Copper foil for flexible printed circuit board, copper-clad laminate using same, flexible printed circuit board, and electronic device

By increasing the Cu content in the copper foil and performing heat treatment to ensure the uniformity of the crystal grain size, the problem of unstable bottom width of the copper circuit in the micro circuit is solved, the linearity and stability of the circuit are achieved, and the interference with adjacent circuits is reduced. risk of exposure.

CN118765335APending Publication Date: 2024-10-11JX NIPPON MINING & METALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023801.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-14
Filing Date
2023-03-15
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In micro circuits, the unstable bottom width of the copper circuit can easily lead to poor contact with adjacent circuits. The existing technology mainly focuses on the collapse problem of the top width of the circuit, but fails to effectively solve the stability of the bottom width.

Method used

By using copper foil with a Cu content of more than 99.96%, and performing EBSD measurement during heat treatment at 300°C x 30 minutes, ensuring that the standard deviation of the crystal grain size is less than 3.0 μm, combined with 10 to 50 ppm of P added elements, the copper foil is optimized. Metal structure uniformity and thus the linearity of the circuit during the etching process.

Benefits of technology

It achieves good linearity of the circuit and is suitable for flexible printed circuit boards with fine circuits. It reduces the unevenness of the bottom width and reduces the risk of contact with adjacent circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765335A_ABST
    Figure CN118765335A_ABST
Patent Text Reader

Abstract

[Problem] To provide: a copper foil for a flexible printed circuit board, which has good circuit linearity and is suitable for a fine circuit; a copper-clad laminate using the copper foil; a flexible printed circuit board; and an electronic device. [Solution] A copper foil for a flexible printed circuit board, which is a rolled copper foil containing 99.96% by mass or more of Cu with the balance made up of unavoidable impurities, and which is characterized in that the rolled copper foil is subjected to a heat treatment at 300 DEG C for 30 minutes, and the measurement field of view of 150 [mu] m * 150 [mu] m of the rolled surface of the rolled copper foil is subjected to EBSD measurement. The standard deviation of the crystal grain size is 3.0 [mu] m or less when the orientation difference is regarded as the grain boundary of 5 DEG or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a copper foil suitable for use in wiring members such as a flexible printed circuit board, a copper-clad laminate using the same, a flexible wiring board, and an electronic device. Background Art

[0002] As a circuit substrate for electronic devices, a flexible printed circuit board (flexible wiring board, hereinafter referred to as "FPC") is widely used. FPC is formed by etching a copper clad laminate (hereinafter referred to as CCL) formed by laminating copper foil and resin to form wiring, and then covering it with a resin layer called a cover layer. The resin bonded to the CCL may be polyimide, liquid crystal polymer, PTFE, but is not limited thereto.

[0003] In addition, in this way, the copper-clad laminate undergoes an etching process to remove unnecessary portions of the copper layer by applying a resist and exposing the printed circuit to form the target circuit. However, there is a problem that when the circuit is formed by etching, the circuit will not become as wide as the shielding pattern pre-formed on the surface.

[0004] This is because the copper circuit formed by etching is etched gradually from the surface of the copper layer downward, that is, toward the resin layer (causing collapse).

[0005] Therefore, a technology for reducing this "collapse" is being developed (Patent Document 1).

[0006] [Prior Technical Literature]

[0007] [Patent Document]

[0008] [Patent Document 1]: Japanese Patent Application Publication No. 2011-216528. Summary of the invention

[0009] [Problems to be solved by the invention]

[0010] As electronic devices become smaller, thinner, and more high-performance, high-density FPC packaging is required. In order to package FPCs at a high density, the circuit needs to be miniaturized, but in order to maintain impedance integrity in a miniaturized circuit, it is important that the circuit width is fixed to the entire circuit. The reason is that if the circuit width is not fixed to the entire circuit, the circuit will be close to (contact) the adjacent circuit, and there is a risk of failure.

[0011] Furthermore, as described above, since the circuit width tends to spread on the resin layer side (bottom side), the bottom side is more likely to come into contact with the adjacent circuit, and it becomes more important to keep the circuit width (bottom width) on the bottom side constant in the entire circuit. This defect is more likely to occur in the case of a fine circuit with a bottom width of 35 μm or less.

