Method for producing component from semi-finished product of nickel-chromium-aluminum alloy

Through high-temperature annealing treatment and element optimization of nickel-chromium-aluminum alloy, the problem of insufficient corrosion resistance and creep strength of nickel-chromium-aluminum alloy under high temperature conditions is solved, the creep strength and ductility of the weld are improved, and the It improves the resistance to 'metal powdering' and extends the service life of the equipment.

CN118765334APending Publication Date: 2024-10-11VDM METALS INTERNATIONAL GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024021.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-10
Filing Date
2023-03-03
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing nickel-chromium-aluminum forgeable alloys have problems with insufficient corrosion resistance and creep strength under high temperature conditions, especially in 'metal powdering' environments, and the creep strength and ductility of the welds are poor, affecting Equipment longevity and safety.

Method used

The semi-finished product manufacturing method of nickel-chromium-aluminum alloy is adopted, and the microstructure of the alloy is optimized to improve creep strength and ductility by performing annealing treatment at high temperature, including homogenization annealing and cooling of the weld seam, combined with solid solution annealing technology, and Phase stability is enhanced by adjusting element content to meet specific Fp relationships.

Benefits of technology

Significantly improves the corrosion resistance and creep strength of nickel-chromium-aluminum alloy at high temperatures, extends the service life of equipment, improves the creep strength and ductility of welds, and enhances resistance to 'metal powdering' .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765334A_ABST
    Figure CN118765334A_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a component partially or completely made of a semi-finished product of a nickel-chromium-aluminum malleable alloy, the invention relates to a nickel-chromium-aluminum malleable alloy having (in mass%) more than 18 to 33% chromium, 1.8 to 4.0% aluminum, 0.01 to 7.0% iron, 0.001 to 0.50% silicon, 0.001 to 2.0% manganese, 0.00 to 0.60% titanium, respectively 0.0 to 0.05% magnesium and / or calcium, 0.005 to 0.12% carbon, 0.0005 to 0.050% nitrogen, 0.0001 to 0.020% oxygen, 0.001 to 0.030% phosphorus, maximum 0.010% sulfur, maximum 2.0% molybdenum, maximum 2.0% tungsten, and the balance of nickel and unavoidable impurities. The invention relates to a method for producing a component, comprising the following steps: (1) welding the component, in which the component contains a weld of the same kind and / or the component has a weld of the same kind during the installation of the equipment, and after the welding, only the weld of the same kind and the heat-affected zone are subjected to an annealing for 0.05 minutes to 24 hours between 980 DEG C and 1250 DEG C, and after the welding, the component contains a weld of the same kind and / or the weld of the same kind and the heat-affected zone is subjected to an annealing for 0.05 minutes to 24 hours. The invention relates to an annealing method for a weld seam for homogenization of the weld seam and / or for reduction of stress, followed by cooling in a stationary protective gas or air, a moving (blown) protective gas or air, with the result that the creep strength and creep ductility of the weld seam are improved by such annealing, in which the following relationships must be satisfied: (1a) Cr + Al > = 28 and (2a) Fp < = 39.9, where (3a) Fp = Cr + 0.272 * Fe + 2.36 * Al + 2.22 * Si + 2.48 * Ti + 0.374 * Mo + 0.538 * W-11.8 * C, wherein Cr, Fe, Al, Si, Ti, Mo, W and C are the concentrations of the related elements in mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a component from a semi-finished product of a nickel-chromium-aluminum wrought alloy having excellent high temperature corrosion resistance, good creep strength and good machinability. Background Art

[0002] Austenitic nickel-chromium-aluminum-wrought alloys with varying nickel, chromium and aluminum contents have long been used in furnace construction and in the chemical and petrochemical industries. For this use, good high-temperature corrosion resistance (even in carburizing atmospheres that produce "metal dusting") and good high-temperature strength / creep strength are required.

[0003] It should be generally noted that the high temperature corrosion resistance of the alloys given in Table 1 increases with increasing chromium content. All of these alloys form a chromium oxide layer (Cr2O3) with a more or less closed aluminum layer (Al2O3) located below it when the corresponding aluminum content. Small additions of elements with strong oxygen affinity (e.g. yttrium or cerium) improve the oxidation resistance. During use in the application field for constructing the protective layer, the chromium content is slowly consumed. Therefore, the service life of the material is increased by a higher chromium content, because the higher content of elemental chromium forming the protective layer delays the time point when the chromium content falls below the critical limit and forms an oxide different from pure chromium oxide (Cr2O3), which can be, for example, an iron-containing and nickel-containing oxide. Further improvement of the high temperature corrosion resistance can be achieved by adding aluminum and silicon. Starting from a certain minimum content, these elements form a closed layer below the chromium oxide layer and thus reduce the consumption of chromium.

[0004] In the carburizing atmosphere (CO, H2, CH4, CO2, H2O mixture, optionally with other non-oxidizing components determined by the process), carbon can penetrate into the material, so that internal carbide formation can occur. This leads to a loss of notched impact strength. The melting point can also drop to very low values ​​(up to 350°C) and transformation processes can occur due to chromium depletion of the matrix.

[0005] High carburization resistance is obtained by materials with low carbon solubility and low carbon diffusion rate. Therefore, nickel alloys are generally more resistant to carburization than iron alloys, because carbon diffusion and carbon solubility in nickel are lower than those in iron. An increase in the chromium content brings higher carburization resistance by forming a protective chromium oxide layer, unless the oxygen partial pressure in the gas is too low for the formation of this protective chromium oxide layer. At very low oxygen partial pressures, silicon- or aluminum-containing materials can be used, because they form silicon oxide layers or even more stable aluminum oxide layers, which are formed at even much lower oxygen partial pressures than chromium oxide.

[0006] In the case of a carbon activity greater than 1 (i.e. the gas is unbalanced), "metal dusting" can occur in nickel-based alloys, iron-based alloys or cobalt-based alloys. In contact with the gas, the alloy can absorb large amounts of carbon. Segregation processes that occur in carbon-supersaturated alloys lead to material destruction. Here, the alloy decomposes into a mixture of metal particles, graphite, carbides and / or oxides. This type of material destruction occurs in a temperature range of approximately 500° C. to 750° C.

[0007] Typical conditions under which “metal dusting” occurs are strongly carburizing CO, H 2 and / or CH 4 gas mixtures, as occur in particular in ammonia synthesis, in methanol plants, in metallurgical processes, but also in quenching furnaces.

[0008] Resistance to "metal dusting" tends to increase as the nickel content of the alloy increases, but even nickel alloys are not resistant to "metal dusting".

[0009] Under "metal dusting" conditions, the chromium and aluminum contents have a significant influence on the corrosion resistance (see Figure 2 ). Nickel alloys with low chromium content, such as alloy Alloy 600 (N06600) (see Table 1) show relatively high corrosion rates under "metal dusting" conditions. Significantly more resistant are the nickel alloys Alloy 602CA (N06025) with a chromium content of 25% and an aluminum content of 2.3%, and Alloy 690 (N06690) with a chromium content of 30% (Hermse, CGM and van Wortel, JC: Metal dus ting: relation between alloy composition and degradation rate. Corros ion Engineering, Science and Technology 44 (2009), pp. 182-185). Resistance to "metal dusting" increases with the sum of chromium and aluminum (Cr+Al).

[0010] The high temperature strength or creep strength at a given temperature (approximately 500 to 750° C.) is improved in particular by a high carbon content. However, high contents of mixed crystal solidifying elements such as chromium, aluminum, silicon, molybdenum and tungsten also improve the high temperature strength or creep strength. In the range of 500° C. to 900° C., the addition of aluminum, titanium and / or niobium can improve the strength by precipitation of γ′ and / or γ″ phases.

[0011] Examples of these alloys according to the prior art are listed in Table 1.

