MXene-based sugar-containing nano material and preparation method thereof

By modifying MXene and grafting chondroitin sulfate oligosaccharides, combined with chondroitin sulfate signaling pathway and photothermal therapy, the heterogeneity problem of existing chondroitin sulfate nanomaterials in tumor and inflammation treatment is solved, achieving more effective tumor ablation and inflammation treatment effects, and expanded neural differentiation applications.

CN118767133APending Publication Date: 2024-10-15JIANGNAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410832835.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing chondroitin sulfate nanomaterials have heterogeneous problems such as large differences in molecular weight and varying degrees of sulfation modification in the fields of regulating tumor treatment, inflammatory response, nervous system development, and injury repair. A single signaling pathway is not effective in treating tumors and inflammation. Not good.

Method used

Modify MXene by selecting appropriate acid etchants and aminosilane reagents, graft chondroitin sulfate oligosaccharides of different sizes and subtypes, prepare MXene-based sugar-containing nanomaterials, and combine chondroitin sulfate signaling pathways and photothermal therapy , to achieve the synergistic effect of tumor treatment, inflammation treatment and neural stem cell differentiation.

Benefits of technology

It enhances the binding ability of chondroitin sulfate to protein receptors, expands the functional applications of MXene, provides more effective tumor ablation, inflammation treatment and neural differentiation effects, and improves biocompatibility and drug delivery efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767133A_ABST
    Figure CN118767133A_ABST
Patent Text Reader

Abstract

The invention relates to an MXene-based sugar-containing nano material and a preparation method thereof, and belongs to the technical field of biology. The preparation method comprises the following steps: S1, reacting MXene with an amino silane reagent in a solvent, and carrying out centrifugal washing and drying to obtain an aminated MXene nano material; the method comprises the following steps: carrying out enzymolysis on chondroitin sulfate by adopting chondroitin sulfatase, and carrying out ultrafiltration to obtain chondroitin sulfate oligosaccharide; s2, enabling the aminated MXene nano material, chondroitin sulfate oligosaccharide and an amide cross-linking agent to react, dialyzing and freeze-drying to obtain the MXene-based sugar-containing nano material. According to the MXene-based sugar-containing nano material, combination between chondroitin sulfate oligosaccharide and various protein receptors is amplified, so that chondroitin sulfate mediated signal channel regulation and photo-thermal synergistic treatment of tumors and inflammations, neural differentiation promotion and the like are achieved, the function and application of MXene are expanded, and the MXene-based sugar-containing nano material has good application prospects in the biomedical field and the chemical industry field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of biotechnology, and in particular relates to a MXene-based sugar-containing nanomaterial and a preparation method thereof. Background Art

[0002] Chondroitin sulfate (CS) is a sulfated glycosaminoglycan that participates in a variety of biological functions, including tumor therapy, inflammatory response, nervous system development, and injury repair. Its sugar chain is composed of 1,4-linked N-acetyl-β-D-galactosamine (β-D-GalNAc) and 1,3-linked β-D-glucuronic acid (β-D-GlcA) repeating disaccharide units. Chondroitin sulfate sugar chains and sulfated derivatives modified at different sites can bind to a variety of cell surface receptors, growth factors / cytokines, etc., thereby regulating a variety of biological phenomena, such as tumor proliferation and apoptosis, immune response, nervous system development, and pathological processes. For example, chondroitin sulfate sugar chains in the extracellular matrix of tumor cells interact with growth factors to store or release them into the extracellular matrix, thereby promoting a variety of intracellular signal transductions. Glycosaminoglycans and molecules based on glycosaminoglycans are considered to be potential anticancer drugs. At the same time, chondroitin sulfate on proteoglycans is an important regulator of inflammatory response. It promotes the movement of leukocytes along the endothelial surface of the inflammatory site, thereby participating in the guidance, migration and activation of leukocytes. In addition, in the central nervous system, chondroitin sulfate sugar chains transmit signals to neurons by interacting with a variety of protein receptors, including heparin-binding growth factors such as midkine (MK), fibroblast growth factor (FGF), pleiotrophin (PTN), etc., thereby participating in the formation of neural networks and axon growth and regeneration in the central nervous system. However, the existing chondroitin sulfate nanomaterials still have many shortcomings in the research on the regulation of tumor treatment, inflammatory response, nervous system development and injury repair: natural macromolecular CS polysaccharides are limited by factors such as animal species and environmental changes, and there are heterogeneity problems such as large molecular weight differences and different degrees of sulfation modification. The single chondroitin sulfate-mediated signaling pathway is not effective in treating tumors, inflammation, etc. Summary of the invention