[0012] However, as described in the above-mentioned Patent Document 1, although a technique for reducing the difference between the top width and the bottom width of a circuit (collapse) is disclosed, no technique focusing on the bottom width is found.

[0013] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a copper foil for a flexible printed circuit board which has excellent circuit linearity and is suitable for a fine circuit, a copper-clad laminate using the same, a flexible printed circuit board, and an electronic device.

[0014] [Technical means to solve the problem]

[0015] The inventors of the present invention have conducted various studies and found that in order to improve the linearity of the circuit formed by etching copper foil, it is important that the metal structure of the copper foil is close to uniform, in other words, the grain size is uniform (the standard deviation of the crystal grain size is small). This is believed to be because if the standard deviation of the crystal grain size is small, the chemical reaction (etching reaction) during circuit formation caused by etching occurs uniformly.

[0016] That is, the copper foil for a flexible printed circuit board of the present invention is a rolled copper foil containing 99.96 mass % or more of Cu, with the remainder being composed of inevitable impurities, and when subjected to a heat treatment at 300° C. for 30 minutes, an EBSD measurement is performed on a measurement field of 150 μm×150 μm on the rolled surface of the rolled copper foil, and the standard deviation of the crystal grain size when an orientation difference of 5° or more is regarded as a grain boundary is 3.0 μm or less.

[0017] The copper foil for a flexible printed circuit board of the present invention is preferably made of refined copper specified in JIS-H3100 (C1100) or oxygen-free copper specified in JIS-H3100 (C1020).

[0018] The copper foil for a flexible printed circuit board of the present invention preferably contains 10 to 50 mass ppm of P.

[0019] The copper-clad laminate of the present invention is obtained by laminating the above-mentioned copper foil for a flexible printed circuit board and a resin layer.

[0020] The flexible printed circuit board of the present invention is formed by forming a circuit in the copper foil in the copper-clad laminate.

[0021] The electronic device of the present invention is obtained by using the above-mentioned flexible printed circuit board.

[0022] [Effects of the Invention]

[0023] According to the present invention, a copper foil for a flexible printed circuit board which has excellent circuit linearity and is suitable for a fine circuit can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] [ Figure 1 ] is a view showing the bottom width w of the circuit formed by etching.

[0025] [ Figure 2 ] is a top view showing a method of measuring the bottom width w of a circuit multiple times.

[0026] [ Figure 3 ] is a view showing an exposure mask used for etching to form a straight line circuit when evaluating the linearity of the circuit.

[0027] [ Figure 4 ] is a schematic diagram showing the state of etching progress in a straight line circuit.

[0028] [ Figure 5 ] is a schematic diagram showing the mechanism of reduced circuit linearity when the metal structure is uneven (the grain size is inconsistent). DETAILED DESCRIPTION

[0029] Hereinafter, an embodiment of the copper foil of the present invention will be described. In addition, in the present invention, % represents mass % unless otherwise specified.

[0030] <Composition>

[0031] The copper foil of the present invention contains 99.96% by mass or more of Cu, and the remainder is composed of inevitable impurities. It is preferred to contain 10 to 50 ppm by mass of P as an additive element. Here, if Cu is in the range of 99.96% by mass or more, in order to improve the mechanical properties of the copper foil, the copper foil may also contain trace amounts of Ag, Sn, Zr, etc.

[0032] If P is contained as an additive element, the metal structure (grain size) tends to become uniform and the bottom width of the circuit after etching tends to become constant. However, if the P content exceeds 50 mass ppm (0.005 mass%), the conductivity decreases and it is not suitable for flexible printed circuit boards.

[0033] The copper foil of the present invention may be made of refined copper specified in JIS-H3100 (C1100) or oxygen-free copper of JIS-H3100 (C1020), or oxygen-free copper or refined copper containing trace amounts of Ag, Sn, Zr, etc., and these compositions may contain 10 to 50 mass ppm of P as an additive element.