[0012] Alloys such as Alloy 602CA (N06025), Alloy 693 (N06693) or Alloy 603 (N06603) have long been known for their excellent corrosion resistance due to the high aluminum content of more than 1.8% compared to Alloy 600 (N06600) or Alloy 601 (N06601). Alloy 602CA (N06025), Alloy 693 (N06693), Alloy 603 (N06603) and Alloy 690 (N06690) show excellent resistance to carburization or "metal dusting" due to their high chromium content and / or aluminum content. At the same time, alloys such as Alloy 602CA (N06025), Alloy 693 (N06693) or Alloy 603 (N06603) show excellent high temperature strength or creep strength in the temperature range where "metal dusting" occurs due to the high carbon content or aluminum content. Alloy 602CA (N06025) and Alloy 603 (N06603) have excellent high temperature strength or creep strength even at temperatures above 1000°C. However, the machinability is impaired, especially due to the high aluminum content, wherein the higher the aluminum content, the greater the damage (Alloy 693-N06693). The same situation applies to silicon to a greater extent, which forms a low melting point phase with nickel. In Alloy 602CA (N06025) or Alloy 603 (N06603), in particular, cold formability is limited due to the high specific gravity of primary carbides.

[0013] WO 2013 / 182177 A1 discloses (in wt%) 24 to 33% chromium, 1.8 to 4.0% aluminum, 0.10 to 7.0% iron, 0.001 to 0.50% silicon, 0.005 to 2.0% manganese, 0.00 to 0.60% titanium, 0.0002 to 0.05% magnesium and / or calcium, respectively, 0.005 to 0.12% carbon, 0.001 to 0.050% nitrogen, 0.0001 to 0.020% oxygen, 0.001 to 0.030% phosphorus, maximum 0.010% sulfur, maximum 2.0% molybdenum, maximum 2.0% tungsten, the remainder nickel and customary process-dependent impurities, wherein the following relationship must be met:

[0014] Cr+Al≥28 (2a) and

[0015] Fp≤39.9 (3a) where

[0016] Fp=Cr+0.272*Fe+2.36*Al+2.22*S i+2.48*Ti

[0017] +0.374*Mo+0.538*W-11.8*C(4a)

[0018] Cr, Fe, Al, Si, Ti, Mo, W and C are the concentrations of the elements involved in mass %. This nickel-chromium-aluminum alloy exhibits excellent high-temperature corrosion resistance under highly corrosive conditions, such as excellent resistance to "metal dusting", good corrosion resistance to air, good phase stability, good high-temperature strength and good creep strength, as well as good machinability.

[0019] US 6623869 B1 discloses a metal material, which is composed of no more than 0.2% C, 0.01-4% Si, 0.05-2.0% Mn, no more than 0.04% P, no more than 0.015% S, 10-35% Cr, 30-78% Ni, 0.005-4.5% Al, 0.005-0.2% N, and 0.015-3% Cu and 0.015-3% Co, or both, and the balance of 100% iron. Here, the value of 40Si+Ni+5Al+40N+10(Cu+Co) is not less than 50, wherein the symbol of the element represents the content of the corresponding element in mass %. The material has excellent corrosion resistance in an environment where "metal dusting" may occur and can therefore be used for furnace tubes, pipe systems, heat exchanger tubes, etc. in refineries or petrochemical equipment, and can significantly improve the service life and safety of the equipment.

[0020] EP 0 508 058 A1 discloses an austenitic nickel-chromium-iron alloy consisting of (in weight %) 0.12-0.3% C, 23-30% Cr, 8-11% Fe, 1.8-2.4% Al, 0.01-0.15% Y, 0.01-1.0% Ti, 0.01-1.0% Nb, 0.01-0.2% Zr, 0.001-0.015% Mg, 0.001-0.01% Ca, maximum 0.03% N, maximum 0.5% Si, maximum 0.25% Mn, maximum 0.02% P, maximum 0.01% S, balance Ni, including unavoidable impurities caused by smelting.

[0021] Alloys used in furnace construction and the petrochemical industry must be weldable in order to manufacture the individual components of the equipment. The individual components must also be weldable when installed in the equipment as appropriate. Due to their structure, welds often show a low creep strength and / or tend to crack. By heat treating the welds, the creep strength can be improved and the tendency to crack can be reduced. Some examples are listed in the following prior art.

[0022] EP 0 234 200 A1 discloses a method and a device for heat treating a longitudinal welded pipe made of austenitic, ferritic or austenitic-ferritic stainless steel, wherein the pipe is annealed after welding the longitudinal weld. The method is characterized in that the pipe is solution annealed only partially in the region of the weld and the heat-affected zone, while the remaining regions are heat treated at a lower temperature. For high-alloy molybdenum-containing steels, annealing is performed at a temperature above 1100° C., preferably above 1250° C., wherein the annealing temperature is maintained for more than 5 seconds, preferably for approximately 25 seconds.

[0023] US 3865639 A discloses a method for producing a welded structural component, the welded parts of which are capable of withstanding operating temperatures in the range of about 900 to 1050° C., wherein the components consist of at least one high-alloy austenitic steel alloyed with chromium, nickel and / or cobalt and containing less than 60% by weight of iron, up to 0.5% by weight of carbon and low concentrations of additional elements such as manganese and silicon. Here, a given component is subjected to welding, wherein welding results in the formation of at least one weld seam having a solidification front corresponding to the physical and chemical discontinuity in the weld seam, wherein the weld seam also consists of a highly alloyed austenitic steel and is then treated in such a way that the solidification front becomes chemically homogenous, so that carbides of the weld seam are present to a maximum extent and according to a finely uniform distribution in the precipitated state, which results in the creep strength and tensile strength of the weld seam being increased to values ​​that are at least approximately the same as the creep strength and tensile strength of all unwelded parts, in that the weld seam and adjacent regions of the welded parts are subjected to a homogenization heat treatment at a temperature of between approximately 1100° C. and 1200° C. for a period of several minutes to several hours, after which at least the weld seam and the adjacent regions are cooled at a cooling rate of approximately 100° C. / hour to approximately 800° C. and then air-cooled to room temperature.

[0024] US 3046167 A describes a method for heat treating welded, hardenable chromium-nickel stainless steel in order to give it a high degree of ductility and toughness in the hardened state, wherein the method comprises the successive steps of welding and converting the welded product by annealing to a structure that is essentially martensitic but contains some ferrite, followed by re-producing the structure of the steel to be essentially austenitic, even if it contains some ferrite. This occurs by annealing at a temperature and time sufficient to re-austenitize the martensite and ferrite and to break up the original cast structure of the weld. The metal is then converted back to a structure that is essentially martensitic with very little ferrite, and finally hardened by appropriate heat treatment to a state that is essentially completely martensitic. In processing a hardenable chromium-nickel-stainless steel product, it is selected from the group of steels having the following analysis: about 17% chromium, 7% nickel, 1% aluminum and the balance iron; about 17% chromium, 4% nickel, 3% copper and the balance iron; about 15% chromium, 7% nickel, 2% molybdenum, 1% aluminum and the balance iron; and about 12% chromium, 8% nickel, 6% molybdenum, 1% aluminum and the balance iron, wherein the method first comprises welding the product under a shielding gas, then transforming the welded product by heating at about 760 to 954.4°C and cooling at about room temperature up to -73.3°C, then annealing the transformed product at about 1065.6°C, then transforming the product by heating and cooling as described above, and finally hardening by heating at about 482.2 to 593.3°C.

[0025] US 4168190 A describes a method and apparatus for local solution annealing of austenitic stainless steel, which is partially sensitized, for example, by local temperature increase without producing a sensitized structure at the thermal boundary between the locally treated section and the remaining material, the method comprising the steps of: (a) rapidly heating the sensitized portion of the material to a temperature at which carbides gradually change into solution; and (b) rapidly quenching the heated material. Summary of the invention

[0026] The object of the present invention is to devise a method for producing a component from a semi-finished product of a nickel-chromium-aluminum wrought alloy, wherein the component contains a weld seam and / or the component is partially or completely installed in a system using a weld seam.