[0003] In order to solve the above technical problems, the present invention provides a MXene-based sugar-containing nanomaterial and a preparation method thereof. First, a single-layer MXene (TiO2) is obtained by selecting an acid etchant, adjusting reaction temperature and time, and the like. 3 C 2 ). Considering the grafting of chondroitin sulfate oligosaccharides on MXene (Ti 3 C 2), a certain degree of freedom is required, and aminosilane reagents are selected to covalently modify MXene. The amino groups are introduced into the MXene surface through the dehydration condensation of the alkoxy groups in the aminosilane reagent, and its hydrophilicity and biocompatibility are increased. Finally, chondroitin sulfate oligosaccharides of different sizes and subtypes are grafted through an amidation reaction to prepare MXene-based sugar-containing nanomaterials. Through the synergy of the chondroitin sulfate signaling pathway and the photothermal therapy of MXene, it can be widely used in the fields of tumor treatment, inflammation treatment, neural stem cell differentiation, etc.

[0004] The first object of the present invention is to provide a method for preparing a MXene-based sugar-containing nanomaterial, comprising the following steps:

[0005] S1, MXene and aminosilane reagent react in a solvent, and the amino MXene nanomaterial is obtained by centrifugal washing and drying;

[0006] Chondroitin sulfate is enzymatically hydrolyzed by chondroitinase, and chondroitin sulfate oligosaccharide is obtained by ultrafiltration;

[0007] The amino-modified MXene nanomaterials described in S2 and S1, the chondroitin sulfate oligosaccharides described in S1 and the amide cross-linking agent are reacted, and the MXene-based sugar-containing nanomaterials are obtained through dialysis and freeze-drying.

[0008] In one embodiment of the present invention, in S1, the potential of the MXene is -10mV to -40mV, the particle size is 100nm-600nm, the thickness is 1nm-5nm, and the number of layers is a single layer; the particle size of the amino MXene nanomaterial is 100nm-800nm.

[0009] In one embodiment of the present invention, in S1, the MXene is obtained by etching MAX with an acid etchant; the acid etchant is obtained by mixing water, HCl and LiF in a volume ratio of (5-10):(2-5):(0.1-0.4), and the etching is carried out at 40°C-50°C for 36h-48h.

[0010] In one embodiment of the present invention, in S1, the aminosilane reagent is selected from one or more of 3-aminopropyltrimethoxysilane (APTS), 3-aminopropyltriethoxysilane (APTES) and 3-(2-aminoethylamino)propyltrimethoxysilane (AEAPTS).

[0011] In one embodiment of the present invention, in S1, the solvent is selected from ethanol and / or water.

[0012] In one embodiment of the present invention, in S1, the mass ratio of the MXene to the aminosilane reagent is (0.01-2):1.

[0013] In one embodiment of the present invention, in S1, the rotation speed of the centrifugal washing is 3500 rpm-6000 rpm, the time is 1 min-15 min, and the reagent is selected from ethanol and / or water.

[0014] In one embodiment of the present invention, in S1, the drying is performed at 25°C-60°C for 4h-48h.

[0015] In one embodiment of the present invention, in S1, the chondroitinase is selected from chondroitin sulfate lyase AC (ChAC) or chondroitin sulfate lyase ABC (ChABC); the chondroitin sulfate is selected from one or more of chondroitin sulfate A, chondroitin sulfate C and chondroitin sulfate E.

[0016] In one embodiment of the present invention, in S1, during the enzymatic hydrolysis process, the concentration of chondroitinase is 5 μg / mL-20 μg / mL, and the concentration of chondroitin sulfate is 1 mg / mL-5 mg / mL; the conditions of the enzymatic hydrolysis are: temperature of 20°C-40°C, and time of 20h-30h.

