Preparation method of dressing with compression resilience controllable slow release function

By using the combined technology of hollow sustained-release fibers and self-healing hydrogel in wound dressings, the compression rebound controlled sustained-release function is achieved, which solves the problems of uncontrollable drug release and short release time in the existing technology, and provides Long-lasting antibacterial and moist environment, adapting to the needs of different stages in the wound healing process.

CN118767196APending Publication Date: 2024-10-15JIAXING UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410766149.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing wound dressings cannot achieve controllable and long-lasting sustained release in terms of drug release, and have insufficient response capabilities to pressure changes, making it difficult to meet the needs of different stages in the wound healing process.

Method used

It adopts the technology of combining hollow sustained-release fibers and self-healing hydrogel, fills the warp-knitted spacer fabric with Schiff base structure and nano-silver, and uses the dynamic cross-linked structure to achieve the controllable slow-release function of compression rebound and self-healing hydrogel. The glue is wrapped in a tricot fabric to provide long-lasting antibacterial release and a moist environment.

Benefits of technology

It achieves controlled release of drugs and long-lasting antibacterial effect, can release antibacterial substances on demand under static and moving conditions, reduces unnecessary drug release, improves the moistness and safety of the wound healing environment, and prolongs the dressing's healing time. release time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767196A_ABST
    Figure CN118767196A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a dressing with a compression-resilience controllable slow-release function, which comprises the following steps: preparing a warp-knitted spacer fabric by using hollow slow-release fibers as surface layer yarns and spacer yarns, and wrapping and permeating the warp-knitted spacer fabric by using self-repairing hydrogel to obtain a product, the hollow slow-release fibers are composed of hollow porous polyester fibers and fillers distributed inside the hollow porous polyester fibers and in micropores; the filler comprises a Schiff base reaction product and nano-silver, and the Schiff base reaction product is a reaction product of dialdehyde modified polyethylene glycol and chitosan; the self-repairing hydrogel is a double-network structure hydrogel composed of a Schiff base structure and ionic bonds, in the double-network structure, the first network structure is the Schiff base structure formed by reaction of amino of polyetherimide and aldehyde group modified sodium alginate, and the second network structure is the ionic bonds formed by reaction of amino of polyetherimide and aldehyde group modified sodium alginate. The second network structure is an ionic bond formed by the aldehyde group modified sodium alginate in the first network structure through a Ca < 2 + > cross-linking reaction. The dressing prepared by the method disclosed by the invention has a compression rebound controllable slow release function.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wound dressings and relates to a method for preparing a dressing with compression-rebound controllable sustained-release function. Background Art

[0002] The skin is one of the most important tissues in the human body that protects the internal organs from external factors and damage. When the skin is damaged, microorganisms can easily invade the human body and cause infection. Wound dressings are currently a common means of treating skin trauma in clinical practice. Traditional wound dressings (such as cotton bandages and gauze) absorb a large part of the moisture in the wound, making the wound surface too dry, resulting in a decrease in the wound healing rate and pain during separation.

[0003] In recent decades, the types of wound dressing products have been continuously enriched, such as hydrogels, sponges, foams, semipermeable membranes, and functional fiber dressings. Compared with traditional dressings, modern dressings have unparalleled advantages in treating chronic wounds that are difficult to heal. They can maintain a moist environment and better promote wound healing.

[0004] Normal wound repair is a complex process. In order to protect the wound from the invasion of the external environment, the dressing should have the ability to inhibit bacterial proliferation or kill bacteria. Therefore, the function of the dressing has also changed from a single physical covering or a single function to a functional dressing, such as antibiotic-loaded dressings, inorganic antibacterial dressings, and dressings containing biological extracts.

[0005] For example, the silver-containing antibacterial wound dressing prepared by Chinese patent CN 103170004 A, the antibacterial fiber carries silver ions, can continuously release volatile antibacterial effects, and is suitable for the treatment of chronic wounds. Chinese patent CN 111973803 A prepares a wound dressing based on chitosan, which has good mechanical properties and antibacterial properties and can be used alone as an antibacterial wound dressing, making up for the defects of mechanical properties and antibacterial properties of chitosan-based dressings.

[0006] Wound healing is a complex dynamic process. During the wound healing process, the release of drugs or trace elements can protect the wound microenvironment and accelerate wound healing. Modern dressings are quite effective in protecting and maintaining a moist microenvironment, but they also have limitations, such as the inability to control the release of drugs and the short release time.

[0007] In order to solve the above problems, functional sustained-release dressings came into being. Chinese patent CN 103990175 A uses electrospinning technology to prepare a double-layer nanofiber dressing of a natural polymer fiber layer and a synthetic biological polymer fiber layer. By introducing antibiotics, the disadvantage of traditional dressings not having antibacterial ability is overcome. The solubility of the double-layer structure material is different, so the mass ratio of the drug in different layers is adjusted to achieve controlled release of the drug, thereby obtaining a double-layer nanofiber wound dressing with controllable drug release function.

[0008] Chinese patent CN 106822982 A provides a drug sustained-release membrane and a preparation method thereof, using SF and SA as materials, and adding GA and Gly, and obtaining a film dressing of uniform thickness by casting and drying. The membrane can be prepared by adjusting the content of each factor and the ratio process to achieve controlled release of the drug.

[0009] However, the controlled drug release of the above-mentioned dressing is actually achieved by regulating the process parameters during the preparation process, and the determination of the process parameters determines that its release process curve or model is unchanged, and it is difficult to actively control the release during the application of the dressing.

[0010] Wound healing is a complex process involving multiple stages. Active controlled release of drugs can effectively avoid the risk of infection at different stages of wound healing and help promote wound repair and tissue regeneration.

[0011] Reference 1 (Dual-Responsive Alginate Hydrogels for Controlled Release of Therapeutics [J]. Molecules, 2019, 24 (11).) and Reference 2 (In-depth drμg delivery to tumoral soft tissues via pH responsive hydrogel [J]. RSC Adv, 2022, 12 (48): 31402-11.) describe active controlled release of drugs by dressings that are mostly temperature-sensitive or pH-sensitive, that is, when the external environment changes, the dressing will release different amounts of drugs.

[0012] When the environmental conditions are determined, the amount of functional substances released by the dressing will be determined. The pH value changes during the wound healing process. Therefore, compared with thermosensitive wound dressings, sustained-release wound dressings that can respond to pH changes are more meaningful. However, sustained-release dressings that are suitable for pH changes in the complex process of wound healing are often more complicated in design.

[0013] Moreover, the above-mentioned dressings, whether temperature-sensitive or pH-sensitive, rely on changes in the wound microenvironment to release the functional substances of the dressings. Therefore, it is of great practical significance to get rid of the dependence on the wound microenvironment and develop dressings with sustained-release functions controlled by pressure.

[0014] Therefore, it is of great significance to study a preparation method of a dressing with compression rebound and controllable sustained release function to solve the above problems. Summary of the invention

[0015] The purpose of the present invention is to solve the problems existing in the prior art and to provide a method for preparing a dressing with compression-rebound controllable sustained-release function.