[0027] The object is achieved by a method for producing a component, which is produced partly or completely from a semi-finished product of a nickel-chromium-aluminum alloy, which has (in % by mass) more than 18% to 33% chromium, 1.8% to 4.0% aluminum, 0.01% to 7.0% iron, 0.001% to 0.50% silicon, 0.001% to 2.0% manganese, 0.00% to 0.60% titanium, 0.0% to 0.05% magnesium and / or calcium, respectively, 0.005% to 0.12% carbon, 0.0005% to 0.050% nitrogen, 0.0001% to 0.020% oxygen, 0.001% to 0.030% phosphorus, a maximum of 0 .010% sulfur, maximum 2.0% molybdenum, maximum 2.0% tungsten, a balance of greater than or equal to 50% nickel and common process-dependent impurities, wherein the component contains welds of the same type and / or the component is partially or completely provided with welds of the same type for installation in a device, wherein after welding, for the purpose of weld homogenization and / or stress reduction, only welds of the same type and heat-affected zones are subjected to annealing at temperatures between above 980° C. and 1250° C. for a period of 0.05 minutes to 24 hours, followed by cooling in static protective gas or air, moving (blown) protective gas or air, as a result of which the creep strength and creep ductility of the weld are improved by this annealing.

[0028] The following relationship must be satisfied:

[0029] Cr+Al≥28 (1a) and

[0030] Fp≤39.9 (2a) where

[0031] Fp=Cr+0.272*Fe+2.36*Al+2.22*S i+2.48*Ti

[0032] +0.374*Mo+0.538*W-11.8*C(3a)

[0033] Wherein Cr, Fe, Al, Si, Ti, Mo, W and C are the concentrations of the elements concerned in mass %.

[0034] Advantageous further developments of the subject matter of the invention can be gathered from the associated dependent claims.

[0035] Semi-finished products made of metal are semi-finished products such as plates, strips, bars, forgings, tubes and wires.

[0036] A component can be joined together by two or more processed semi-finished products and / or other components. The joining can be carried out, for example, by a fusion welding method, optionally with additional welding additives. The welding additive can be provided during the welding process, for example, by a welding rod or welding wire.

[0037] The same type of welding filler has a composition comparable to the adjacent processed semi-finished product and / or component. In the case of a corresponding configuration of the weld seam geometry, the same type of welding filler can also consist of a part of at least one adjacent semi-finished product to be welded.

[0038] The nickel-chromium-aluminum-wrought alloy (herein referred to as Alloy NiCrAl-H) used in the present invention is preferably melted in an electric furnace or arc furnace in an open state and then processed in a VOD (vacuum, oxidation, deoxidation) or VLF (vacuum ladle furnace) device. However, it can also be melted and cast in a vacuum. The alloy is then cast into blocks, electrodes or in the form of continuous casting to form a primary product. Optionally, the primary product is then annealed at a temperature between 900 and 1270°C for 0.1 hour to 70 hours. In addition, the alloy can be remelted once or more using ESU (electric-slag-remelting equipment) and / or VAR (vacuum arc remelting). The alloy is then formed into the desired semi-finished product form. To this end, annealing is performed at a temperature between 900 and 1270°C for 0.1 hour to 70 hours, and then hot deformation is performed, and intermediate annealing is performed between 900 and 1270°C for 0.05 hours to 70 hours. The surface of the material can be chemically and / or mechanically stripped for cleaning, as appropriate (even multiple times) during and / or after the hot forming. Then, in a moving annealing atmosphere or in a water bath, it can be cold-formed to the desired semi-finished form with a deformation degree of up to 98%, and an intermediate annealing between 800 and 1250° C. can be carried out for 0.05 minutes to 70 hours under a protective gas (for example argon or hydrogen), and then air cooling can be carried out. Then, in a moving annealing atmosphere or in a water bath, it can be solution annealed for 0.05 minutes to 70 hours in a temperature range of 800 to 1250° C. under a protective gas (for example argon or hydrogen), and then air cooling can be carried out. Chemical and / or mechanical cleaning of the material surface can be carried out during and / or after the final annealing, as appropriate.

[0039] Preferably, solution annealing occurs between the following temperatures:

[0040] -1000 or >1000 to 1200℃ or <1200℃

[0041] -1000 or >1000 to 1175℃ or <1175℃

[0042] -1025 or >1025 to 1150℃ or <1150℃

[0043] -1050 or >1050 to 1130℃ or <1130℃

[0044] -1080 or >1080 to 1130℃ or <1130℃

[0045] Preferably, solution annealing occurs within the following time range:

[0046] -0.05 minutes to 24 hours

[0047] -0.05 minutes to 8 hours

[0048] -0.05 minutes to 4 hours

[0049] -0.1 minutes to 1 hour

[0050] - 1 minute to 1 hour

[0051] -5 minutes to 1 hour

[0052] The nickel-chromium-aluminum-wrought alloy (Al loy NiCrAl-H) used in the present invention can be readily manufactured and used in the form of semi-finished products in the form of strips, plates, bars, forgings, wires, longitudinal seam welded tubes and seamless pipes.

[0053] These semi-finished forms are manufactured with an average particle size of 30 to 600 μm. The preferred range is:

[0054] -40μm to 300μm.

[0055] -60μm to 300μm.

[0056] -75μm to 200μm.

[0057] The parts required for the component are cut or separated from the semi-finished product, processed accordingly and then connected by means of a fusion welding method under protective gas.

[0058] Optionally, the fusion welding method may be, for example, one of the following methods:

[0059] -Tungsten Inert Gas Welding (WIG)

[0060] -Metal Inert Gas Welding (MIG)

[0061] -Metal active gas welding (MAG)

[0062] -Plasma welding

[0063] -Electron beam welding

[0064] -Laser beam welding

[0065] - Gas welding or oxyacetylene welding

[0066] -Electrode welding / manual arc welding

[0067] The protective gas may preferably be either argon or argon and hydrogen or argon and nitrogen.

[0068] However, submerged arc welding and other methods are also conceivable.

[0069] The same type of welding additive is preferably a nickel + chromium-aluminum alloy, which contains (in mass %) more than 18% to 33% chromium, 1.8% to 4.0% aluminum, 0.01% to 7.0% iron, 0.001% to 0.50% silicon, 0.001% to 2.0% manganese, 0.00% to 0.60% titanium, 0.0% to 0.05% magnesium and / or calcium, respectively, 0.005% to 0.12% carbon, 0.0005% to 0.050% nitrogen, 0.0001%-0.020% oxygen, 0.001 to 0.030% phosphorus, maximum 0.010% sulfur, maximum 2.0% molybdenum, maximum 2.0% tungsten, the balance nickel greater than or equal to 50%, and the usual process-dependent impurities, wherein the following relationship must be met:

[0070] Cr+Al≥28 (1a) and

[0071] Fp≤39.9 (2a) where Fp=Cr+0.272*Fe+2.36*Al+2.22*Si+2.48*Ti

[0072] +0.374*Mo+0.538*W-11.8*C(3a)

[0073] Wherein Cr, Fe, Al, Si, Ti, Mo, W and C are the concentrations of the elements concerned in mass %.

[0074] The following refinements of the subject matter of the invention with regard to composition are advantageous both for the production of semi-finished nickel-chromium-aluminum alloy Alloy NiCrAl-H and for welding fillers of the same type.