[0017] In one embodiment of the present invention, in S1, the molecular weight of the chondroitin sulfate oligosaccharide is less than 3 KDa.

[0018] In one embodiment of the present invention, in S2, the amide cross-linking agent includes EDC and NHS; the mass ratio of EDC to NHS is 1:(1.5-3).

[0019] In one embodiment of the present invention, the mass ratio of the amino MXene nanomaterial, chondroitin sulfate oligosaccharide and amide cross-linker is (2-10):(1-5):(1-5).

[0020] The second object of the present invention is to provide a MXene-based sugar-containing nanomaterial prepared by the method described, wherein the particle size of the MXene-based sugar-containing nanomaterial is 100nm-900nm.

[0021] The technical solution of the present invention has the following advantages over the prior art:

[0022] (1) The monolayer MXene (TiO2) used in the MXene-based sugar-containing nanomaterial of the present invention 3 C 2), the surface contains -OH, -O or -F groups, which give MXene excellent hydrophilicity, facilitating surface functional modification; MXene exhibits efficient light absorption and heat conversion capabilities in photothermal therapy, and MXene has a large specific surface area, which can provide abundant anchoring sites and accommodate high-density sugar ligands to enhance sugar molecule-mediated interactions, making it a very suitable photothermal therapy material for drug delivery. After the MXene of this application is modified with chondroitin sulfate oligosaccharides, its photothermal effect can still meet the requirements of tumor ablation and inflammation treatment.

[0023] (2) The MXene-based sugar-containing nanomaterials described in the present invention amplify the binding between chondroitin sulfate oligosaccharides and various protein receptors to exert chondroitin sulfate-mediated signal pathway regulation and photothermal synergistic treatment of tumors, inflammation, and promote neural differentiation, etc. The functions and applications of MXene have been expanded, and it has good application prospects in the biomedical and chemical fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0025] Figure 1 This is the potential diagram of MXene of Test Example 1 of the present invention;

[0026] Figure 2 It is a transmission electron microscope (TEM) image of test example 2 of the present invention; wherein, the left image is a TEM image of MXene, the middle image is a TEM image of an amino-modified MXene nanomaterial, and the right image is a TEM image of a MXene-based sugar-containing nanomaterial;

[0027] Figure 3 This is an atomic force microscope (AFM) image of MXene of Test Example 3 of the present invention; wherein the left image is an AFM image of MXene, and the right image is a thickness image of MXene;

[0028] Figure 4 The X-ray diffraction patterns (XRD) of MXene and MAX of Example 1 in Test Example 4 of the present invention; wherein the left figure is the XRD pattern of MAX, and the right figure is the XRD pattern of MXene;

[0029] Figure 5 The X-ray diffraction pattern (XRD) of MXene of comparative example 1 of test example 4 of the present invention;

[0030] Figure 6 The X-ray diffraction pattern (XRD) of MXene of Comparative Example 2 of Test Example 4 of the present invention;

[0031] Figure 7The X-ray diffraction pattern (XRD) of MXene of comparative example 3 of test example 4 of the present invention;

[0032] Figure 8 This is the X-ray photoelectron spectrum (XPS) of Test Example 5 of the present invention; wherein the left figure is the XPS figure of the amino-modified MXene nanomaterial, and the right figure is the XPS figure of MXene;

[0033] Fig. 9 This is the near-infrared photothermal response diagram of MXene in Test Example 6 of the present invention; the upper left is 1W / cm 2 Temperature variation of MXene solutions with different concentrations over time under different power levels, with 1W / cm2 on the upper right 2 Near-infrared thermal imaging of MXene solutions with different concentrations under different powers. The lower left is a graph showing the temperature change of MXene solutions over time under different powers. The lower right is a graph showing the near-infrared thermal imaging of MXene solutions under different powers.