[0034] The analysis of phosphorus concentration was carried out by using the phosphorus molybdic acid blue absorption measurement method using phosphorus molybdic acid extraction specified in JIS H 1058 (phosphoquantitative method for phosphorus in copper and copper alloys) (P concentration: applicable to 0.0005% to 0.01%).

[0035] <Standard Deviation of Crystal Grain Size>

[0036] When the rolled copper foil was heat treated at 300°C for 30 minutes, EBSD measurement was performed on the rolled surface after the heat treatment with a measurement field of 150 μm×150 μm. The standard deviation of the grain size when the orientation difference of 5° or more was regarded as the grain boundary was 3.0 μm or less.

[0037] The standard deviation of the crystal grain size is calculated by crystal orientation analysis in EBSD (Electron Back Scatter Diffraction) measurement.

[0038] The actual measurement was carried out by electrolytically polishing the sample surface and then observing it using SEM-EBSD (JSM-IT500HR, TSL EDAX SCAN GENERATOR-II, TSL OIM DATA COLECTION 7, JEOL Ltd.) under the following conditions.

[0039] In addition, EBSD measurement may be performed on a sample plate (150 mm×150 mm) cut out from the copper foil after the heat treatment.

[0040] WD: 15.0mm or 16.0mm

[0041] Camera elevation angle: 2.7 degrees

[0042] Sample tilt angle: 70.0 degrees

[0043] Camera azimuth: 0.0 degrees

[0044] Accelerating voltage: 15.0 kV

[0045] Probe current: 9.5nA

[0046] SS-CCD camera: 8×8 grid

[0047] Gain: 300-350 (Pattern brightness: 0.90-0.95)

[0048] Exposure time: 4ms

[0049] Background integration count: 20 times

[0050] Observation magnification: 600 times

[0051] Observation field: 150μm×150μm

[0052] ·Step width: 0.5μm

[0053] Scanning pattern: Hexagonal grid

[0054] Phase list: Copper

[0055] The analysis of the obtained measurement data was performed using OIM Analysis Ver8.0 x64Advancedpackage under the following conditions.

[0056] ·Perform Crean Up using the grain expansion method once (grain tolerance angle: 5, minimum grain size: 2 points, multiple rows: 1, iteration score: 0.25)

[0057] · Grains at the edge of the EBSD image are not calculated

[0058] · Calculate the average and standard deviation of the grain size (Diameter) using the Number method (a method that simply divides the total area to be calculated by the number of grains)

[0059] The Number method is different from the cutting method in that it determines the grain size by simply dividing the total area to be calculated by the number of grains by considering the grain boundaries with an orientation difference of 5° or more.

[0060] It is considered that when the standard deviation of the crystal grain size is 3.0 μm or less, the metal structure of the copper foil becomes nearly uniform (the crystal grain size is uniform), and a chemical reaction (etching reaction) during circuit formation by etching occurs uniformly.

[0061] <Circuit Linearity>

[0062] After the copper foil was surface treated, a sample plate (150 mm × 150 mm) was cut out and heat treated to form a copper-clad laminate. A straight line circuit was formed from the copper foil side of the copper-clad laminate under the following etching conditions (refer to Figure 2 ), when the bottom width w of the circuit is measured multiple times, it is preferred that σ / Aw represented by the standard deviation σ(μm) of the bottom width w(μm) and the average value Aw(μm) of the bottom width w is less than 0.03. The reason for this is that if σ / Aw is less than 0.03, it is empirically known that there is a tendency for the circuit to have excellent linearity.

[0063] Etching conditions:

[0064] Etching solution composition: CuCl 2 -2H 2O=3 mol / L (specific gravity 1.24), HCl=4 mol / L, liquid temperature=50°C, etching liquid spray pressure=0.22 MPa, the rolled copper foil that shields the circuit portion is etched to form a circuit.

[0065] σ / Aw is calculated by measuring the actual bottom width w of the circuit formed by etching multiple times (preferably 10 or more locations, more preferably 50 locations, and even more preferably 100 locations per 30 μm in the long side direction of the circuit) to obtain σ and Aw.