[0016] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0017] A method for preparing a dressing with a compression-rebound controllable sustained-release function, comprising: preparing a warp-knitted spacer fabric with hollow sustained-release fibers as surface fibers and spacer fibers, wrapping the warp-knitted spacer fabric with a self-repairing hydrogel and allowing the self-repairing hydrogel to penetrate into the three-dimensional structure of the warp-knitted spacer fabric, thereby preparing a dressing with a compression-rebound controllable sustained-release function; mechanically reinforcing the hollow sustained-release fibers with a warp knitting machine to impart a three-dimensional network structure, wherein the warp-knitted spacer structure provides a certain strength, and the three-dimensional spatial characteristics provide conditions for subsequent penetration and filling of the self-repairing hydrogel, and the filling of the self-repairing hydrogel forms a whole with the three-dimensional structure, thereby enhancing the compression recovery effect of the dressing;

[0018] The hollow sustained-release fiber is composed of a hollow porous polyester fiber and a filler distributed inside the hollow porous polyester fiber and in the micropores; the filler includes a Schiff base reaction product and nanosilver, the Schiff base reaction product is a reaction product of a dialdehyde-modified PEG and chitosan, and the aldehyde group reacts with the amino group to form a Schiff base structure (-N=C-);

[0019] The self-healing hydrogel is a double network structure hydrogel composed of Schiff base structure and ionic bond. In the double network structure, the first network structure is a dynamic cross-linked structure (Schiff base structure) formed by the reaction of amino groups of polyetherimide (PEI) and sodium alginate modified with aldehyde groups, and the second network structure is the sodium alginate modified with aldehyde groups in the first network structure. 2+ Ionic bonds formed by cross-linking reactions.

[0020] In order to achieve a relatively long-term sustained release effect, the present invention changes the preparation process of the fiber so that the fiber is filled with a filler with a Schiff base structure. When the hollow sustained-release fiber is stimulated by an external force (pressing), the release of nanosilver will be promoted, and the Schiff base structure will also be destroyed; after the external force is removed, the Schiff base structure realizes self-repair (i.e., regeneration), which accelerates the recovery of the deformed hollow fiber, thereby reducing the release of nanosilver and achieving a long-term sustained-release antibacterial effect; and the Schiff base structure of the hollow sustained-release fiber can be broken and generated multiple times by external force, thereby realizing active control of the release of nanosilver.

[0021] In order to produce a dressing with compression rebound and controllable sustained release function, the hydrogel used in the preparation should also have a self-repair function, so that the final dressing can achieve active release while also self-recovery, thereby being able to meet the effect of multiple releases.

[0022] As the preferred technical solution:

[0023] The preparation method of the dressing with a controllable sustained-release function of compression rebound as described above, the preparation process of the hollow sustained-release fiber is as follows: the hollow porous polyester fiber (cut length is 120-180 cm) is divided into two sections A and B, the section A is immersed in a pressurized container, the pressurized container contains a precursor composite solution, and the constant temperature is maintained at 40-50° C. to maintain the fluidity of the precursor composite solution, the section B is placed in a vacuum container, and the section A is pressurized and the section B is vacuumed (the section A is pressurized and the section B is vacuumed at the same time), the pressurization and vacuuming process is repeated 3-5 times, and the pressure difference between the two sections A and B is controlled to be 0.05-0.3 MPa. After the reaction is completed, it is washed with anhydrous ethanol and dried in sequence, and then plasma treated to achieve the reduction of nanosilver to obtain the hollow sustained-release fiber;

[0024] The precursor composite solution is a mixture of solution A and solution B, wherein solution A is a mixed solution of polyethylene glycol modified with a dialdehyde group and silver ions, and solution B is a chitosan solution.

[0025] As the preferred technical solution:

[0026] The preparation method of the dressing with compression rebound controllable sustained release function as described above comprises the following steps: slowly dropping 0.01 mol·L-1 into a 0.2 g / mL dialdehyde-modified polyethylene glycol solution at a rate of 1 to 2.5 mL / s. -1silver nitrate solution, keep the polyethylene glycol solution at a constant temperature of 30-40°C during the dropping process, stir for 30-60 minutes to obtain solution A; add chitosan to a mixture of acetic acid and water (the volume ratio of acetic acid to water is 1:100), stir for 2-5 hours at 30-36°C, and filter 2-4 times to obtain solution B; mix solution A and solution B in equal volumes to obtain a precursor composite solution;

[0027] The mass ratio of the silver nitrate solution to the polyethylene glycol solution is 1:30-60; the mass fraction of solution B is 1-4%.

[0028] The preparation method of a dressing with compression rebound controllable sustained release function as described above, the plasma treatment process is: the hollow porous polyester fiber after the reaction, cleaning and drying with anhydrous ethanol is placed in the vacuum chamber of a low-pressure cold plasma device, the input power is 150-200W, a mixture of Ar and water vapor is used as the carrier gas, the gas is introduced into the vacuum chamber at a flow rate of 50-80sccm, and the plasma treatment is performed for 30-50min in an Ar / water vapor atmosphere.

[0029] In the method for preparing a dressing with compression rebound controllable sustained release function as described above, the ratio of the lengths of sections A and B is 1:1.

[0030] In the method for preparing a dressing with compression rebound controllable sustained release function as described above, the preparation process parameters of the warp knitted spacer fabric are as follows:

[0031] Horizontal density: 45 to 60 vertical lines / 5 cm on the front side, 45 to 60 vertical lines / 5 cm on the back side;

[0032] Vertical density: 45-60 horizontal rows / 5cm on the front side, 50-85 horizontal rows / 5cm on the back side;

[0033] The spacing wire arrangement density is 100 to 180 pieces / cm 2 The spacing wire arrangement angle is 20-40°, the spacing wire arrangement is "V" shaped, and the surface density is 120-300g / m 2 ;

[0034] The thickness of the warp knitted spacer fabric is 2.82 to 3.42 mm.

[0035] The preparation method of the dressing with compression rebound controllable sustained release function as described above, using the self-repairing hydrogel to wrap the warp knitted spacer fabric and allowing the self-repairing hydrogel to penetrate into the warp knitted spacer fabric, the specific steps are as follows:

[0036] (1) modifying sodium alginate to obtain aldehyde-modified sodium alginate;

[0037] (2) dissolving the aldehyde-modified sodium alginate in deionized water to prepare an aldehyde-modified sodium alginate solution having a concentration of 1.5 to 3 wt %;

[0038] (3) dissolving PEI in deionized water to obtain a PEI solution with a concentration of 1.5 to 3 wt %;

[0039] (4) Cut the warp knitted spacer fabric into a cylindrical shape and place it in a hollow cylindrical polytetrafluoroethylene mold, wherein the diameter and height of the polytetrafluoroethylene mold are not less than the warp knitted spacer fabric;

[0040] (5) The aldehyde-modified sodium alginate solution and the PEI solution were mixed in a volume ratio of 7:3 to 3:7, and after being drawn up with a syringe, they were injected into the polytetrafluoroethylene mold from top to bottom until the warp knitted spacer fabric was immersed. After standing for 10 to 20 minutes, CaCl with a concentration of 0.2 to 0.25 mol / L was added. 2 The solution is allowed to stand for 5 to 10 minutes again, and then the polytetrafluoroethylene mold is placed at 36 to 45°C for 12 to 24 hours to completely gel it and form a self-repairing hydrogel, thereby obtaining a dressing with compression rebound and controllable sustained release function; wherein, hydrogel molding is a sol-gel transformation process, and the filling of warp-knitted spacer fabric with hydrogel requires time control to ensure its good fluidity, that is, filling the fabric in its sol stage, and after it completely covers the fabric, the gelation process occurs.