[0034] Fig.10 Thermogravimetric graphs (TGA) of MXene, amino-modified MXene nanomaterials, and MXene-based sugar-containing nanomaterials of Test Example 7 of the present invention;

[0035] Fig.11 This is the near-infrared photothermal response diagram of the MXene-based sugar-containing nanomaterial of Test Example 8 of the present invention; the upper left is 1 W / cm 2 Temperature variation of MXene-based sugar-containing nanomaterial solutions with different concentrations over time under different power levels. The upper right figure is 1W / cm 2 Near-infrared thermal imaging of MXene-based sugar-containing nanomaterial solutions with different concentrations under different powers. The lower left is a graph showing the temperature change of MXene-based sugar-containing nanomaterial solutions over time under different power conditions. The lower right is a graph showing the near-infrared thermal imaging of MXene-based sugar-containing nanomaterial solutions under different power conditions.

[0036] Fig.12 This is a cytotoxicity diagram of the MXene-based sugar-containing nanomaterial of Test Example 9 of the present invention. DETAILED DESCRIPTION

[0037] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. It should be understood that the specific embodiments are only used to explain the present invention, but the embodiments are not intended to limit the present invention.

[0038] In the present invention, unless otherwise explained, technical and scientific terms used in the present invention have the same meanings as commonly understood by those skilled in the art to which the present invention belongs.

[0039] In the present invention, unless otherwise stated, the term "and / or" used in the present invention includes any and all combinations of one or more of the associated listed items.

[0040] In the present invention, unless otherwise stated, the experimental methods used in the embodiments of the present invention are conventional methods unless otherwise stated, and the materials, reagents, etc. used are all commercially available unless otherwise stated.

[0041] Example 1

[0042] The MXene-based sugar-containing nanomaterial and the preparation method thereof of this embodiment specifically include the following steps:

[0043] S1. Preparation of MXene solution: 2.5 mL of deionized water, 7.5 mL of 12 M HCl solution, and 800 mg of LiF were added to a polytetrafluoroethylene beaker in sequence, and stirred at room temperature for 30 min to obtain an acid etchant. 500 mg of MAX(TiO2) was then slowly added to the acid etchant. 3 AlC 2 ), 40 ° C for 48h; after the reaction, the reaction was centrifuged with deionized water at a speed of 5000 rpm for 3 min each time, and a total of 5 centrifugal washes were performed until the pH of the supernatant was > 6, and then ultrasonicated for 1.0h, and continued to centrifuge at a speed of 3500 rpm for 15min to obtain MXene (Ti 3 C 2 ) and store the supernatant at -20°C.

[0044] S2. Preparation of amino MXene nanomaterials: Move the MXene solution from -20°C to room temperature, add deionized water, prepare 10mL 5mg / mL MXene solution, add 100mL anhydrous ethanol and 0.05mL APTES, and react at room temperature for 24h; after the reaction, centrifuge and wash with anhydrous ethanol three times at a speed of 5000rpm for 10min, precipitate and vacuum dry at 45°C for 12h to obtain amino MXene nanomaterials;

[0045] S3. Preparation of chondroitin sulfate A oligosaccharides of different sizes: 24 mg of chondroitin sulfate A was dissolved in 12 mL of enzymatic hydrolysis buffer 20 mM Tris-HCl (pH = 7.0), 0.13 mL of 1 mg / mL ChAC was added, and the mixture was placed on a shaker at 37°C and 100 rpm for 24 h. After the shaking, the mixture was boiled and filtered to remove the protein to obtain a chondroitin sulfate A oligosaccharide mixture; the chondroitin sulfate A oligosaccharide mixture was passed through 3KDa and 1KDa ultrafiltration centrifuge tubes in sequence, and the mixture was collected after centrifugation at 4°C and 4000 rpm for 50 min to obtain chondroitin sulfate A oligosaccharides of <1KDa and 1KDa-3KDa;

[0046] S4. Preparation of MXene-based sugar-containing nanomaterials: 2.5 mg of chondroitin sulfate A oligosaccharide (<1 KDa) was dissolved in 0.5 mL of MES buffer at pH = 5.5, and then 1 mg of EDC and 2 mg of NHS were added for activation at room temperature for 30 min; the pH of the activation solution was then adjusted to 7.3 with PBS buffer at pH = 8; 5 mg of amino-modified MXene was fully ultrasonically dispersed in 2.5 mL of PBS buffer at pH = 7.4, added to the chondroitin sulfate A oligosaccharide solution at pH 7.3, reacted at room temperature for 2 h, dialyzed for 3 days, and freeze-dried to obtain MXene-based sugar-containing nanomaterials.