[0066] Specifically, if Figure 1 As shown, the circuits 21 and 22 formed by etching the copper foil are extended from the surface toward the bottom (resin layer 4 side (bottom side)), and the circuit width (bottom width) w on the bottom side is measured multiple times. Here, the symbol wt is the circuit width (top width) on the surface (top) side.

[0067] In addition, if Figure 2 As shown, the circuits 21 and 22 can be measured at specific measurement points, such as 50 locations of the circuit widths w1, w2, w100, w101, w102, w200, etc. Alternatively, the measurement can be performed on one circuit.

[0068] When σ / Aw is less than 0.03, the variation in the bottom width w is small, indicating excellent circuit linearity. In particular, it is preferred that the bottom width w is in the range of 10 to 35 μm, and the circuit linearity is also excellent.

[0069] The shielding of the circuit portion of the copper foil can be formed by, for example, using a known method of using a photoresist (dry film resist, etc.) to leave the resist only on the portion remaining as the circuit through a mask. As a dry film resist, for example, RY-5107 (thickness 7 μm) manufactured by Hitachi Chemical can be used.

[0070] Here, Figure 3 This indicates the exposure mask used to etch a straight line circuit when evaluating the linearity of the circuit. There are 10 types of resist / space patterns for the exposure mask, and they are Figure 3 The design is that the space is wider on the left side (number 10 side) and narrower on the right side. After all patterns are sequentially exposed, developed, etched, and dry film stripped, a circuit close to the target L / S (L / S = 10 / 40 to 30 / 20) is selected from all patterns using SEM for evaluation.

[0071] The thickness of the copper foil is preferably 17 μm or less in terms of the nominal thickness specified in JIS C 6515. The thinner the thickness, the less stress is applied to the copper foil, which helps improve the bendability and also helps to make portable devices smaller, thinner, and lighter.

[0072] <Manufacturing>

[0073] The copper foil of the present invention can be produced, for example, as follows: First, P is added to a copper ingot as necessary, and the ingot is melted and cast, followed by hot rolling, cold rolling, and annealing to produce a foil.

[0074] Here, intermediate annealing at a predetermined cooling rate may be performed during cold rolling, oxide scale generated during intermediate annealing may be removed, intermediate cold rolling may be performed, and then final annealing and final cold rolling may be performed to obtain a foil having a target final thickness.

[0075] The maximum temperature of the intermediate annealing can be 350 to 500° C. The cooling rate of the intermediate annealing is preferably 50 to 150° C. / h from the maximum temperature TM (° C.) in the intermediate annealing to a temperature of (TM-200)° C.

[0076] As described above, if the cooling rate of the intermediate annealing is set to 50 to 150°C / h, the cooling rate becomes slower than the general conditions. Moreover, the slower the cooling rate of the intermediate annealing, the smaller the temperature gradient in the material (the temperature difference between the first cooled part and the last cooled part becomes smaller), thereby making the metal structure more uniform (the grain size is uniform), and the standard deviation of the grain size when the foil of the final thickness is heat treated becomes smaller. As a result, it is believed that the chemical reaction (etching reaction) during the circuit formation caused by etching occurs uniformly, so the circuit linearity is improved.

[0077] Figure 4 , Figure 5 This is a mechanism that indicates that the more uniform the metal structure (the more uniform the grain size), the better the circuit linearity.

[0078] like Figure 4 As shown in the figure, etching is the process of the etching liquid penetrating into the copper foil from the part without resist (equivalent to the space between the straight lines) and expanding, while etching is the process of expanding from the space to the left and right of the copper foil. Figure 1 As shown, etching (circuit) spreads from the surface toward the bottom (resin layer side (bottom side)).

[0079] Here, if Figure 5 As shown in (a), when the metal structure is not uniform (the grain size is not uniform), Figure 1 The bottom width w of the circuits 21 and 22 shown in FIG. Figure 5 In (a), the edges of the circuits 21 and 22 are not straight lines but are curved in an undulating manner).