[0041] Sodium alginate is a carbohydrate, a random block copolymer formed by linear (1→4) bonded β-D-mannuronic acid (Mannuronic acid, M) and α-L-guluronic acid (Guluronic acid, G). Calcium ions form a monomer complex with the G block; then the monomer complex forms an "egg-box" model dimer under the action of calcium ions; finally, the dimers form a three-dimensional network structure through lateral bonding.

[0042] In the method for preparing a dressing with a compression-rebound controllable sustained-release function as described above, the process of modifying sodium alginate in step (1) is as follows: sodium periodate is added to a sodium alginate solution, and after being placed away from light for 10 to 14 hours, ethylene glycol in an amount equimolar to that of sodium periodate is added, and after stirring for 1 to 2.5 hours to calm the reaction, the obtained product is first precipitated with excess ethanol, and then filtered and dialyzed (dialyzed with a dialysis membrane with a molecular weight cutoff of 10 kDa for 3 days, with water changed every 12 hours), and finally freeze-dried to obtain powdered aldehyde-modified sodium alginate; in order to realize a Schiff base dynamic cross-linking structure, sodium alginate itself has poor water solubility, and the sodium alginate is modified by a classic sodium periodate oxidation method, and aldehyde groups are obtained by modification to improve its water solubility;

[0043] The concentration of the sodium alginate solution is 2-4wt%, and the mass ratio of sodium periodate to the sodium alginate solution is 1.5-4:100.

[0044] In the method for preparing a dressing having a compression-rebound controllable sustained-release function as described above, in step (5), CaCl 2 The molar ratio of sodium alginate to sodium alginate is 2:5.

[0045] Invention mechanism:

[0046] In order to construct a compression-rebound controllable sustained-release functional dressing, the present invention fills the hydrogel into the three-dimensional structure of a warp knitted fabric to obtain a wound dressing. The hollow sustained-release fiber is wrapped inside by the hydrogel. In a static state, the antibacterial substance (nanosilver) inside the hollow sustained-release fiber is slowly released and enters the microenvironment through the hydrogel. The hydrogel wrapping improves the sustained-release effect of the antibacterial substance (nanosilver) in the static state of the dressing. During movement or active slight pressing, more antibacterial substances (nanosilver) inside the hollow sustained-release fiber will be slowly released and enter the microenvironment through the hydrogel, thereby achieving the effect of release on demand. After the pressure is removed, due to the self-repairing effect of the fiber and the hydrogel, the dressing returns to its initial state. During the recovery process, due to the action of the dynamic cross-linking bond, the release amount of the antibacterial substance (nanosilver) will be reduced.

[0047] The classic hydrogel structure is a double covalent network structure with strong mechanical properties, but this type of structure does not have self-repairing ability. In the present invention, the sodium alginate aldehyde group and the PEI amino group undergo Schiff base reaction to construct the first network structure, and the sodium alginate constructs the second network structure through ionic cross-linking, and finally forms a double network structure composed of ionic bonds and Schiff base bonds. The hybrid cross-linked double network hydrogel composed of non-covalent bonds (ionic bonds) and dynamic covalent bonds (Schiff base bonds) has self-repairing ability, and the dynamic covalent bonds complete the reversible recovery process.

[0048] Beneficial effects:

[0049] (1) A method for preparing a dressing with a compression-rebound controllable sustained-release function according to the present invention, wherein the warp-knitted structure inside the dressing with a compression-rebound controllable sustained-release function and the self-repairing hydrogel coated on the outer layer both have a Schiff base structure and a double dynamic cross-linking structure, and the double dynamic cross-linking structure enables the dressing as a whole to have a good compression recovery effect;

[0050] (2) The present invention provides a method for preparing a dressing with a compression-rebound controllable sustained-release function. The self-repairing hydrogel coating prolongs the sustained-release time of the functional warp-knitted spacer fabric inside. The self-repairing hydrogel coating prevents the warp-knitted spacer fabric inside from direct contact with the human body, thereby improving its safety. The dressing can also be combined with different hydrogels or functional fibers, thereby broadening its application range.

[0051] (3) A method for preparing a dressing with a compression-rebound controllable sustained-release function according to the present invention, wherein the sustained-release of antibacterial substances inside the hollow sustained-release fibers can prevent wound infection for a long time, and the moist environment maintained by the hydrogel can accelerate the migration and proliferation of epithelial cells, thereby promoting faster wound healing;

[0052] (4) The present invention provides a method for preparing a dressing with a controllable sustained-release function by compression and rebound. The dressing can slowly release itself in a relatively static state. During movement or active slight pressing, the antibacterial substance inside the hollow sustained-release fiber will be slowly released, so that the antibacterial substance in the dressing can be actively released on demand by compression and rebound. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 is a schematic diagram of a warp knitted spacer fabric;

[0054] Figure 2 Schematic diagram of the self-healing hydrogel structure;

[0055] Figure 3 This is the schematic diagram of the Schiff base reaction of self-healing hydrogel;

[0056] Figure 4 Schematic diagram of the preparation of a dressing with compression-rebound controllable sustained-release function;

[0057] Among them, 1-surface silk, 2-spacer silk, 3-self-repairing hydrogel, 4-sodium alginate molecular chain, 5-PEI molecular chain. DETAILED DESCRIPTION

[0058] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0059] The test method involved in the present invention is as follows:

[0060] Silver ion release performance: The silver ion concentration was measured using inductively coupled plasma atomic emission spectrometry (ICPAES);

[0061] Test of static silver ion release performance of dressings: The dressings with compression-rebound controllable sustained-release function were uniformly prepared into patches with a diameter of 2 cm using a puncher, and the dressings were immersed in PBS buffer at a mass ratio of 1:40, and shaken in a 36°C water bath at 50 rpm. Samples were taken out at 24 h, 72 h and 168 h to test the silver release in PBS buffer;

[0062] Test of the silver ion release performance of the dressing after being compressed: The dressing with compression rebound controllable sustained release function is uniformly prepared into a patch with a diameter of 2 cm by using a puncher, and compressed to 50% deformation by using a mechanical universal testing machine, a sensor of 50N, a compression speed of 0.5mm / min, and cyclic compression 5 to 10 times. The height is fixed by a metal pin and transferred to a beaker containing PBS buffer for the first immersion. The mass ratio of the dressing to the PBS buffer is 1:40. The extract is taken out after 24h, 72h and 168h, and the silver ion concentration is determined; the metal pin is removed, and the dressing is immersed in PBS buffer again, and it is left to stand for 3 to 7h to allow it to self-repair to the initial state, and it is shaken in a 36°C water bath at 50rpm. The extract is taken out after 24h, 72h and 168h, and the silver release in the extract is tested;

[0063] Antibacterial test: According to FZ / T 73023-2006 "Antibacterial knitwear": Oscillation method: Place the compressed dressing with fixed height and metal pin removed in an agar dish containing PBS buffer, and then inoculate 100 μL of 10 5 CFU / mL of bacterial suspension, the bacterial species is Staphylococcus aureus or Escherichia coli, and the colony status is observed within a certain period of time.