[0047] Example 2

[0048] The MXene-based sugar-containing nanomaterial and the preparation method thereof of this embodiment specifically include the following steps:

[0049] S1. Preparation of MXene solution: same as Example 1;

[0050] S2. Preparation of amino MXene nanomaterials: Move the MXene solution from -20°C to room temperature, add deionized water, prepare 10mL 5mg / mL MXene solution, add a mixed solution of 10mL anhydrous ethanol and 90mL deionized water, and then continue to add 0.05mL APTES, and react at room temperature for 24h; after the reaction, centrifuge and wash 50% ethanol solution 3 times at a speed of 5000rpm for 10min, and precipitate and dry in vacuum at 45°C for 12h to obtain amino MXene nanomaterials;

[0051] S3. Preparation of chondroitin sulfate A oligosaccharides of different sizes: same as Example 1;

[0052] S4. Preparation of MXene-based sugar-containing nanomaterials: 2.5 mg of chondroitin sulfate A oligosaccharide (1KDa-3KDa) was dissolved in 0.5 mL of MES buffer at pH = 5.5, and then 1 mg of EDC and 2 mg of NHS were added for activation at room temperature for 30 min; the pH of the activation solution was then adjusted to 7.3 with PBS buffer at pH = 8; 5 mg of amino-modified MXene was fully ultrasonically dispersed in 2.5 mL of PBS buffer at pH = 7.4, added to the chondroitin sulfate A oligosaccharide solution at pH 7.3, reacted at room temperature for 2 h, dialyzed for 3 days, and freeze-dried to obtain MXene-based sugar-containing nanomaterials.

[0053] Example 3

[0054] The MXene-based sugar-containing nanomaterial and the preparation method thereof of this embodiment specifically include the following steps:

[0055] S1. Preparation of MXene solution: same as Example 1;

[0056] S2. Preparation of amino MXene nanomaterials: same as in Example 1;

[0057] S3. Preparation of chondroitin sulfate C oligosaccharides of different sizes: 24 mg of chondroitin sulfate C was dissolved in 12 mL of enzymatic hydrolysis buffer 20 mM Tris-HCl (pH=7.0), 0.13 mL of 1 mg / mL ChAC was added, and the mixture was placed on a shaker at 37°C and 100 rpm for 24 h. After the shaking, the mixture was boiled and filtered to remove the protein to obtain a chondroitin sulfate C oligosaccharide mixture; the chondroitin sulfate C oligosaccharide mixture was passed through 3KDa and 1KDa ultrafiltration centrifuge tubes in sequence, and collected after centrifugation at 4°C and 4000 rpm for 50 min to obtain chondroitin sulfate C oligosaccharides of <1KDa and 1KDa-3KDa;

[0058] S4. Preparation of MXene-based sugar-containing nanomaterials: 2.5 mg of chondroitin sulfate C oligosaccharide (<1 KDa) was dissolved in 0.5 mL of MES buffer at pH = 5.5, and then 1 mg of EDC and 2 mg of NHS were added for activation at room temperature for 30 min; the pH of the activation solution was then adjusted to 7.3 with PBS buffer at pH = 8; 5 mg of amino-modified MXene was fully ultrasonically dispersed in 2.5 mL of PBS buffer at pH = 7.4, added to the chondroitin sulfate C oligosaccharide solution at pH 7.3, reacted at room temperature for 2 h, dialyzed for 3 days, and freeze-dried to obtain MXene-based sugar-containing nanomaterials.

