the above embodiments without departing from the scope of the present disclosure. Similarly, the various technical features of the above embodiments may be arbitrarily combined to form other embodiments of the present invention that may not be explicitly described. Therefore, the above embodiments only express several implementations of the present invention and do not limit the scope of protection of the patent of the present invention.

Claims

1. A porous current collector, characterized in that: include: A first porous structure layer and a second porous structure layer are stacked, wherein the materials of the first porous structure layer and the second porous structure layer both include copper powder, zinc powder and polyvinylidene fluoride; The pore size of the first porous structure layer is larger than the pore size of the second porous structure layer, and the porosity of the first porous structure layer is smaller than the porosity of the second porous structure layer.

2. The porous current collector according to claim 1, characterized in that: The porous current collector satisfies at least one of the following characteristics (1) to (6): (1) The pore size of the first porous structure layer is 2 μm to 5 μm; (2) The pore size of the second porous structure layer is less than 2 μm; (3) The porosity of the first porous structure layer is 10% to 20%; (4) The porosity of the second porous structure layer is 25% to 35%; (5) The thickness of the first porous structure layer is 10 μm to 20 μm; (6) The thickness of the second porous structure layer is 5 μm to 10 μm.

3. A method for preparing a porous current collector, characterized in that: The method comprises the following steps: S1: dissolving a first copper powder, a first zinc powder and a polyvinylidene fluoride powder in a first solvent, and mixing them uniformly to obtain a first mixture; S2: coating the first mixture on a carrier and performing drying treatment to obtain a first porous structure layer; S3: dissolving a second copper powder, a second zinc powder and a polyvinylidene fluoride powder in a second solvent, and mixing them uniformly to obtain a second mixture; the particle size of the first copper powder and the first zinc powder is different from the particle size of the second copper powder and the second zinc powder; S4: coating the second mixture on the first porous structure layer and performing drying treatment to obtain a second porous structure layer stacked on the first porous structure layer; the pore size of the first porous structure layer is larger than the pore size of the second porous structure layer, and the porosity of the first porous structure layer is smaller than the porosity of the second porous structure layer.

4. The method for preparing a porous current collector according to claim 3, characterized in that: Step S1 satisfies at least one of the following characteristics (1) to (3): (1) The mass ratio of the first copper powder, the first zinc powder and the polyvinylidene fluoride powder is (80-90): (10-20): 0.1; (2) The particle size of the first copper powder and the first zinc powder is 2 μm to 5 μm; (3) The first solvent includes at least one of N-methylpyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide.

5. The method for preparing a porous current collector according to claim 3, characterized in that: Step S2 satisfies at least one of the following characteristics (1) to (6): (1) The coating thickness of the first mixture is 10 μm to 20 μm; (2) The coating process of the first mixture is spraying; (3) The drying process is vacuum drying at a temperature of 80°C to 100°C; (4) The carrier comprises a quartz plate; (5) The pore size of the first porous structure layer is 2 μm to 5 μm; (6) The porosity of the first porous structure layer is 10% to 20%.

6. The method for preparing a porous current collector according to claim 3, characterized in that: Step S3 satisfies at least one of the following characteristics (1) to (3): (1) The mass ratio of the second copper powder, the second zinc powder and the polyvinylidene fluoride powder is (80-90): (10-20): 0.1; (2) The particle size of the second copper powder and the second zinc powder is 1 μm to 2 μm; (3) The second solvent includes at least one of N-methylpyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide.

7. The method for preparing a porous current collector according to claim 3, characterized in that: Step S4 satisfies at least one of the following characteristics (1) to (4): (1) The coating thickness of the second mixture is 5 μm to 10 μm; (2) The second mixture is applied by spraying; (3) The pore size of the second porous structure layer is less than 2 μm; (4) The porosity of the second porous structure layer is 25% to 35%.

8. The method for preparing a porous current collector according to any one of claims 3 to 7, characterized in that: The method further comprises: Place a pressing plate on the second porous structure layer, perform heat treatment on the first porous structure layer and the second porous structure layer under a protective gas atmosphere, take out the first porous structure layer and the second porous structure layer after cooling, wash and dry them; wherein the heat treatment has at least one of the following characteristics: a) the protective gas includes a reducing gas or includes a reducing gas and an inert gas; b) the temperature of the heat treatment is 400°C~500°C; c) the insulation time of the heat treatment is 2h~4h; d) the heating rate of the heat treatment is 5°C / min~10°C / min.

9. A negative electrode plate, characterized in that: The negative electrode plate comprises the porous current collector according to claim 1 or 2, or comprises the porous current collector prepared by the preparation method according to any one of claims 3 to 8.

10. A battery, characterized in that: Including the negative electrode sheet as described in claim 9.