[0075] The extended range of elemental chromium is between 18 and 33%, where the preferred range can be adjusted as follows:

[0076] -20 or >20 to 33 or <33%

[0077] -22 or >22 to 33 or <33%

[0078] -24 or >24 to 33 or <33%

[0079] -24 or >24 to 32 or <32%

[0080] -25 or >25 to 32 or <32%

[0081] -26 or >26 to 32 or <32%

[0082] -27 or >27 to 32 or <32%

[0083] -28 or >28 to 32 or <32%

[0084] -28 or >28 to 31 or <31%

[0085] -28 or >28 to 30 or <30%

[0086] -29 or >29 to 31 or <31%

[0087] The aluminum content is between 1.8 and 4.0%, wherein here too the preferred aluminum content can be adjusted as follows depending on the area of ​​use of the alloy:

[0088] -1.8 or >1.8 to <4.0%

[0089] -1.8 or >1.8 to 3.2 or <3.2%

[0090] -2.0 or >2.0 to 3.2 or <3.2%

[0091] -2.0 or >2.0 to 3.0 or <3.0%

[0092] -2.0 or >2.0 to 2.8 or <2.8%

[0093] -2.0 or >2.2 to 2.8 or <2.8%

[0094] -2.0 or >2.2 to 2.6 or <2.6%

[0095] The iron content is between 0.01 and 7.0%, wherein the preferred content can be set within the following extended ranges depending on the field of application:

[0096] -0.01 to 4.0 or <4.0%

[0097] -0.01 to 3.0 or <3.0%

[0098] -0.01 to 2.5 or <2.5%

[0099] -0.1 to 2.0 or <2.0%

[0100] -0.1 to 1.0 or <1.0%

[0101] The silicon content is between 0.001 and 0.50%. Preferably, Si can be adjusted in the alloy within an extended range as follows:

[0102] -0.001 to 0.20 or <0.20%

[0103] -0.001 to 0.10 or <0.10%

[0104] -0.001 to 0.05 or <0.05%

[0105] The same applies to the element manganese, which may be contained in the alloy in amounts of 0.001 to 2.0%. Alternatively, the following extended ranges are also conceivable:

[0106] -0.005 to 0.50 or <0.20%

[0107] -0.005 to 0.20 or <0.20%

[0108] -0.001 to 0.20 or <0.20%

[0109] -0.005 to 0.10 or <0.10%

[0110] -0.005 to 0.05 or <0.05%

[0111] The titanium content is between 0.00 and 0.60%. Preferably, Ti can be adjusted in the alloy within an extended range as follows:

[0112] -0.001 to 0.60 or <0.60%

[0113] -0.001 to 0.50 or <0.50%

[0114] -0.001 to 0.30 or <0.30%

[0115] -0.001 to 0.25 or <0.25%

[0116] -0.001 to 0.10 or <0.10%

[0117] -0.001 to 0.02 or <0.02%

[0118] -0.01 to 0.10 or <0.10%

[0119] Magnesium and / or calcium may also be included in a content of 0.00 to 0.05%. There is preferably the possibility of adjusting these elements in the alloy as follows:

[0120] -0.00 to 0.03 or <0.03%

[0121] -0.00 to 0.02 or <0.02%

[0122] The alloy contains 0.005 to 0.12% carbon. Preferably, the carbon can be adjusted in the alloy within an extended range as follows:

[0123] -0.01 to <0.12%

[0124] -0.01 to 0.10 or <0.10%

[0125] -0.01 to 0.08 or <0.08%

[0126] -0.01 to 0.05 or <0.05%

[0127] -0.02 to 0.10 or <0.10%

[0128] -0.03 to 0.10 or <0.10%

[0129] The same applies to the element nitrogen, which is contained in a content of between 0.0005 and 0.05%. Preferred contents can be given as follows:

[0130] -0.001 to 0.04%

[0131] The alloy furthermore contains oxygen in a content of between 0.0001 and 0.020%, in particular 0.0001 to 0.010%.

[0132] The alloy furthermore contains phosphorus in a content of 0.001 to 0.030%. Preferred contents can be given as follows:

[0133] -0.001 to 0.020%

[0134] The elemental sulfur in the alloy can be given as:

[0135] -Maximum 0.010%

[0136] Molybdenum and tungsten are contained in the alloy individually or in combination in a maximum content of 2.0%. Preferred contents can be given as follows:

[0137] -Momax 1.0%

[0138] -W max 1.0%

[0139] -Momax<1.0%

[0140] -Wmax<1.0%

[0141] -Momax<0.50%

[0142] -Wmax<0.50%

[0143] -Momax<0.10%

[0144] -W maximum<0.10%

[0145] -Momax<0.05%

[0146] -W maximum<0.05%

[0147] Nickel is the balance. Preferably, the balance can be given as follows:

[0148] ->50% or ≥50%

[0149] ->55% or ≥55%

[0150] ->60% or ≥60%

[0151] ->65% or ≥65%

[0152] ->67% or ≥67%

[0153] For highly corrosive conditions, but especially for good "metal dusting" resistance, it is advantageous for Cr to Al to satisfy the following relationship:

[0154] Cr+Al≥28(1a)

[0155] Wherein chromium and aluminum are the concentrations of the elements concerned in mass %. The preferred range can be adjusted as follows:

[0156] Cr+Al≥29(1b)

[0157] Cr+Al≥30(1c)

[0158] Cr+Al≥31(1d)

[0159] Furthermore, the following relationship must be satisfied, thereby giving sufficient phase stability:

[0160] Fp≤39.9(2a), where

[0161] Fp=Cr+0.272*Fe+2.36*Al+2.22*S i+2.48*Ti

[0162] +0.374*Mo+0.538*W-11.8*C (3a) wherein Cr, Fe, Al, Si, Ti, Mo, W and C are the concentrations of the elements concerned in mass %.

[0163] The preferred range can be adjusted as follows:

[0164] Fp≤38.4(2b)

[0165] Fp≤36.6(2c)

[0166] Optionally, the element niobium can be incorporated in the alloy in a content of 0.0 to 1.10%. Preferably, niobium can be incorporated in the alloy in an extended range as follows:

[0167] -0.001 to <1.10%

[0168] -0.001 to 1.0 or <1.0%

[0169] -0.001 to 0.70 or <0.70%

[0170] -0.001 to 0.50 or <0.50%

[0171] -0.001 to 0.30 or <0.30%

[0172] -0.01 to 0.30 or <0.30%

[0173] If niobium is present in the alloy, equation (3a) must be supplemented with the term containing niobium as follows:

[0174] Fp=Cr+0.272*Fe+2.36*Al+2.22*S i+2.48*Ti

[0175] +1.26*Nb+0.374*Mo+0.538*W-11.8*C (3b) wherein Cr, Fe, Al, Si, Ti, Nb, Mo, W and C are the concentrations of the elements concerned in mass %.

[0176] Optionally, the zirconium content may be between 0.0 and 0.20%. Preferably, zirconium may be adjusted in the alloy within an extended range as follows:

[0177] -0.0 to 0.15 or <0.15%

[0178] -0.0 to 0.10 or <0.10%

[0179] -0.001 to 0.07 or <0.07%

[0180] -0.001 to 0.04 or <0.04%

[0181] -0.01 to 0.04 or <0.04%

[0182] Optionally, the element yttrium can be adjusted in the alloy in a content of 0.0 to 0.20%. Preferably, yttrium can be adjusted in the alloy within an extended range as follows:

[0183] -0.0 to 0.15 or <0.15%

[0184] -0.0 to 0.10% or <0.10%

[0185] -0.0 to 0.08 or <0.08%

[0186] -0.001 to <0.045%

[0187] -0.01 to 0.04 or <0.04%

[0188] Optionally, the element lanthanum can be adjusted in the alloy in a content of 0.0 to 0.20%. Preferably, lanthanum can be adjusted in the alloy in an extended range as follows:

[0189] -0.0 to 0.15 or <0.15%

[0190] -0.0 to 0.10 or <0.10%

[0191] -0.0 to 0.08 or <0.08%

[0192] -0.001 to 0.04 or <0.04%

[0193] -0.01 to 0.04 or <0.04%

[0194] Optionally, the element cerium can be adjusted in the alloy in a content of 0.0 to 0.20%. Preferably, cerium can be adjusted in the alloy in an extended range as follows:

[0195] -0.0 to 0.15 or <0.15%

[0196] -0.0 to 0.10% or <0.10%

[0197] -0.0 to 0.08 or <0.08%

[0198] -0.001 to 0.04 or <0.04%

[0199] -0.01 to 0.04 or <0.04%

[0200] Alternatively, in the case of simultaneous addition of cerium and lanthanum, a cerium mixed metal can also be used in a content of 0.0 to 0.20%. Preferably, the cerium mixed metal can be adjusted in the alloy within an extended range as follows:

[0201] -0.0 to 0.15 or <0.15%

[0202] -0.0 to 0.10% or <0.10%

[0203] -0.0 to 0.08 or <0.08%

[0204] -0.001 to 0.04 or <0.04%

[0205] -0.01 to 0.04 or <0.04%

[0206] Optionally, the element hafnium can be adjusted in the alloy in a content of 0.0 to 0.20%. Preferably, hafnium can be adjusted in the alloy within an extended range as follows:

[0207] -0.0 to 0.15 or <0.15%

[0208] -0.0 to 0.10 or <0.10%

[0209] -0.001 to 0.07 or <0.07%

[0210] -0.001 to 0.04 or <0.04%

[0211] -0.01 to 0.04 or <0.04%.