[0059] Example 4

[0060] The MXene-based sugar-containing nanomaterial and the preparation method thereof of this embodiment specifically include the following steps:

[0061] S1. Preparation of MXene solution: same as Example 1;

[0062] S2. Preparation of amino MXene nanomaterials: same as in Example 1;

[0063] S3. Preparation of chondroitin sulfate C oligosaccharides of different sizes: same as Example 3;

[0064] S4. Preparation of MXene-based sugar-containing nanomaterials: 2.5 mg of chondroitin sulfate C oligosaccharide (1KDa-3KDa) was dissolved in 0.5 mL of MES buffer at pH = 5.5, and then 1 mg of EDC and 2 mg of NHS were added to activate at room temperature for 30 min; then the pH of the activation solution was adjusted to 7.3 with PBS buffer at pH = 8; 5 mg of amino-modified MXene was fully ultrasonically dispersed in 2.5 mL of PBS buffer at pH = 7.4, added to the chondroitin sulfate C oligosaccharide solution at pH 7.3, reacted at room temperature for 2 h, dialyzed for 3 days, and freeze-dried to obtain MXene-based sugar-containing nanomaterials.

[0065] Comparative Example 1

[0066] Basically the same as Example 1, except for the preparation of the MXene solution: the reaction conditions were 35° C. for 24 h.

[0067] Comparative Example 2

[0068] The method is basically the same as Example 1, except that the MXene solution is prepared as follows: the acid etchant is 1.25 mL of deionized water, 3.75 mL of 12 M HCl solution, and 800 mg of LiF.

[0069] Comparative Example 3

[0070] Basically the same as Example 1, except for the preparation of MXene solution: 2.5 mL of deionized water, 7.5 mL of 12 M HCl solution, and 1200 mg of LiF.

[0071] Test Example 1

[0072] The MXene prepared in Example 1 was diluted to 50 μg / mL, and the MXene potential was characterized by dynamic light scattering of a nanoparticle size analyzer. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that since the MXene surface contains negatively charged groups such as -OH, -F, and -O, MXene is electronegative, and the measured potential of MXene is -27 mV.

[0073] Test Example 2

[0074] The MXene, amino-modified MXene nanomaterials, and MXene-based sugar-containing nanomaterials prepared in Example 1 were diluted to 50 μg / mL and characterized by transmission electron microscopy. The results are as follows: Figure 2 As shown. Figure 2It can be seen that MXene is a flat lamellar structure, and the lamellars are evenly dispersed without stacking, and the lateral size is about 350nm, which is conducive to the modification of the MXene surface by the amination reagent. After modification by the amination reagent, the particle size is further increased, and the lateral size is about 400nm. After modification by chondroitin sulfate, the particle size is further increased, and the lateral size is about 500nm.

[0075] Test Example 3

[0076] The MXene prepared in Example 1 was diluted to 50 μg / mL and characterized by atomic force microscopy. The results are as follows Figure 3 As shown. Figure 3 It can be seen that the thickness of MXene is around 1.5 nm, which is a single layer, and is conducive to further amino modification.

[0077] Test Example 4

[0078] The MXene and MAX prepared in Example 1 and Comparative Examples 1-3 were subjected to X-ray diffraction tests. The results are as follows: Figure 4-Figure 7 As shown. Figure 4 It can be seen that for the raw material MAX, the peak of 104 appears at 39.4°, which is the signal peak of Al of the raw material MAX, and the peak of 002 appears at 9.53°. After etching, the peak of 104 at 39.4° of the obtained MXene disappears, and the peak of 002 shifts to 7.8, indicating that the etched MXene is pure. At the same time, the peaks at 36.8, 44.3, and 61.4 correspond to the -OH end group. This result shows that the etching has obtained a pure MXene with -OH, so as to further modify it by amino. Figure 5 It can be seen that after etching, the 104 peak still exists, and the 002 peak shifts to 6.9. This result shows that the MXene obtained by this etching method is not pure and the etching is not complete, indicating that the appropriate etching time and temperature need to be selected. Figure 6 It can be seen that after etching, the 104 peak still exists, and the 002 peak has not shifted significantly. This result shows that the MXene obtained by this etching method has not been successfully etched, indicating that a suitable etchant concentration needs to be selected. Figure 7 It can be seen that after etching, the peak of 104 still exists, and the peak of 002 shifts to 7.9. This result shows that the MXene obtained by this etching method is not pure and the etching is incomplete, indicating that the ratio of MAX, HCl, deionized water and LiF needs to be adjusted.