[0064] Example 1

[0065] A method for preparing a dressing with compression rebound controllable sustained release function, the specific steps are as follows:

[0066] (1) Slowly add 0.01 mol·L-1 d-butylene glycol (molecular weight 600, Chongqing Yuci Pharmaceutical Technology Co., Ltd.) to a 0.2 g / mL solution of dialdehyde-modified polyethylene glycol at a rate of 1 mL / s. -1 silver nitrate solution, keeping the polyethylene glycol solution at a constant temperature of 35°C during the addition, stirring for 40 minutes to obtain solution A;

[0067] Wherein, the mass ratio of silver nitrate solution to polyethylene glycol solution is 1:40;

[0068] (2) adding chitosan to a mixture of acetic acid and water in a volume ratio of 1:100, stirring at 36°C for 2 h, and filtering 4 times to obtain a solution B with a mass fraction of 1%;

[0069] (3) mixing solution A and solution B in equal volumes to obtain a precursor composite solution;

[0070] (4) The hollow porous polyester fiber is divided into two sections, A and B, with a length ratio of 1:1. Section A is immersed in a pressurized container, the pressurized container contains a precursor composite solution, and the temperature is maintained at 50°C. Section B is placed in a vacuum container, and section A is pressurized and section B is vacuumed. The pressurization and vacuuming process is repeated 3 times, and the pressure difference between sections A and B is controlled to be 0.1 MPa. After the reaction is completed, it is washed with anhydrous ethanol and dried in turn;

[0071] Among them, the specification of hollow porous polyester fiber is 75D / 24F, the hollowness is 30%, the fiber elongation is 32%, and the average pore size of micropores is 0.05μm;

[0072] (5) placing the hollow porous polyester fiber after the reaction in step (4) and after being washed with anhydrous ethanol and dried in a vacuum chamber of a low-pressure cold plasma device, with an input power of 200 W, a mixture of Ar and water vapor as a carrier gas, Ar and water vapor are introduced into the vacuum chamber at flow rates of 80 sccm and 75 sccm, respectively, and plasma treatment is performed for 30 min in an Ar / water vapor atmosphere to obtain a hollow sustained-release fiber;

[0073] (6) Figure 1 As shown, a warp knitted spacer fabric with a thickness of 3.02 mm was prepared using a six-bar E-18 double needle bed Raschel warp knitting machine with hollow slow-release fibers as surface yarns and spacer yarns;

[0074] The preparation process parameters of warp knitted spacer fabrics are as follows:

[0075] Horizontal density: 50 vertical lines / 5cm on the front side, 45 vertical lines / 5cm on the back side;

[0076] Vertical density: 40 horizontal rows / 5cm on the front side, 80 horizontal rows / 5cm on the back side;

[0077] The spacing wire arrangement density is 180 pieces / cm 2 The spacing wires are arranged in a V-shaped pattern with an inclination angle of 35° and a surface density of 200g / m 2 ;

[0078] (7) Wrapping the warp knitted spacer fabric with the self-repairing hydrogel and allowing the self-repairing hydrogel to penetrate into the warp knitted spacer fabric, the specific steps are as follows:

[0079] (7.1) Sodium periodate is added to the sodium alginate solution, and after being placed in dark for 10 hours, ethylene glycol in an amount equal to that of the sodium periodate is added. After stirring for one hour, the obtained product is first precipitated with excess ethanol, then filtered and dialyzed, and finally freeze-dried to obtain aldehyde-modified sodium alginate;

[0080] The concentration of the sodium alginate solution is 2wt%, and the mass ratio of sodium periodate to the sodium alginate solution is 1.5:100;

[0081] (7.2) dissolving the aldehyde-modified sodium alginate in deionized water to prepare an aldehyde-modified sodium alginate solution with a concentration of 1.5 wt %;

[0082] (7.3) PEI (from Sigma-Aldrich, CAS No.: 9002-98-6) was dissolved in deionized water to obtain a PEI solution with a concentration of 2 wt%;

[0083] (7.4) Cut the warp knitted spacer fabric into a cylindrical shape and place it in a hollow cylindrical polytetrafluoroethylene mold. The diameter and height of the polytetrafluoroethylene mold are not less than the warp knitted spacer fabric;

[0084] (7.5) Figures 2-3 As shown in the figure, the aldehyde-modified sodium alginate solution and the PEI solution were mixed in a volume ratio of 3:7, and after being sucked up with a syringe, they were injected into the polytetrafluoroethylene mold from top to bottom until the warp knitted spacer fabric was immersed. After standing for 10 minutes, 0.2 mol / L CaCl 2 The solution was allowed to stand for 5 minutes again, and then the polytetrafluoroethylene mold was placed at 36°C for 24 hours to completely gel and form a self-healing hydrogel 3, thereby obtaining a dressing with compression-rebound controllable sustained release function;

[0085] Among them, CaCl 2 The molar ratio of sodium alginate to sodium alginate is 2:5.

[0086] The self-healing hydrogel 3 is a double network structure hydrogel composed of a Schiff base structure and an ionic bond. In the double network structure, the first network structure is a Schiff base structure formed by the reaction of the amino group of PEI (PEI molecular chain 5) and the aldehyde-modified sodium alginate (sodium alginate molecular chain 4), and the second network structure is the aldehyde-modified sodium alginate in the first network structure. 2+ Ionic bonds formed by cross-linking reactions.

[0087] After immersion for 24h, 72h and 168h, the static silver ion release of the prepared dressing with compression rebound controllable sustained release function was 12μg / mL, 19μg / mL and 26μg / mL respectively. After 10 cycles of compression, the compressed silver ion release of the dressing with compression rebound controllable sustained release function after the first immersion for 24h, 72h and 168h was 30μg / mL, 40μg / mL and 46μg / mL respectively, and the second immersion for 24h, 72h The compressed silver ion release amounts after 168h were 16μg / mL, 23μg / mL and 30μg / mL respectively; the antibacterial rates of the dressing with fixed height after compression against Escherichia coli were 99.9% and 99.9% respectively after 168h; after the metal pin was removed, the dressing was left to stand for 6h to return to its initial state, and the antibacterial rates of the dressing returned to its initial state were 99% and 99.1% respectively after 168h against Escherichia coli and Staphylococcus aureus.

[0088] Example 2

[0089] A method for preparing a dressing with compression rebound controllable sustained release function, the specific steps are as follows:

[0090] (1) Slowly add 0.01 mol·L-1 d-butylene glycol (molecular weight 600, Chongqing Yuci Pharmaceutical Technology Co., Ltd.) to a 0.2 g / mL solution of dialdehyde-modified polyethylene glycol at a rate of 1.5 mL / s. -1 silver nitrate solution, keeping the polyethylene glycol solution at a constant temperature of 30°C during the addition, stirring for 60 minutes to obtain solution A;

[0091] Wherein, the mass ratio of silver nitrate solution to polyethylene glycol solution is 1:40;

[0092] (2) adding chitosan to a mixture of acetic acid and water in a volume ratio of 1:100, stirring at 30°C for 5 h, and filtering twice to obtain a solution B with a mass fraction of 1%;

[0093] (3) mixing solution A and solution B in equal volumes to obtain a precursor composite solution;

[0094] (4) The hollow porous polyester fiber is divided into two sections, A and B, with a length ratio of 1:1. Section A is immersed in a pressurized container, the pressurized container contains a precursor composite solution, and the temperature is maintained at 40°C. Section B is placed in a vacuum container, and section A is pressurized and section B is vacuumed. The pressurization and vacuuming process is repeated 3 times, and the pressure difference between sections A and B is controlled to be 0.1 MPa. After the reaction is completed, it is washed with anhydrous ethanol and dried in turn;

[0095] Among them, the specification of hollow porous polyester fiber is 75D / 24F, the hollowness is 25%, the fiber elongation is 30%, and the average pore size of micropores is 0.3μm;