[0212] Optionally, 0.001 to 0.60% tantalum may also be contained in the alloy. The preferred tantalum content may be given as follows:

[0213] -0.001 to 0.50 or <0.50%

[0214] -0.001 to 0.40 or <0.40%

[0215] -0.001 to 0.30 or <0.30%

[0216] -0.001 to 0.20 or <0.30%

[0217] -0.001 to 0.10 or <0.10%

[0218] -0.01 to 0.10 or <0.10%

[0219] Optionally, the element boron may be present in the alloy as follows:

[0220] - Boron 0.0001 to 0.008%

[0221] Preferred contents can be given as follows:

[0222] - Boron 0.0005 to 0.008%

[0223] - Boron 0.0005 to 0.004%

[0224] In addition, the alloy may contain between 0.0 and 5.0% cobalt as desired, and may furthermore be limited to the following:

[0225] -0.01 to 5.0 or <5.0%

[0226] -0.01 to 2.0 or <2.0%

[0227] -0.10 to 2.0 or <2.0%.

[0228] -0.01 to 0.5 or <0.5%

[0229] -0.01 to 0.1 or <0.1%

[0230] Furthermore, a maximum of 0.5% copper may optionally be present in the alloy.

[0231] Additionally, the copper content can be limited as follows:

[0232] -Cu maximum<0.20 or 0.20%

[0233] -Cu maximum<0.10 or 0.10%

[0234] -Cu maximum<0.05 or 0.05%

[0235] -Cu max<0.015%

[0236] If copper is present in the alloy, equation (3a) must be supplemented with the term for copper as follows:

[0237] Fp=Cr+0.272*Fe+2.36*Al+2.22*S i+2.48*Ti

[0238] +0.477*Cu+0.374*Mo+0.538*W-11.8*C (3c) wherein Cr, Fe, Al, Si, Ti, Cu, Mo, W and C are the concentrations of the elements concerned in mass %.

[0239] If niobium and copper are present in the alloy, equation (3a) must be supplemented with a term containing niobium and a term containing copper as follows:

[0240] Fp=Cr+0.272*Fe+2.36*Al+2.22*S i+2.48*Ti

[0241] +1.26*Nb+0.477*Cu+0.374*Mo+0.538*W-11.8*C(3d)wherein Cr, Fe, Al, Si, Ti, Nb, Cu, Mo, W and C are the concentrations of the elements concerned in mass %.

[0242] Furthermore, a maximum of 0.5% vanadium may optionally be contained in the alloy.

[0243] Furthermore, the vanadium content may be limited as follows:

[0244] -Vmax<0.10%

[0245] Finally, as impurities, the elements lead, zinc and tin can also be given in the following amounts:

[0246] Lead 0.002% max

[0247] Zinc max 0.002%

[0248] Tin max 0.002%

[0249] The annealing of the weld seam and the heat-affected zone can be carried out, for example, in particular by means of heating mats, infrared radiators, lasers or inductive electrical heating. Optionally, partial regions of the remaining structure can be cooled simultaneously.

[0250] For the purpose of homogenizing the weld and / or reducing stresses, it is also possible that, after welding, the entire component having welds of the same type is subjected to an annealing at between 980° C. and 1250° C. for a period of 0.05 minutes to 24 hours, followed by cooling in static protective gas or air, moving (blown) protective gas or air, with the result that, through this annealing (optionally after solution annealing of the semi-finished product), the creep strength and creep ductility of welds of the same type are improved.

[0251] Furthermore, it is possible to repeat this annealing after welding and homogenizing the weld seams of the same type, either by annealing the entire component including the weld seams or by annealing only the weld seams of the same type and the heat-affected zones, selectively by annealing the entire component including the weld seams of the same type or by annealing only the weld seams of the same type and the heat-affected zones. The order of partial annealing of only the weld seams of the same type and the heat-affected zones and the order of annealing the entire component is arbitrary.

[0252] Preferably, annealing occurs after soldering at temperatures between:

[0253] -1000 or >1000 to 1200 or <1200℃

[0254] -1000 or >1000 to 1175 or <1175℃

[0255] -1025 or >1025 to 1150 or <1150℃

[0256] -1050 or >1050 to 1130 or <1130℃

[0257] -1080 or >1080 to 1130 or <1130℃

[0258] Preferably, annealing occurs within the following time range:

[0259] -0.05 minutes to 16 hours

[0260] -0.05 minutes to 8 hours

[0261] -0.05 minutes to 4 hours

[0262] -0.1 minutes to 1 hour

[0263] - 1 minute to 1 hour

[0264] -5 minutes to 1 hour

[0265] The shielding gas used for annealing after welding may preferably (if not in air) consist of the following gases:

[0266] -Argon

[0267] -Argon-air mixture

[0268] -hydrogen

[0269] -Hydrogen-air mixture

[0270] -Argon-Nitrogen mixture

[0271] The improvement of the creep strength and creep ductility of welds of the same type occurs in particular in the range of gamma prime formation, which is a temperature range of up to 750° C.

[0272] After annealing of components with welds of the same type or only after annealing of welds and heat-affected zones of the same type of components or welds and heat-affected zones of the same type installed in the equipment, the surface can be cleaned or processed selectively by brushing, etching, sandblasting, grinding, peeling, planing and / or milling. One or more of these processes can also selectively take place after welding. In particular, the processing of the annealed surface, especially the weld and heat-affected zone, by grinding, peeling, planing, milling and stripping the material after the last annealing improves the corrosion resistance, especially the "metal dusting" resistance.

[0273] After grinding of the weld seam and heat-affected zone, it is advantageous if a roughness value Ra of 0.01 to 15 μm is achieved, since this improves the corrosion resistance and in particular the metal dusting resistance and raises it almost to the value of the base material.

[0274] The components manufactured according to the invention should preferably be used in areas where highly corrosive conditions (eg highly carburizing conditions, atmospheres producing "metal dusting") prevail, for example in components in the petrochemical industry. In addition, these components are also suitable for furnace construction. Example:

[0275] Manufacturing of components made from semi-finished products

[0276] Figure 1a On the left, a sketch of a semi-finished product in the form of a sheet ( 1 ), a strip ( 2 ), a rod ( 3 ), a tube ( 4 ), a wire or a welding filler in wire form ( 5 ) is shown in a top view and in cross section. Figure 1aOn the right, it is shown by way of example how a product or a primary product (7) is produced, for example by cutting two components (1a, 1b) from a semi-finished sheet metal and chamfering them (ii) and then joining them (iv) by means of a V-shaped seam (6a) by means of welding (iii) using a welding filler in the form of a wire (5). Figure 1b On the left is shown another example of the production of a product or a preliminary product (7), in which, for example, two tube components (4a, 4b) are cut from a semi-finished tube and chamfered (ii) and then joined (iv) by fusion welding (iii) with a V-shaped seam (6b) using a welding filler in the form of a wire (5). Figure 1b Also shown in the center is another example of the production of a product or a primary product (7), in which a hole (ii) is milled out of a sheet metal semi-finished product or a sheet metal component (1c), a tube semi-finished product or a tube component (3c) is inserted into the hole and joined (iv) by fusion welding (iii) with a fillet weld (6c) using a welding filler in the form of a wire (5). Figure 1b Another example of the production of a product or preliminary product (7) is shown on the right, in which two strip segments (2a, 2b) (ii) separated from a semi-finished strip are processed so that their edges are aligned and are joined together (6d) (iv) by fusion welding (iii) using a part of the edge as a welding additive (9).

[0277] Tests performed:

[0278] The phases occurring in equilibrium were calculated for the various alloy variants using the JMatPro program from Thermotech. The database of nickel-based alloys TTNI7 from Thermotech was used as the data basis for the calculations.