[0080] The reason is believed to be Figure 5As shown in (b), for example, within a field of view of 150μm×150μm, if the grains of the copper foil on the circuit 21 side are large and the grains of the copper foil on the circuit 22 side are small, the metal structure is not uniform (the grain sizes are inconsistent), and the etching speed on the circuit 21 side with large grains increases, and the etching amount changes between the parts with small grains, and even the unevenness of the bottom width w increases.

[0081] In addition, Figure 5 In (b), since the etching rates in the crystal grains and the crystal grain boundaries are different, if the crystal grain sizes are not uniform, the etching rate will vary greatly locally. In addition, in the etching solution of this test, the etching rate of the crystal grain boundaries is slower than that of the crystal grains, but the opposite situation also exists.

[0082] <Copper-clad laminate and flexible printed circuit board>

[0083] In addition, for the copper foil of the present invention, for example, (1) a resin precursor (for example, a polyimide precursor called varnish) is cast and heat is applied to polymerize it and (2) a base film is laminated to the copper foil of the present invention using a thermoplastic adhesive of the same type as the base film, thereby obtaining a copper-clad laminate (CCL) consisting of two layers of copper foil and a resin substrate. In addition, by laminating a base film coated with an adhesive to the copper foil of the present invention, a copper-clad laminate (CCL) consisting of three layers of copper foil, a resin substrate and an adhesive layer therebetween can be obtained. When manufacturing these CCLs, the copper foil is heat-treated and recrystallized.

[0084] A circuit is formed on these using a photolithography technique, and the circuit is plated as necessary, followed by laminating a coverlay film, thereby obtaining a flexible printed circuit board (flexible wiring board).

[0085] Therefore, the copper-clad laminate of the present invention is formed by laminating a copper foil and a resin layer. In addition, the flexible printed circuit board of the present invention is formed by forming a circuit on the copper foil of the copper-clad laminate.

[0086] The resin layer may be PET (polyethylene terephthalate), PI (polyimide), LCP (liquid crystal polymer), or PEN (polyethylene naphthalate), but is not limited thereto. In addition, these resin films may be used as the resin layer.

[0087] As a lamination method of the resin layer and the copper foil, the material to be the resin layer can be applied to the surface of the copper foil and heated to form a film. In addition, a resin film can be used as the resin layer, and the following adhesive can be used between the resin film and the copper foil, or the resin film can be hot-pressed to the copper foil without using an adhesive. However, it is preferable to use an adhesive in order not to apply excess heat to the resin film.

[0088] When a film is used as a resin layer, the film can be laminated to a copper foil via an adhesive layer. In this case, an adhesive having the same composition as the film is preferably used. For example, when a polyimide film is used as a resin layer, a polyimide adhesive is also preferably used for the adhesive layer. In addition, the polyimide adhesive referred to herein refers to an adhesive containing an imide bond, and also includes polyetherimide, etc.

[0089] The present invention is not limited to the above-described embodiment. The copper alloy in the above-described embodiment may contain other components as long as the effects of the present invention are exhibited.

[0090] For example, the copper foil surface may be subjected to a surface treatment such as a roughening treatment, a rust-proof treatment, a heat-resistant treatment, or a combination of these treatments.

[0091] [Example]

[0092] Next, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0093] Ingots are made using electrolytic copper in a non-oxidizing environment. The proportion of copper contained in the ingot is 99.96% by mass or more. After the ingot is homogenized and annealed at above 900°C, hot rolling and cold rolling are performed. During the cold rolling, an intermediate annealing with a maximum temperature of 400°C is performed, and the cooling rate of the intermediate annealing is set to the value in Table 1, and the temperature is cooled to 200°C lower than the maximum temperature. The cooling rate of the embodiment is estimated based on the measured data of the material temperature when annealing a material different from the embodiment. After removing the oxide scale generated during the intermediate annealing and performing intermediate cold rolling, the final annealing and final cold rolling are performed to obtain a foil with a target final thickness of 12μm. In addition, for the comparative example, the cooling rate of the intermediate annealing to a temperature 200°C lower than the maximum temperature is obtained by heat transfer simulation and recorded in Table 1.