[0096] (5) placing the hollow porous polyester fiber after the reaction in step (4) and after being washed with anhydrous ethanol and dried in a vacuum chamber of a low-pressure cold plasma device, with an input power of 150 W, a mixture of Ar and water vapor as a carrier gas, Ar and water vapor are introduced into the vacuum chamber at flow rates of 50 sccm and 40 sccm, respectively, and plasma treatment is performed for 30 min in an Ar / water vapor atmosphere to obtain a hollow sustained-release fiber;

[0097] (6) Using the hollow slow-release fiber as the surface yarn and the spacer yarn, a warp knitted spacer fabric with a thickness of 2.96 mm was prepared using an E-18 double needle bed Raschel warp knitting machine with six guide bars;

[0098] The preparation process parameters of warp knitted spacer fabrics are as follows:

[0099] Horizontal density: 50 vertical lines / 5cm on the front side, 50 vertical lines / 5cm on the back side;

[0100] Vertical density: 50 horizontal rows / 5cm on the front side, 50 horizontal rows / 5cm on the back side;

[0101] The spacing wire arrangement density is 100 pieces / cm 2 The spacing wire arrangement angle is 40°, the spacing wire arrangement is "V" shaped, and the surface density is 120g / m 2 ;

[0102] (7) Wrapping the warp knitted spacer fabric with the self-repairing hydrogel and allowing the self-repairing hydrogel to penetrate into the warp knitted spacer fabric, the specific steps are as follows:

[0103] (7.1) Sodium periodate is added to the sodium alginate solution, and after being placed in dark for 12 hours, ethylene glycol in an amount equal to that of the sodium periodate is added, and after stirring for 2.5 hours, the obtained product is first precipitated with excess ethanol, then filtered and dialyzed, and finally freeze-dried to obtain aldehyde-modified sodium alginate;

[0104] The concentration of the sodium alginate solution is 4wt%, and the mass ratio of sodium periodate to the sodium alginate solution is 3:100;

[0105] (7.2) dissolving the aldehyde-modified sodium alginate in deionized water to prepare an aldehyde-modified sodium alginate solution with a concentration of 3 wt %;

[0106] (7.3) PEI (from Sigma-Aldrich, CAS No.: 9002-98-6) was dissolved in deionized water to obtain a PEI solution with a concentration of 2.5 wt%;

[0107] (7.4) Cut the warp knitted spacer fabric into a cylindrical shape and place it in a hollow cylindrical polytetrafluoroethylene mold. The diameter and height of the polytetrafluoroethylene mold are not less than the warp knitted spacer fabric;

[0108] (7.5) The aldehyde-modified sodium alginate solution and the PEI solution were mixed in a volume ratio of 7:3, and after being drawn up with a syringe, they were injected into the polytetrafluoroethylene mold from top to bottom until the warp knitted spacer fabric was immersed. After standing for 20 min, 0.25 mol / L CaCl was added. 2 The solution was allowed to stand for 10 minutes again, and then the polytetrafluoroethylene mold was placed at 38°C for 21 hours to completely gel and form a self-healing hydrogel, thereby obtaining a dressing with compression-rebound controllable sustained-release function;

[0109] Among them, CaCl 2 The molar ratio of sodium alginate to sodium alginate is 2:5.

[0110] The self-healing hydrogel is a double network structure hydrogel composed of Schiff base structure and ionic bond. In the double network structure, the first network structure is a Schiff base structure formed by the reaction of PEI amino group and aldehyde-modified sodium alginate, and the second network structure is the aldehyde-modified sodium alginate in the first network structure. 2+ Ionic bonds formed by cross-linking reactions.

[0111] After immersion for 24h, 72h and 168h, the static silver ion release of the prepared dressing with compression rebound controllable sustained release function was 18μg / mL, 25μg / mL and 29μg / mL respectively. After 5 cycles of compression, the compressed silver ion release of the dressing with compression rebound controllable sustained release function after the first immersion for 24h, 72h and 168h was 23μg / mL, 34μg / mL and 40μg / mL respectively, and the second immersion for 24h, 72h and 168h was 24μg / mL, 72h and 168h respectively. The release of compressed silver ions after 68 hours were 22μg / mL, 29μg / mL and 36μg / mL respectively; the antibacterial rate of the dressing with a fixed height after compression against Escherichia coli was 99.9% after 168 hours, and the antibacterial rate against Staphylococcus aureus was 99.9%; after the metal pin was removed, the dressing was left to stand for 3 hours to return to its initial state, and the antibacterial rate of the dressing returned to its initial state was 99.7% against Escherichia coli after 168 hours, and the antibacterial rate against Staphylococcus aureus was 99.3%.

[0112] Example 3

[0113] A method for preparing a dressing with compression rebound controllable sustained release function, the specific steps are as follows:

[0114] (1) Slowly add 0.01 mol·L-1 d-butylene glycol (molecular weight 400, Chongqing Yuci Pharmaceutical Technology Co., Ltd.) to a 0.2 g / mL solution of dialdehyde-modified polyethylene glycol at a rate of 1 mL / s. -1 silver nitrate solution, keeping the polyethylene glycol solution at a constant temperature of 32°C during the addition, stirring for 50 minutes to obtain solution A;

[0115] Wherein, the mass ratio of silver nitrate solution to polyethylene glycol solution is 1:60;

[0116] (2) chitosan was added to a mixture of acetic acid and water in a volume ratio of 1:100, stirred at 32°C for 4 h, and filtered three times to obtain a solution B with a mass fraction of 2.5%;

[0117] (3) mixing solution A and solution B in equal volumes to obtain a precursor composite solution;

[0118] (4) The hollow porous polyester fiber is divided into two sections, A and B, with a length ratio of 1:1. Section A is immersed in a pressurized container, the pressurized container contains a precursor composite solution and maintains a constant temperature of 42°C. Section B is placed in a vacuum container, and section A is pressurized and section B is vacuumed. The pressurization and vacuuming process is repeated 4 times, and the pressure difference between sections A and B is controlled to be 0.05 MPa. After the reaction is completed, it is washed with anhydrous ethanol and dried in turn;

[0119] Among them, the specification of hollow porous polyester fiber is 75D / 36F, the hollowness is 30%, the fiber elongation is 28%, and the average pore size of micropores is 0.1μm;

[0120] (5) placing the hollow porous polyester fiber after the reaction in step (4) and after being washed with anhydrous ethanol and dried in a vacuum chamber of a low-pressure cold plasma device, with an input power of 200 W, a mixture of Ar and water vapor as a carrier gas, and Ar and water vapor are introduced into the vacuum chamber at flow rates of 80 sccm and 80 sccm respectively, and plasma treatment is performed for 35 min in an Ar / water vapor atmosphere to obtain a hollow sustained-release fiber;

[0121] (6) Using the hollow slow-release fiber as the surface yarn and the spacer yarn, a warp knitted spacer fabric with a thickness of 3.42 mm was prepared using an E-18 double needle bed Raschel warp knitting machine with six guide bars;

[0122] The preparation process parameters of warp knitted spacer fabrics are as follows:

[0123] Horizontal density: 60 vertical lines / 5cm on the front side, 50 vertical lines / 5cm on the back side;

[0124] Vertical density: 50 horizontal rows / 5cm on the front side, 70 horizontal rows / 5cm on the back side;

[0125] The spacing wire arrangement density is 140 pieces / cm 2 The spacing wire arrangement angle is 30°, the spacing wire arrangement is "V" shaped, and the surface density is 280g / m 2 ;

[0126] (7) Wrapping the warp knitted spacer fabric with the self-repairing hydrogel and allowing the self-repairing hydrogel to penetrate into the warp knitted spacer fabric, the specific steps are as follows:

[0127] (7.1) Sodium periodate is added to the sodium alginate solution, and after being placed in dark for 10 hours, ethylene glycol in an amount equal to that of the sodium periodate is added, and after stirring for 1.5 hours, the obtained product is first precipitated with excess ethanol, then filtered and dialyzed, and finally freeze-dried to obtain aldehyde-modified sodium alginate;

[0128] The concentration of the sodium alginate solution is 2.5wt%, and the mass ratio of sodium periodate to the sodium alginate solution is 1.6:100;

[0129] (7.2) dissolving the aldehyde-modified sodium alginate in deionized water to prepare an aldehyde-modified sodium alginate solution with a concentration of 2 wt %;

[0130] (7.3) PEI (from Sigma-Aldrich, CAS No.: 9002-98-6) was dissolved in deionized water to obtain a PEI solution with a concentration of 1.5 wt%;

[0131] (7.4) Cut the warp knitted spacer fabric into a cylindrical shape and place it in a hollow cylindrical polytetrafluoroethylene mold. The diameter and height of the polytetrafluoroethylene mold are not less than the warp knitted spacer fabric;

[0132] (7.5) The aldehyde-modified sodium alginate solution and the PEI solution were mixed in a volume ratio of 5:5, and after being drawn up with a syringe, they were injected into the polytetrafluoroethylene mold from top to bottom until the warp knitted spacer fabric was immersed. After standing for 15 min, 0.2 mol / L CaCl was added. 2 The solution was allowed to stand for 10 minutes again, and then the polytetrafluoroethylene mold was placed at 40°C for 18 hours to completely gel and form a self-healing hydrogel, thereby obtaining a dressing with compression-rebound controllable sustained-release function;

[0133] Among them, CaCl 2 The molar ratio of sodium alginate to sodium alginate is 2:5.

[0134] The self-healing hydrogel is a double network structure hydrogel composed of Schiff base structure and ionic bond. In the double network structure, the first network structure is a Schiff base structure formed by the reaction of PEI amino group and aldehyde-modified sodium alginate, and the second network structure is the aldehyde-modified sodium alginate in the first network structure. 2+Ionic bonds formed by cross-linking reactions.

[0135] After immersion for 24h, 72h and 168h, the static silver ion release of the prepared dressing with compression rebound controllable sustained release function was 14μg / mL, 23μg / mL and 28μg / mL respectively. After 8 cycles of compression, the compressed silver ion release of the dressing with compression rebound controllable sustained release function after the first immersion for 24h, 72h and 168h was 27μg / mL, 38μg / mL and 42μg / mL respectively, and the second immersion for 24h, 72h and 168h was 24μg / mL, 72h and 168h respectively. The release of compressed silver ions after 68 hours were 17μg / mL, 24μg / mL and 31μg / mL respectively; the antibacterial rate of the dressing with a fixed height after compression against Escherichia coli was 99.9% after 168 hours, and the antibacterial rate against Staphylococcus aureus was 99.9%; after the metal pin was removed, the dressing was left to stand for 7 hours to return to its initial state, and the antibacterial rate of the dressing returned to its initial state was 99.7% against Escherichia coli after 168 hours, and the antibacterial rate against Staphylococcus aureus was 99.4%.

[0136] Example 4

[0137] A method for preparing a dressing with compression rebound controllable sustained release function, the specific steps are as follows:

[0138] (1) Slowly add 0.01 mol·L-1 dicalcium hydroxide to a 0.2 g / mL solution of dialdehyde-modified polyethylene glycol (molecular weight 1000, Chongqing Yuci Pharmaceutical Technology Co., Ltd.) at a rate of 2 mL / s. -1 silver nitrate solution, keeping the polyethylene glycol solution at a constant temperature of 38°C during the addition, stirring for 40 minutes to obtain solution A;

[0139] Wherein, the mass ratio of silver nitrate solution to polyethylene glycol solution is 1:30;

[0140] (2) adding chitosan to a mixture of acetic acid and water in a volume ratio of 1:100, stirring at 34°C for 3 h, and filtering 4 times to obtain a solution B with a mass fraction of 4%;

[0141] (3) mixing solution A and solution B in equal volumes to obtain a precursor composite solution;

[0142] (4) The hollow porous polyester fiber is divided into two sections, A and B, with a length ratio of 1:1. Section A is immersed in a pressurized container, the pressurized container contains a precursor composite solution, and the temperature is maintained at 48°C. Section B is placed in a vacuum container, and section A is pressurized and section B is vacuumed. The pressurization and vacuuming process is repeated 5 times, and the pressure difference between sections A and B is controlled to be 0.3 MPa. After the reaction is completed, it is washed with anhydrous ethanol and dried in turn;

[0143] Among them, the specification of hollow porous polyester fiber is 75D / 72F, the hollowness is 35%, the fiber elongation is 25%, and the average pore size of micropores is 0.05μm;

[0144] (5) placing the hollow porous polyester fiber after the reaction in step (4) and after being washed with anhydrous ethanol and dried in a vacuum chamber of a low-pressure cold plasma device, with an input power of 180 W, a mixture of Ar and water vapor as a carrier gas, Ar and water vapor are introduced into the vacuum chamber at flow rates of 60 sccm and 55 sccm, respectively, and plasma treatment is performed for 40 min in an Ar / water vapor atmosphere to obtain a hollow sustained-release fiber;

[0145] (6) Using the hollow slow-release fiber as the surface yarn and the spacer yarn, a warp knitted spacer fabric with a thickness of 2.82 mm was prepared using an E-18 double needle bed Raschel warp knitting machine with six guide bars;

[0146] The preparation process parameters of warp knitted spacer fabrics are as follows:

[0147] Horizontal density: 60 vertical lines / 5cm on the front side, 55 vertical lines / 5cm on the back side;

[0148] Vertical density: 45 horizontal rows / 5cm on the front side, 80 horizontal rows / 5cm on the back side;

[0149] The spacing wire arrangement density is 170 pieces / cm 2 The spacing wires are arranged in a V-shaped pattern with an inclination angle of 20° and a surface density of 300 g / m 2 ;

[0150] (7) Wrapping the warp knitted spacer fabric with the self-repairing hydrogel and allowing the self-repairing hydrogel to penetrate into the warp knitted spacer fabric, the specific steps are as follows:

[0151] (7.1) Sodium periodate is added to the sodium alginate solution, and after being placed in dark for 11 hours, ethylene glycol in an amount equal to that of the sodium periodate is added, and after stirring for 2 hours, the obtained product is first precipitated with excess ethanol, then filtered and dialyzed, and finally freeze-dried to obtain aldehyde-modified sodium alginate;

[0152] The concentration of the sodium alginate solution is 3wt%, and the mass ratio of sodium periodate to the sodium alginate solution is 2:100;

[0153] (7.2) dissolving the aldehyde-modified sodium alginate in deionized water to prepare an aldehyde-modified sodium alginate solution with a concentration of 2.5 wt %;

[0154] (7.3) PEI (from Sigma-Aldrich, CAS No.: 9002-98-6) was dissolved in deionized water to obtain a 3 wt% PEI solution;

[0155] (7.4) Cut the warp knitted spacer fabric into a cylindrical shape and place it in a hollow cylindrical polytetrafluoroethylene mold. The diameter and height of the polytetrafluoroethylene mold are not less than the warp knitted spacer fabric;

[0156] (7.5) The aldehyde-modified sodium alginate solution and the PEI solution were mixed in a volume ratio of 3:7, and after being drawn up with a syringe, they were injected into the polytetrafluoroethylene mold from top to bottom until the warp knitted spacer fabric was immersed. After standing for 20 min, 0.2 mol / L CaCl was added. 2 The solution was allowed to stand for 5 minutes again, and then the polytetrafluoroethylene mold was placed at 42°C for 15 hours to completely gel and form a self-healing hydrogel, thereby obtaining a dressing with compression-rebound controllable sustained-release function;

[0157] Among them, CaCl 2 The molar ratio of sodium alginate to sodium alginate is 2:5.