[0279] The creep strength is determined in an uninterrupted uniaxial creep test using strain measurement under tensile load according to DIN EN ISO 204. For this purpose, the sample is inserted into a creep testing machine and loaded with a constant test force. The rupture time t u And the elongation at break A u b The time to rupture is a measure of creep strength and the elongation at rupture is a measure of creep ductility. The measuring range has a diameter of 10 mm and an initial reference length L of 50 mm. r0 The test is carried out on round samples. The sampling is carried out transversely to the forming direction of the semi-finished product.

[0280] Description of features

[0281] The nickel-chromium-aluminum alloy Al loy NiCrAl-H used in the present invention has good phase stability and creep strength in addition to excellent corrosion resistance under highly corrosive conditions (here, for example, excellent “metal dusting” resistance).

[0282] Phase stability

[0283] In the nickel-chromium-aluminum-iron system with additions of titanium and / or niobium, different brittle TCP phases (topologically close packed phases) such as Laves phases, σ phases or μ phases or also brittle η phases or ε phases can be formed, depending on the alloy content. For example, the calculation of the temperature-dependent equilibrium specific gravity for N06690, batch 111389 (see Table 2 for the composition used here) shows by calculation that at 720° C. (T S BCC ) in large proportions to form α-chromium ( Figure 3 BCC phase in the alloy). Since this phase is very different from the parent material in analysis, it is generally difficult to form this phase. However, if the formation temperature T S BCC Very high, this phase may arise from this, as described, for example, in "ES Levolden, JZ Albertsen. U. Fink, Tjeldbergodden Methanol Plant: Meta l Dus ting Inves ting ions", Corros ion / 2011, Paper No. 11144 (Houston, TX: NACE 2011), page 15" for a variant of Alloy 693 (UNS 06693). Figure 4 and Figure 5 The phase diagram of Alloy 693 variant (from US 4,882,125; Table 1) in Table 2 is shown as Alloy 3 or Alloy 10. This phase is brittle and leads to undesirable embrittlement of the material. Alloy 3 has a formation temperature T of 1079°C. S BCC, and Alloy 10 is 939°C. In "ES Levolden, JZ Albertsen. U. Fink, Tjeldbergodden Methanol Plant: "Meta lDus ting Inves t igat ions", Corros ion / 2011, paper number 11144 (Houston, TX: NACE 2011), page 15", there is no description of the exact analysis of the alloy when α-chromium (BCC) is present. However, based on this, the examples or analyses listed in Table 2 for Alloy 693, which have the highest formation temperature T calculated, are given in Table 2. S BCC (e.g., Alloy 10) can form α-chromium (BCC phase). In the corrected analysis (with a reduced formation temperature T S BCC ), in "E. Slevolden, JZ Albertsen. U. Fink, Tjeldbergodden Methanol Plant: Metal Dusting Investigations", Corrosion / 2011, Paper No. 11144 (Houston, TX: NACE 2011), page 15", α-chromium is therefore only still observed near the surface. In order to avoid the appearance of such brittle phases, in the case of the nickel-chromium-aluminum alloy (Al loy NiCrAl-H) used in the present invention, the formation temperature T S BCC It should be less than or equal to 939°C, which is the lowest formation temperature T in the example of Alloy 693 in Table 2 (from Table 1 of US Pat. No. 4,882,125). S BCC .

[0284] This is especially the case when the following formula is satisfied:

[0285] Fp≤39.9(2a), where

[0286] Fp=Cr+0.272*Fe+2.36*Al+2.22*S i+2.48*Ti

[0287] +1.26*Nb+0.477*Cu+0.374*Mo+0.538*W-11.8*C(3d)wherein Cr, Al, Fe, Si, Ti, Nb, Cu, Mo, W and C are the concentrations of the elements in mass %. Table 2 with alloys shows that the Fp for Alloy 8, Alloy 3 and Alloy 2 is greater than 39.9 and the Fp for Alloy 10 is exactly 39.9. For all other alloys, T S BCC Less than 939°C and therefore Fp<39.9.

[0288] Examples and properties for producing welded components

[0289] Tables 3a and 3b show the analysis of a batch melted on an industrial scale of the AlloyNiCrAl-H alloy used in the present invention, from which plates and welded bars are made. In the batch, the formula (2a) Al+Cr≥28 is satisfied and therefore the requirements for "metal dusting" resistance are met. The values ​​of Fp are also calculated according to formula (3a) for the compositions in Tables 3a and 3b. Fp is less than 39.9 as required.

[0290] The batches were melted openly in an amount of 16t and then processed in a VOD plant. Electrodes were then cast and ESU remelted. Thereafter, the alloy was annealed at a temperature between 900 and 1270°C for 0.1 to 70 hours and hot formed with an intermediate annealing between 900 and 1270°C for 0.1 to 70 hours. Hot rolled plates with a thickness of 25 or 16 mm were produced from batch 319144. Hot rolled wire was produced from batch 318385. After hot rolling at 1100°C for 40 minutes, the plates were solution annealed and then cooled in air. They were then sandblasted, acid etched and ground to remove the oxide layer. The 25mm thick plate had a grain size of about 89μm and the 16mm thick plate had a grain size of about 82μm. Therefore, the 25mm plate and the 16mm plate had comparable grain sizes. The rolled wire is also sandblasted, pickled and ground and then cold drawn to final thickness with an intermediate annealing between 800 and 1250° C. for 0.05 minutes to 70 hours. Subsequently, the wire is solution annealed in a temperature range of 800 to 1250° C. under hydrogen for 0.05 minutes to 70 hours and processed into welding bars with diameters of 2.0 and 2.4 mm.

[0291] Plate sections were cut from 25 mm thick solution-annealed semi-finished plates and annealed at 980° C. for 3 hours with subsequent air cooling. Samples for creep tests transverse to the rolling direction were produced from only solution-annealed and additionally annealed plates or plate sections. Table 5 shows the results of the creep tests according to DIN EN ISO 204.

[0292] Sheet sections with dimensions of 150×500 mm were cut from 16 mm thick semi-finished sheet metal. Two pieces were respectively welded with a 70° V-joint by means of WIG manual welding under pure argon using 2.0 and 2.4 mm thick welding rods from batch 318385 as welding additives with the welding parameters given in Table 4. The weld seam and the heat-affected zone were brushed directly after welding. Some parts of the welded sheet metal produced in this way were annealed at 980° C. for 3 hours with subsequent air cooling, others at 1100° C. for 40 minutes with subsequent air cooling, and still others at 1100° C. for 3 hours with subsequent air cooling. Some were not annealed. Seams or seam sections were also produced which were ground or not reprocessed at all. Samples for creep tests transverse to the weld seam were produced from welded sheets or welded and annealed sheets or sheet metal sections. Table 5 shows the results of the creep test according to DIN EN ISO 204.

[0293] As can be seen from Table 5, in the creep test at 600°C, the solution annealed plates with additional annealing at 980°C for 3 hours followed by air cooling (samples 1945B or 1946B) resulted in a longer rupture time t compared to the plates only solution annealed (samples 1923B or 197B). u Creep tests transverse to the weld (samples 302W or 303W) without further annealing (prior art T) also show a significantly reduced rupture time t compared to creep tests on plates that were only solution annealed. u Effect of additional annealing of the welded sections (from which creep specimens were made) at 980°C for 3 hours followed by air cooling (samples 247W and 249W) on the time to rupture t u No significant effect, but significantly reduced the elongation at break A u b In contrast, an additional annealing according to the invention of the welded segments (from which the creep specimens were produced) at 1100° C. for 40 minutes followed by air cooling (samples 250W or 503W) resulted in a significant increase in the rupture time t by a factor of about 3 compared to the samples which were not annealed after welding (samples 302W or 303W). u And the elongation at break A u bIn particular, additional annealing according to the invention for 3 hours at 1100° C. and subsequent air cooling of the welded sections (samples 511W or 506W) from which the creep specimens were made, respectively, resulted in a rupture time t of t 100° C. greater than that of the unwelded sheets which were only solution annealed (samples 1923B or 197B). u The further significant increase of the elongation at break A u b Almost increased to this value.