[0094] The obtained foil was subjected to a heat treatment of 300°C for 30 minutes in an atmospheric environment to obtain a copper foil sample. Specifically, in order to prevent oxidation, the copper foil sample was sandwiched between two C7025 plates of 30 mm in width, 130 mm in length, and 0.15 mm in thickness. After packaging with A4-sized annealed C1100, the door of a high-temperature hot air dryer at 300°C was opened and put in. After 30 minutes, the door was opened for recovery and the copper foil sample was taken out. The heat-treated copper foil simulates the state of heat treatment during the lamination of CCL. After the rolled surface of the heat-treated copper foil was electrolytically polished, the EBSD measurement was performed on the measurement field of 150μm×150μm to obtain the standard deviation of the grain size when the orientation difference of 5° or more was regarded as the grain boundary. The conditions for the EBSD measurement are as described above.

[0095] In addition, after the foil obtained by the final cold rolling was surface treated, 25 μm of Upilex VT (manufactured by Ube Industries, Ltd.) was laminated, and after heat treatment at 300°C × 30 minutes using a heating press to form a copper-clad laminate, the circuit part of the copper foil was masked by photoetching using a dry film resist (product name RY-5107 manufactured by Hitachi Chemical, thickness 7 μm), and dry film patterning with a L+S pitch of 50 μm was performed. The development, etching and stripping of the resist were performed using the "Development, Etching and Stripping Production Line" (device name: DERM) of SunTechno System Co., Ltd. The etching conditions are as described in the above "<Circuit Linearity>".

[0096] <Evaluation of Circuit Linearity>

[0097] The above etching conditions were actually measured, and the etching time was changed in a manner close to the target L / S (L / S = 10 / 40 to 30 / 20) for each embodiment and each comparative example, and the conditions were set. As a result, the average value Aw of the bottom width w became the value shown in Table 1. The average value Aw represents L of L / S. In addition, "50μm-average value Aw" represents S of L / S. For each embodiment and each comparative example, the bottom width w of each circuit was set as shown in Table 1. Figure 2 50 points were measured as shown, and the average value Aw was calculated.

[0098] In addition, each example changes the etching time within the range of 36 to 54 seconds for the same copper foil. Similarly, each comparative example changes the etching time within the range of 36 to 54 seconds for the same copper foil.

[0099] The obtained results are shown in Table 1. Here, the P concentrations of Examples 1 to 7 were in the range of 10 to 50 mass ppm, and the P concentrations of Comparative Examples 1 to 7 were less than 10 ppm. The P concentration was analyzed by the above-mentioned method.

[0100] [Table 1]

[0101]

[0102] A flexible printed circuit board was produced using the copper foil of the example having a standard deviation of crystal grain size of 3.0 μm or less. The results showed that σ / Aw was less than 0.03, and almost no contact with adjacent circuits was observed, indicating excellent circuit linearity.

[0103] On the other hand, when a flexible printed circuit board was produced using the copper foil of the comparative example having a standard deviation of crystal grain size exceeding 3.0 μm, σ / Aw was 0.03 or more, contact with adjacent circuits was seen everywhere, and the circuit linearity was poor.

Claims

1. A copper foil for a flexible printed circuit board, wherein the copper foil for a flexible printed circuit board is a rolled copper foil containing 99.96% by mass or more of Cu, the remainder of which is composed of inevitable impurities, When the rolled copper foil was heat treated at 300°C for 30 minutes, EBSD measurement was performed on the rolled surface of the rolled copper foil in a measurement field of 150 μm×150 μm. The standard deviation of the grain size when the orientation difference of 5° or more was regarded as the grain boundary was 3.0 μm or less. 2 . The copper foil for a flexible printed circuit board according to claim 1 , wherein the copper foil for a flexible printed circuit board is made of refined copper specified in JIS-H3100 (C1100) or oxygen-free copper specified in JIS-H3100 (C1020). 3 . The copper foil for a flexible printed circuit board according to claim 1 , wherein the copper foil for a flexible printed circuit board contains 10 to 50 mass ppm of P. 4 . A copper-clad laminate, comprising laminating the rolled copper foil for a flexible printed substrate according to claim 1 and a resin layer.