[0158] The self-healing hydrogel is a double network structure hydrogel composed of Schiff base structure and ionic bond. In the double network structure, the first network structure is a Schiff base structure formed by the reaction of PEI amino group and aldehyde-modified sodium alginate, and the second network structure is the aldehyde-modified sodium alginate in the first network structure. 2+ Ionic bonds formed by cross-linking reactions.

[0159] After immersion for 24h, 72h and 168h, the static silver ion release of the prepared dressing with compression rebound controllable sustained release function was 16μg / mL, 24μg / mL and 27μg / mL respectively. After 6 cycles of compression, the compressed silver ion release of the dressing with compression rebound controllable sustained release function after the first immersion for 24h, 72h and 168h was 26μg / mL, 32μg / mL and 44μg / mL respectively, and the second immersion for 24h, 72h and 168h was 24μg / mL, 72μg / mL and 168h respectively. The release of compressed silver ions after 68 hours were 20μg / mL, 27μg / mL and 33μg / mL respectively; the antibacterial rate of the dressing with a fixed height after compression against Escherichia coli was 99.9% after 168 hours, and the antibacterial rate against Staphylococcus aureus was 99.9%; after the metal pin was removed, the dressing was left to stand for 5 hours to return to its initial state, and the antibacterial rate of the dressing returned to its initial state was 99.6% against Escherichia coli after 168 hours, and the antibacterial rate against Staphylococcus aureus was 99.2%.

[0160] Example 5

[0161] A method for preparing a dressing with compression rebound controllable sustained release function, the specific steps are as follows:

[0162] (1) Slowly add 0.01 mol·L-1 d-butylene glycol (molecular weight 400, Chongqing Yuci Pharmaceutical Technology Co., Ltd.) to a 0.2 g / mL solution of dialdehyde-modified polyethylene glycol at a rate of 2.5 mL / s. -1 silver nitrate solution, keep the polyethylene glycol solution at a constant temperature of 40°C during the addition, and stir for 30 minutes to obtain solution A;

[0163] Wherein, the mass ratio of silver nitrate solution to polyethylene glycol solution is 1:50;

[0164] (2) adding chitosan to a mixture of acetic acid and water in a volume ratio of 1:100, stirring at 35°C for 2.5 h, and filtering twice to obtain a solution B with a mass fraction of 2%;

[0165] (3) mixing solution A and solution B in equal volumes to obtain a precursor composite solution;

[0166] (4) The hollow porous polyester fiber is divided into two sections, A and B, with a length ratio of 1:1. Section A is immersed in a pressurized container, the pressurized container contains a precursor composite solution, and the temperature is maintained at 40°C. Section B is placed in a vacuum container, and section A is pressurized and section B is vacuumed. The pressurization and vacuuming process is repeated 3 times, and the pressure difference between sections A and B is controlled to be 0.2 MPa. After the reaction is completed, it is washed with anhydrous ethanol and dried in turn;

[0167] (5) placing the hollow porous polyester fiber after the reaction in step (4) and after being washed with anhydrous ethanol and dried in a vacuum chamber of a low-pressure cold plasma device, with an input power of 160 W, a mixture of Ar and water vapor as a carrier gas, Ar and water vapor are introduced into the vacuum chamber at flow rates of 70 sccm and 70 sccm, respectively, and plasma treatment is performed for 50 min in an Ar / water vapor atmosphere to obtain a hollow sustained-release fiber;

[0168] Among them, the specification of hollow porous polyester fiber is 75D / 24F, the hollowness is 28%, the fiber elongation is 34%, and the average pore size of micropores is 0.01μm;

[0169] (6) Using the hollow slow-release fiber as the surface yarn and the spacer yarn, a warp knitted spacer fabric with a thickness of 3.16 mm was prepared using an E-18 double needle bed Raschel warp knitting machine with six guide bars;

[0170] The preparation process parameters of warp knitted spacer fabrics are as follows:

[0171] Horizontal density: 45 vertical lines / 5cm on the front side, 60 vertical lines / 5cm on the back side;

[0172] Vertical density: 60 horizontal rows / 5cm on the front side, 85 horizontal rows / 5cm on the back side;

[0173] The spacing wire arrangement density is 110 pieces / cm 2 The spacing wire arrangement angle is 30°, the spacing wire arrangement is "V" shaped, and the surface density is 160g / m 2 ;

[0174] (7) Wrapping the warp knitted spacer fabric with the self-repairing hydrogel and allowing the self-repairing hydrogel to penetrate into the warp knitted spacer fabric, the specific steps are as follows:

[0175] (7.1) Sodium periodate is added to the sodium alginate solution, and after being placed in dark for 14 hours, ethylene glycol in an amount equal to that of the sodium periodate is added, and after stirring for 1.5 hours, the obtained product is first precipitated with excess ethanol, then filtered and dialyzed, and finally freeze-dried to obtain aldehyde-modified sodium alginate;

[0176] The concentration of the sodium alginate solution is 3.2wt%, and the mass ratio of sodium periodate to the sodium alginate solution is 2.2:100;

[0177] (7.2) dissolving the aldehyde-modified sodium alginate in deionized water to prepare an aldehyde-modified sodium alginate solution with a concentration of 3 wt %;

[0178] (7.3) PEI (from Sigma-Aldrich, CAS No.: 9002-98-6) was dissolved in deionized water to obtain a PEI solution with a concentration of 2 wt%;

[0179] (7.4) Cut the warp knitted spacer fabric into a cylindrical shape and place it in a hollow cylindrical polytetrafluoroethylene mold. The diameter and height of the polytetrafluoroethylene mold are not less than the warp knitted spacer fabric;

[0180] (7.5) The aldehyde-modified sodium alginate solution and the PEI solution were mixed in a volume ratio of 7:3, and after being drawn up with a syringe, they were injected into the polytetrafluoroethylene mold from top to bottom until the warp knitted spacer fabric was immersed. After standing for 10 min, 0.25 mol / L CaCl 2 The solution was allowed to stand for 8 minutes again, and then the polytetrafluoroethylene mold was placed at 45°C for 12 hours to completely gel and form a self-healing hydrogel, thereby obtaining a dressing with compression-rebound controllable sustained-release function;

[0181] Among them, CaCl 2 The molar ratio of sodium alginate to sodium alginate is 2:5.

[0182] The self-healing hydrogel is a double network structure hydrogel composed of Schiff base structure and ionic bond. In the double network structure, the first network structure is a Schiff base structure formed by the reaction of PEI amino group and aldehyde-modified sodium alginate, and the second network structure is the aldehyde-modified sodium alginate in the first network structure. 2+Ionic bonds formed by cross-linking reactions.