[0294] At 700°C, creep tests transverse to the weld without further annealing (prior art T) (sample 306W) showed a reduced rupture time t compared to creep tests on plates that were only solution annealed (sample 3034B) as at 600°C. u Additional annealing of the welded segments (from which the creep specimens were made) at 980° C. for 3 hours followed by air cooling (sample 248W) again yielded a rupture time t of 0.001 t compared to sample 306W which was not annealed after welding. u In contrast, an additional annealing according to the invention of the welded segments (from which the creep specimens were made) at 1100° C. for 40 minutes followed by air cooling (sample 251W) resulted in a significant increase in the rupture time t by a factor of about 2 relative to the sample that was not annealed after welding (306W). u And the elongation at break A u b Significantly increased beyond its value.

[0295] In particular, additional annealing according to the invention of the welded segments from which the creep specimens were made at 1100° C. for 3 hours followed by air cooling (sample 253W) resulted in a further increase in the rupture time t over the rupture time of the creep tests on the plates which had been solution annealed only. u .

[0296] At 800°C, solution annealed plates with additional annealing at 980°C for 3 hours followed by air cooling (Sample 1949B) produced similar fracture times t compared to plates that were solution annealed only (Sample 1922B). u Creep tests transverse to the weld without further annealing (Prior Art T) (Sample 309W) also have similar rupture times t compared to creep tests on plates that were only solution annealed (Sample 19 22B). u Additional annealing of the welded sections (from which creep specimens were made) at 1100°C for 40 minutes followed by air cooling (sample 519W) also yielded similar rupture times t compared to creep tests on the plates that were only solution annealed (sample 1922B). u .

[0297] This means that a heat treatment of the weld seam for at least 40 minutes after welding at 1100° C. according to the invention significantly improves the rupture time and the elongation at rupture of creep specimens transverse to the weld seam at temperatures between 600 and 700° C. and thus in the range of γ′ formation. At higher temperatures above the γ′ solvus temperature, the unannealed weld seam has a similar to better rupture time t compared to the plate which was only solution annealed. u Annealing of welds of the same type has only an insignificant effect on the rupture time at operating temperatures above the γ′ solvus temperature.

[0298] Therefore, the claimed limits for the method and the nickel-chromium-aluminum alloy Al loy NiCrAl-H used in the present invention can be justified in detail as follows:

[0299] Too low a chromium content means that when the alloy is used in a corrosive atmosphere, the chromium concentration below the oxide layer drops very rapidly below a critical limit, so that a closed chromium oxide layer can no longer be formed. Therefore, 18% chromium is the lower limit for chromium. Especially in the case of high aluminum contents of ≥ 1.8%, too high a chromium content deteriorates the phase stability of the alloy. Therefore, 33% chromium is regarded as an upper limit.

[0300] The formation of an aluminum oxide layer beneath the chromium oxide layer reduces the oxidation rate. Below 1.8% aluminum, the aluminum oxide layer is not too complete to fully function. Too high an aluminum content impairs the machinability of the alloy. Therefore, an aluminum content of 4.0% forms an upper limit.

[0301] The cost of the alloy increases with decreasing iron content. Below 0.01%, the costs increase excessively, since special prefabricated materials must be used. Therefore, for cost reasons, 0.01% iron is considered as a lower limit. With increasing iron content, the phase stability decreases (embrittled phases are formed), especially in the case of high chromium and aluminum contents. Therefore, 7% iron is a meaningful upper limit to ensure the phase stability of the alloy according to the invention.

[0302] Silicon is required when preparing the alloy. Therefore, a minimum content of 0.001% is required. Too high a content in turn impairs processability and phase stability, especially in the case of high aluminum and chromium contents. Therefore, the silicon content is limited to 0.50%.

[0303] To improve the machinability, a minimum content of 0.001% manganese is required. Manganese is limited to 2.0% because this element reduces oxidation resistance.

[0304] Titanium improves high temperature strength. Starting from 0.60%, oxidation behavior may be deteriorated, so 0.60% is the maximum value.

[0305] The already very low magnesium and / or calcium contents also improve processing by binding away sulfur, thereby avoiding the formation of low-melting NiS eutectics. In the case of excessively high contents, intermetallic Ni-Mg or Ni-Ca phases may occur, which in turn significantly impair the processability. Therefore, the magnesium and / or calcium content is limited to a maximum of 0.05%.

[0306] A minimum carbon content of 0.005% is necessary for good creep strength. Carbon is limited to a maximum of 0.12% since, starting from this content, this element reduces the machinability due to excessive formation of primary carbides.

[0307] A minimum content of 0.0005% nitrogen is required, thereby improving the machinability of the material. Nitrogen is limited to a maximum of 0.05% since this element reduces machinability by forming coarse carbonitrides.

[0308] The oxygen content must be ≤ 0.020% to ensure the manufacturability of the alloy. Too low an oxygen content increases the costs. The oxygen content is therefore ≥ 0.0001%.

[0309] The phosphorus content should be ≤ 0.030% because this interface-active element impairs the oxidation resistance. Too low a phosphorus content increases the costs. The phosphorus content is therefore ≥ 0.001%.

[0310] The sulfur content should be kept as low as possible, since this interface-active element impairs the oxidation resistance. A maximum of 0.010% sulfur is therefore established.

[0311] Molybdenum is limited to a maximum of 2.0% since this element reduces oxidation resistance.

[0312] Tungsten is limited to a maximum of 2.0% since this element also reduces oxidation resistance.

[0313] Nickel is a residual element. Too low a nickel content, especially in the case of high chromium contents, reduces the phase stability. Nickel must therefore be greater than or equal to 50%.

[0314] For highly corrosive conditions, but especially for good "metal dusting" resistance it is advantageous if the following relationship is satisfied between Cr and Al:

[0315] Cr+Al≥28(1a)

[0316] Where Cr and Al are the concentrations in mass % of the elements involved. Only in this way is the content of oxide-forming elements high enough to ensure adequate "metal dusting" resistance.

[0317] Furthermore, the following relationship must be satisfied, thereby imparting sufficient phase stability:

[0318] Fp≤39.9(2a), where

[0319] Fp=Cr+0.272*Fe+2.36*Al+2.22*S i+2.48*Ti

[0320] +0.374*Mo+0.538*W-11.8*C(3a)

[0321] Wherein Cr, Fe, Al, Si, Ti, Mo, W and C are the concentrations of the elements concerned in mass %. The limits of Fp and the reasons why additional elements may be included are explained in detail above.

[0322] If necessary, oxygen-affinity elements such as yttrium, lanthanum, cerium, cerium mixed metals, zirconium, hafnium can be added to further improve the oxidation resistance. This is achieved by incorporating them into the oxide layer and blocking the diffusion paths for oxygen at the grain boundaries there.

[0323] Yttrium improves oxidation resistance. For cost reasons, the upper limit is 0.20%.

[0324] Lanthanum improves oxidation resistance. For cost reasons, the upper limit is 0.20%.

[0325] Cerium improves oxidation resistance. For cost reasons, the upper limit is 0.20%.

[0326] Cerium mixed metal improves oxidation resistance. For cost reasons, the upper limit is 0.20%.

[0327] Niobium can be added as needed, as it also improves high temperature strength. Higher contents increase costs significantly. Therefore, the upper limit is set at 1.10%.

[0328] The alloy may also contain tantalum as required, as it also improves high temperature strength and oxidation resistance. Higher contents increase costs significantly. Therefore the upper limit is set at 0.60%. A minimum content of 0.001% is required to achieve the effect.

[0329] If desired, the alloy may also contain zirconium. Zirconium improves high temperature strength and oxidation resistance. For cost reasons, the upper limit is set at 0.20% zirconium.

[0330] If desired, the alloy may also contain hafnium. Hafnium improves high temperature strength and oxidation resistance. For cost reasons, the upper limit is set at 0.20% hafnium.

[0331] Boron can be added to the alloy as needed, since it improves creep strength. Therefore, a content of at least 0.0001% should be present. At the same time, this interface-active element deteriorates oxidation resistance. Therefore, a maximum of 0.008% boron is determined.

[0332] Up to 5.0% cobalt may be included in the alloy. Higher contents significantly reduce oxidation resistance.

[0333] Copper is limited to a maximum of 0.5% since this element reduces oxidation resistance.