[0079] Test Example 5

[0080] The MXene and amino MXene nanomaterials in Example 2 were tested by X-ray photoelectron spectroscopy. The results are as follows: Figure 8 As shown. Figure 8It can be seen that MXene has a C1s signal at 281.56 eV, a Ti2p signal at 455.24 eV, a F1s signal at 686.01 eV, and an O1s signal at 530.08 eV. Since APTES carries silicon and nitrogen elements, after amino modification, an N1s signal appears at 401.16 eV and an Si2p signal appears at 102.05 eV. In addition, after amino modification, the C1s and O1s signals are enhanced. The results show the successful preparation of amino MXene nanomaterials, which can be further modified with chondroitin sulfate to prepare MXene-based sugar-containing nanomaterials.

[0081] Test Example 6

[0082] The MXene prepared in Example 1 was subjected to near-infrared thermal testing, and the results are as follows: Fig. 9 As shown. Fig. 9 It can be seen that 808 nm laser was used to irradiate MXene solutions of different concentrations, and the power was selected to be 1 W / cm 2 It can be seen that in the low concentration range of 0-45μg / mL, the temperature rises significantly with the increase of irradiation time. When the laser irradiation power is increased to 1.5W / cm 2 When irradiated for 10 minutes, the temperature can reach 52°C. MXene has a local surface plasmon resonance effect, a good linear extinction coefficient and excellent photothermal conversion efficiency in the near-infrared (NIR) region. This result shows that MXene can be used as a photothermal material to exert its photothermal effect in the fields of tumor ablation and reducing inflammation.

[0083] Test Example 7

[0084] The MXene and amino MXene nanomaterials (MXene-NH 2 ), MXene-based sugar-containing nanomaterials (MXene-NH 2 -CS) was subjected to thermogravimetric testing, and the results were as follows Fig.10 As shown. Fig.10 It can be seen that in the entire temperature range up to 800°C, for MXene, the weight loss of MXene nanosheets shows an increasing trend, where the weight loss below 200°C is due to the evaporation of physically adsorbed water, and further mass loss is observed afterwards, which is due to the degradation of MXene functional groups (-OH, -F and =O), and the mass residual rate of MXene at 800°C is 88.74%. For amino MXene nanomaterials, CO is generated after 150°C. 2 , between 100℃-220℃, methane and amine anions decompose, and between 400℃-550℃, a sharp drop occurs, including NH 3 NH 2 and N2 The change in can be attributed to the intercalation of APTES between MXene layers and the NH 3+ Electrostatic interaction with the -OH surface termination groups of MXene. The residual mass of the amino MXene nanomaterial at 800°C was 75.83%. This result further indicates the successful synthesis of the amino MXene nanomaterial for further grafting of chondroitin sulfate oligosaccharides. For MXene-based sugar-containing nanomaterials, the mass reduction is large at 150°C-350°C, which is caused by the decomposition of the sugar groups of chondroitin sulfate oligosaccharides in the MXene-based sugar-containing nanomaterials. The residual mass at 800°C is 72.79%, indicating the successful preparation of MXene-based sugar-containing nanomaterials to further exert their chondroitin sulfate-mediated signaling pathway regulation and photothermal synergistic treatment of tumors, inflammation, and promote neural differentiation.

[0085] Test Case 8

[0086] The MXene-based sugar-containing nanomaterials prepared in Example 1 were subjected to near-infrared photothermal testing, and the results were as follows: Fig.11 As shown. Fig.11 It can be seen that the 808nm laser was used to irradiate the MXene-based sugar nanomaterial solutions with different concentrations and the power was selected to be 1W / cm 2 It can be seen that in the low concentration range of 0-45μg / mL, the temperature rises significantly with the increase of irradiation time. When the laser irradiation power is increased to 1.5W / cm 2 When irradiated for 10 minutes, the temperature can reach 48°C. Compared with the photothermal effect of MXene, the photothermal effect of MXene-based sugar-containing nanomaterials is slightly reduced due to the surface modification of MXene, but it still meets the requirements of tumor ablation, inflammation treatment, and neural differentiation.