[0183] After immersion for 24h, 72h and 168h, the static silver ion release of the prepared dressing with compression rebound controllable sustained release function was 15μg / mL, 23μg / mL and 28μg / mL respectively. After 8 cycles of compression, the compressed silver ion release of the dressing with compression rebound controllable sustained release function after the first immersion for 24h, 72h and 168h was 28μg / mL, 39μg / mL and 42μg / mL respectively, and the second immersion for 24h, 72h and 168h was 28μg / mL, 39μg / mL and 42μg / mL respectively. The amount of compressed silver ions released after 68 hours was 18μg / mL, 26μg / mL and 34μg / mL respectively; the antibacterial rate of the dressing with a fixed height after compression against Escherichia coli was 99.9% after 168 hours, and the antibacterial rate against Staphylococcus aureus was 99.9%; after the metal pin was removed, the dressing was left to stand for 4 hours to return to its initial state, and the antibacterial rate of the dressing returned to its initial state was 99.2% against Escherichia coli after 168 hours, and the antibacterial rate against Staphylococcus aureus was 99.3%.

Claims

1. A method for preparing a dressing with compression-rebound controllable sustained-release function, characterized in that: After preparing a warp-knitted spacer fabric with hollow sustained-release fibers as surface fibers and spacer fibers, the warp-knitted spacer fabric is wrapped with a self-repairing hydrogel and the self-repairing hydrogel is allowed to penetrate into the warp-knitted spacer fabric to obtain a dressing with a compression-rebound controllable sustained-release function; The hollow sustained-release fiber is composed of a hollow porous polyester fiber and a filler distributed inside the hollow porous polyester fiber and in the micropores; the filler includes a Schiff base reaction product and nanosilver, and the Schiff base reaction product is a reaction product of polyethylene glycol PEG modified with a dialdehyde group and chitosan; The self-healing hydrogel is a double network structure hydrogel composed of Schiff base structure and ionic bond. In the double network structure, the first network structure is a Schiff base structure formed by the reaction of amino group of polyetherimide and sodium alginate modified with aldehyde group, and the second network structure is the sodium alginate modified with aldehyde group in the first network structure. 2+ Ionic bonds formed by cross-linking reactions.

2. The method for preparing a dressing with compression-rebound controllable sustained-release function according to claim 1, characterized in that: The preparation process of the hollow slow-release fiber is as follows: the hollow porous polyester fiber is divided into two sections, A and B, the A section is immersed in a pressurized container, the pressurized container contains a precursor composite solution, and the temperature is maintained at 40-50° C. The B section is placed in a vacuum container, and the A section is pressurized and the B section is vacuumed respectively. The pressurization and vacuuming process is repeated 3-5 times, and the pressure difference between the A section and the B section is controlled to be 0.05-0.3 MPa. After the reaction is completed, the fiber is washed with anhydrous ethanol and dried in sequence, and then plasma treated to obtain the hollow slow-release fiber. The precursor composite solution is a mixture of solution A and solution B, wherein solution A is a mixed solution of polyethylene glycol modified with a dialdehyde group and silver ions, and solution B is a chitosan solution.

3. The method for preparing a dressing with compression-rebound controllable sustained-release function according to claim 2, characterized in that: The preparation process of the precursor composite solution is as follows: slowly add 0.01 mol·L into a 0.2 g / mL dialdehyde-modified polyethylene glycol solution at a rate of 1 to 2.5 mL / s. -1 silver nitrate solution, keep the polyethylene glycol solution at a constant temperature of 30-40°C during the dropwise addition, and stir for 30-60 minutes to obtain solution A; add chitosan to the mixture of acetic acid and water, stir at 30-36°C for 2-5 hours, and filter 2-4 times to obtain solution B; mix solution A and solution B in equal volumes to obtain a precursor composite solution; The mass ratio of the silver nitrate solution to the polyethylene glycol solution is 1:30-60; the mass fraction of solution B is 1-4%.

4. The method for preparing a dressing with compression-rebound controllable sustained-release function according to claim 2, characterized in that: The plasma treatment process is as follows: the hollow porous polyester fiber after the reaction, cleaning with anhydrous ethanol and drying treatment is placed in the vacuum chamber of a low-pressure cold plasma device, the input power is 150-200W, a mixture of Ar and water vapor is used as the carrier gas, and the gas is introduced into the vacuum chamber at a flow rate of 50-80sccm. In the Ar / water vapor atmosphere, the plasma treatment is performed for 30-50 minutes.

5. The method for preparing a dressing with compression-rebound controllable sustained-release function according to claim 2, characterized in that: The ratio of the lengths of segments A and B is 1:

1.

6. The method for preparing a dressing with compression-rebound controllable sustained-release function according to claim 1, characterized in that: The preparation process parameters of warp knitted spacer fabrics are as follows: Horizontal density: 45 to 60 vertical lines / 5 cm on the front side, 45 to 60 vertical lines / 5 cm on the back side; Vertical density: 45-60 horizontal rows / 5cm on the front side, 50-85 horizontal rows / 5cm on the back side; The spacing wire arrangement density is 100 to 180 pieces / cm 2 The spacing wire arrangement angle is 20-40°, the spacing wire arrangement is "V" shaped, and the surface density is 120-300g / m 2 ; The thickness of the warp knitted spacer fabric is 2.82 to 3.42 mm.

7. The method for preparing a dressing with compression-rebound controllable sustained-release function according to claim 1, characterized in that: The self-repairing hydrogel is used to wrap the warp knitted spacer fabric and the self-repairing hydrogel is allowed to penetrate into the warp knitted spacer fabric. The specific steps are as follows: (1) modifying sodium alginate to obtain aldehyde-modified sodium alginate; (2) dissolving the aldehyde-modified sodium alginate in deionized water to prepare an aldehyde-modified sodium alginate solution having a concentration of 1.5 to 3 wt %; (3) dissolving PEI in deionized water to obtain a PEI solution with a concentration of 1.5 to 3 wt %; (4) Cut the warp knitted spacer fabric into a cylindrical shape and place it in a hollow cylindrical polytetrafluoroethylene mold, wherein the diameter and height of the polytetrafluoroethylene mold are not less than the warp knitted spacer fabric; (5) The aldehyde-modified sodium alginate solution and the PEI solution were mixed in a volume ratio of 7:3 to 3:7, and after being drawn up with a syringe, they were injected into a polytetrafluoroethylene mold from top to bottom until the warp-knitted spacer fabric was immersed. After standing for 10 to 20 minutes, a CaCl2 solution with a concentration of 0.2 to 0.25 mol / L was added, and the mixture was allowed to stand for another 5 to 10 minutes. The polytetrafluoroethylene mold was then placed at 36 to 45°C for 12 to 24 hours to allow it to completely gel and form a self-healing hydrogel, thereby obtaining a dressing with compression-rebound controllable sustained release function.

8. The method for preparing a dressing with compression-rebound controllable sustained-release function according to claim 7, characterized in that: The process of modifying sodium alginate in step (1) is as follows: sodium periodate is added to the sodium alginate solution, and after being placed away from light for 10 to 14 hours, ethylene glycol in an amount equal to that of the sodium periodate is added, and after stirring for 1 to 2.5 hours, the obtained product is first precipitated with excess ethanol, and then filtered and dialyzed, and finally freeze-dried to obtain aldehyde-modified sodium alginate; The concentration of the sodium alginate solution is 2-4wt%, and the mass ratio of sodium periodate to the sodium alginate solution is 1.5-4:

100.

9. The method for preparing a dressing with compression-rebound controllable sustained-release function according to claim 7, characterized in that: The molar ratio of CaCl2 to sodium alginate in step (5) is 2:5.