[0334] Vanadium is limited to a maximum of 0.5% since this element reduces oxidation resistance.

[0335] Lead is limited to a maximum of 0.002% since this element reduces the oxidation resistance. The same applies to zinc and tin.

[0336] Too small a grain size of less than 30 μm leads to poor creep strength at higher temperatures. Too large a grain size of more than 600 μm leads to very low creep ductility at temperatures in the range of gamma prime formation.

[0337] Homogenization and / or stress reduction of welds of the same type by further annealing at temperatures between 980°C and 1250°C for 0.05 minutes to 24 hours, followed by cooling in static protective gas or air, moving (blowing) protective gas or air, improves the creep strength and creep ductility of the welds in the range of γ′ formation. At too low temperatures of 980°C or less, the temperature is too low to be able to carry out homogenization economically due to the long time required. At temperatures significantly higher than solution annealing, significant grain growth occurs, which reduces the high temperature strength at low temperatures and the elongation in creep tests in the range of γ′ formation. Even at very high temperatures, short times of less than 0.05 minutes are not sufficient. In particular, in the case of larger components, times longer than 24 hours are not economical.

[0338] Annealing under a protective gas reduces oxidation of the material during the annealing and thus reduces material loss. BRIEF DESCRIPTION OF THE DRAWINGS

[0339] Figure 1a : Left: A top view and a schematic cross-sectional view of a semi-finished profile sheet 1, a strip 2, a rod 3, a tube 4 and a wire or welding filler in the form of a wire 5. Right: An exemplary production of a component 7 by chamfering two sheets 1a, 1b and joining them by welding with a V-shaped seam 6a using a welding filler in the form of a wire 5.

[0340] Figure 1b: shows an exemplary production of a component 7, with the left side showing that two tubes are chamfered at the ends 4a, 4b and joined by welding with a V-shaped seam 6b using a welding filler 5 in the form of a wire. Center: a hole is milled in the sheet metal 1c and a tube 4c is inserted and joined by welding with a V-shaped seam 6c using a welding filler 5 in the form of a wire. Right side: two strip sections 2a, 2b processed to fit the edge are joined in a butt-joined manner by welding 6d using a portion of the edge as a welding filler 9.

[0341] Figure 2 It is shown that the following activities are observed in the presence of 37% CO, 9% H2O, 7% CO2, 46% H2 and c =163 and p(02)=2.5·10 -27 Metal loss due to "metal dusting" in a strongly carburizing gas as a function of the aluminum content and the chromium content (from Hermse, CGM and van Wortel, JC: Metal dus ting: relationship between alloy composition and degradation rate. Corrosion Engineering, Science and Technology 44 (2009), pp. 182-185).

[0342] Figure 3 The amount ratio of phases of Alloy 690 (N06690), taking batch 111389 as an example, depends on the temperature in thermodynamic equilibrium.

[0343] Figure 4 Taking Alloy 3 in Table 2 as an example, Alloy 693 (N06693) depends on the amount ratio of the phases in thermodynamic equilibrium depending on the temperature.

[0344] Figure 5 Taking Alloy 10 in Table 2 as an example, Alloy 693 (N06693) depends on the amount ratio of the phases in thermodynamic equilibrium at temperature.

[0345]

[0346]

[0347]

[0348]

[0349]

Claims

1. A method for producing a component, wherein the component is partially or completely produced from a semi-finished product of a nickel-chromium-aluminum alloy, wherein the alloy has (in mass %) more than 18% to 33% chromium, 1.8% to 4.0% aluminum, 0.01% to 7.0% iron, 0.001% to 0.50% silicon, 0.001% to 2.0% manganese, 0.00% to 0.60% titanium, 0.0% to 0.05% magnesium and / or calcium, respectively, 0.005% to 0.12% carbon, 0.0005% to 0.050% nitrogen, 0.0001% to 0.020% oxygen, 0.001% to 0.030% phosphorus, a maximum of 0.010% sulphur, molybdenum up to 2.0%, tungsten up to 2.0%, nickel balance greater than or equal to 50% and usual process-dependent impurities, wherein the component contains welds of the same type and / or the component is partially or completely provided with welds of the same type for installation in a system, wherein after welding, for homogenization of the welds and / or for stress reduction, only the welds of the same type and the heat-affected zones are subjected to annealing at between 980° C. and 1250° C. for a period of 0.05 minutes to 24 hours and subsequent cooling in static protective gas or air, in moving (blown) protective gas or air, as a result of which the creep strength and creep ductility of the welds are improved by this annealing, The following relationship must be satisfied: Cr+Al≥28(1a) and Fp≤39.9(2a) where Fp=Cr+0.272*Fe+2.36*Al+2.22*Si+2.48*Ti+0.374*Mo+0.538*W-11.8*C(3a) Wherein Cr, Fe, Al, Si, Ti, Mo, W and C are the concentrations of the elements in mass percentage.

2. The method according to claim 1, wherein the components contain welds of the same type and, after welding, for homogenizing the welds and / or for stress reduction, the entire component with the welds is subjected to annealing at temperatures between greater than 980 and 1250° C. for a period of 0.05 minutes to 24 hours, followed by cooling in a stationary protective gas or air, in a moving (blown) protective gas or in water, with the result that the creep strength and creep ductility of the welds are improved by this annealing.

3. The method according to claim 1 , wherein after the grinding process of the weld seam and the heat-affected zone, it is advantageous if a roughness value Ra of 0.01 to 15 μm is achieved, since this improves corrosion resistance and in particular improves “metal dusting” resistance and is raised almost to the value of the base material of the component.

4. The method according to one or more of claims 1 to 3, wherein the semi-finished product has a particle size of 30 to 600 μm.

5. The method according to one or more of claims 1 to 4, having a chromium content of 20 to 33%.

6. The method according to one or more of claims 1 to 5, having an aluminum content of 1.8 to 3.2%.

7. The method according to one or more of claims 1 to 6, having an iron content of 0.01 to 4.0%.

8. The method according to one or more of claims 1 to 7, with an additional content of niobium of 0.0 to 1.1% as required, wherein formula (43a) is supplemented with the term with Nb: Fp=Cr+0.272*Fe+2.36*Al+2.22*Si+2.48*Ti+1.26*Nb+0.374*Mo+0.538*W-11.8*C(3b) And Cr, Fe, Al, Si, Ti, Nb, Mo, W and C are the concentrations of the elements concerned in mass %.

9. The method according to one or more of claims 1 to 8, optionally with a zirconium content of 0.0 to 0.20%.

10. The method according to one or more of claims 1 to 9, optionally with an yttrium content of 0.001 to 0.20%.

11. The method according to one or more of claims 1 to 10, optionally with a lanthanum content of 0.001 to 0.20%.

12. The method according to one or more of claims 1 to 11, optionally with a cerium content of 0.001 to 0.20%.

13. The method according to one or more of claims 1 to 12, optionally with a cerium mixed metal content of 0.001 to 0.20%.

14. The method according to one or more of claims 1 to 13, optionally with a hafnium content of 0.001 to 0.20%.

15. The method according to one or more of claims 1 to 14, optionally with a tantalum content of 0.001 to 0.60%.

16. The method according to one or more of claims 1 to 15, optionally with a boron content of 0.0001 to 0.008%.

17. The process according to one or more of claims 1 to 16, optionally additionally containing 0.0 to 5.0% of cobalt.

18. The method according to one or more of claims 1 to 17, optionally additionally containing a maximum of 5.0% copper, wherein formula (4a) is supplemented with the term with Cu: Fp=Cr+0.272*Fe+2.36*Al+2.22*Si+2.48*Ti+0.477*Cu+0.374*Mo+0.538*W-11.8*C(3c) And Cr, Fe, Al, Si, Ti, Cu, Mo, W and C are the concentrations of the elements concerned in mass %.

19. Process according to one or more of claims 1 to 18, optionally additionally containing a maximum of 0.5% vanadium.

20. The method according to one or more of claims 1 to 19, wherein the impurities are adjusted to a content of max. 0.002% Pb, max. 0.002% Zn, max. 0.002% Sn.

21. Use of the process according to one or more of claims 1 to 20 in the petrochemical industry.