[0087] Test Example 9

[0088] The MXene-based sugar-containing nanomaterials prepared in Example 4 were tested for cytotoxicity, and the results were as follows: Fig.12 As shown. Fig.12 It can be seen that astrocytes among nerve cells were selected to verify the biocompatibility of MXene-based sugar-containing nanomaterials. In the concentration range of 15 μg / mL-120 μg / mL, the activity of astrocytes was above 90%, indicating that the prepared MXene-based sugar-containing nanomaterials had low toxicity to AST cells and good biocompatibility, and could be used for further cell experiments.

[0089] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for preparing MXene-based sugar-containing nanomaterials, It is characterized in that The following steps are involved: S1, MXene and aminosilane reagent react in a solvent, and the amino MXene nanomaterial is obtained by centrifugal washing and drying; Chondroitin sulfate is enzymatically hydrolyzed by chondroitinase, and chondroitin sulfate oligosaccharide is obtained by ultrafiltration; The amino-modified MXene nanomaterials described in S2 and S1, the chondroitin sulfate oligosaccharides described in S1 and the amide cross-linking agent are reacted, and the MXene-based sugar-containing nanomaterials are obtained through dialysis and freeze-drying.

2. The method for preparing the MXene-based sugar-containing nanomaterial according to claim 1, It is characterized in that In S1, the potential of the MXene is -10mV to -40mV, the particle size is 100nm-600nm, the thickness is 1nm-5nm, and the number of layers is a single layer; the particle size of the amino MXene nanomaterial is 100nm-800nm.

3. The method for preparing the MXene-based sugar-containing nanomaterial according to claim 1, It is characterized in that In S1, the MXene is obtained by etching MAX with an acid etchant; the acid etchant is obtained by mixing water, HCl and LiF in a volume ratio of (5-10):(2-5):(0.1-0.4), and the etching is carried out at 40°C-50°C for 36h-48h.

4. The method for preparing the MXene-based sugar-containing nanomaterial according to claim 1, It is characterized in that In S1, the aminosilane reagent is selected from one or more of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane and 3-(2-aminoethylamino)propyltrimethoxysilane.

5. The method for preparing the MXene-based sugar-containing nanomaterial according to claim 1, It is characterized in that In S1, the mass ratio of the MXene and the aminosilane reagent is (0.01-2):

1.

6. The method for preparing the MXene-based sugar-containing nanomaterial according to claim 1, It is characterized in that In S1, the chondroitinase is selected from chondroitin sulfate lyase AC or chondroitin sulfate lyase ABC; the chondroitin sulfate is selected from one or more of chondroitin sulfate A, chondroitin sulfate C and chondroitin sulfate E.

7. The method for preparing the MXene-based sugar-containing nanomaterial according to claim 1, It is characterized in that In S1, during the enzymatic hydrolysis process, the concentration of chondroitinase is 5 μg / mL-20 μg / mL, and the concentration of chondroitin sulfate is 1 mg / mL-5 mg / mL; the conditions of the enzymatic hydrolysis are: temperature is 20°C-40°C, and time is 20h-30h.

8. The method for preparing the MXene-based sugar-containing nanomaterial according to claim 1, It is characterized in that In S2, the amide cross-linking agent includes EDC and NHS; the mass ratio of EDC to NHS is 1:(1.5-3).

9. The method for preparing the MXene-based sugar-containing nanomaterial according to claim 1, It is characterized in that The mass ratio of the amino MXene nanomaterial, chondroitin sulfate oligosaccharide and amide cross-linking agent is (2-10):(1-5):(1-5).

10. A MXene-based sugar-containing nanomaterial prepared by the method according to any one of claims 1 to 9, It is characterized in that The particle size of the MXene-based sugar-containing nanomaterial is 100nm-900nm.

Citation Information

Cited By

  • Chondroitin sulfate oligosaccharide composition and application thereof in preparation of Parkinson's disease treatment medicine

    CN119909093A