Hydrogen bond organic framework ion rectification membrane and preparation method and application thereof

By combining self-assembled hydrogen-bonded organic framework porous membranes and amino-functionalized macroporous membranes, a highly selective hydrogen-bonded organic framework ion rectifying membrane was prepared, which solved the problems of low transmission efficiency of nanofluidic ICR membranes and insufficient research on hydrogen-bonded membranes. , achieving high-performance salinity gradient infiltration energy conversion and stability, and improving energy conversion efficiency.

CN118767698APending Publication Date: 2024-10-15NANJING NORMAL UNIVERSITY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410765189.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing nanofluidic ICR membranes are disordered in terms of ion transmission efficiency and selectivity, resulting in low energy conversion efficiency, and there are few studies on hydrogen-bonded organic framework membranes, making it difficult to design and manufacture high-performance ultra-high-selectivity membranes.

Method used

The self-assembled arranged hydrogen-bonded organic skeleton porous membrane is combined with the amino-functionalized macroporous structural membrane material, and the hydrogen-bonded organic skeleton ion rectifying membrane is prepared through solution processing method, using the pores and amino functionalization of the hydrogen-bonded organic skeleton porous membrane. The macropores of the membrane material are connected correspondingly to form a highly selective nanochannel composite membrane.

Benefits of technology

A hydrogen-bonded organic framework ion rectification membrane with stable performance and green environmental protection has been realized, which improves the selectivity and conversion power of salinity gradient osmotic energy conversion, overcomes the process complexity and poor controllability in the existing technology, and exhibits high efficiency. Energy conversion performance and good stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767698A_ABST
    Figure CN118767698A_ABST
Patent Text Reader

Abstract

The invention discloses a hydrogen bond organic framework ion rectification membrane and a preparation method and application thereof. The composite membrane comprises a layer of self-assembled and arranged porous hydrogen bond organic framework membrane and a layer of membrane material with a macroporous structure, holes in the self-assembled and arranged porous hydrogen bond organic framework membrane are correspondingly communicated with part of macropores in the membrane material with the macropore structure, and the hydrogen bond organic framework membrane is assembled through an organic or metal organic building unit under the action of intermolecular hydrogen bonds. The hydrogen bond organic framework material is used as a functional material for the first time and is used for manufacturing the nano-channel ion rectification membrane, and the hydrogen bond organic framework is excellent and stable in performance, mild in preparation condition, simple to operate and environmentally friendly. The prepared hydrogen bond organic framework ion rectification membrane can be used as an ion selective membrane to be applied to salinity gradient energy conversion, and has the advantages of being excellent and stable in performance, high in conversion power and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an ultra-high selectivity hydrogen bond organic skeleton ion rectifying membrane and a preparation method and application thereof, belonging to the field of nano-pore composite membranes. Background Art

[0002] With the continuous growth of energy demand, it is imperative to give priority to the development of efficient, renewable, and completely green energy. Among these energy sources, huge osmotic energy is widely regarded as an environmentally friendly and pollution-free energy source, which can be easily obtained from the salinity gradient energy conversion between seawater and freshwater. Compared with other methods, reverse electrodialysis (RED) is currently the most promising osmotic energy conversion method, which heavily relies on permselective membranes including homogeneous membranes and hybrid membranes. In recent years, bio-nanofluidic ion current rectification (ICR) membranes have shown unprecedented superiority in osmotic energy harvesting. Benefiting from the asymmetry of surface charge, chemical composition or geometric structure, ICR membranes allow ions to pass in one direction but are blocked under reverse bias. Studies have shown that nanofluidic ICR devices can suppress power consumption by blocking reverse current, effectively suppress the common ion concentration polarization (ICP) phenomenon in the process of osmotic energy harvesting, improve the permeability and selectivity of ions, and thus improve the energy conversion efficiency under RED.

[0003] Nanofluidic ICR membranes can be constructed by depositing a variety of materials, including polymers, two-dimensional (2D) nanosheet materials, and mesoporous carbons, on nanoporous supports. However, ion transport in these devices is often disordered due to the inability to precisely design ion channels at the molecular level, ultimately leading to low ion transport efficiency. In contrast, porous framework materials such as metal-organic frameworks (MOFs) and covalent organic frameworks (COFs) have tailorable nanochannel diversity and exhibit structural advantages in osmotic energy conversion. However, the synthesis of these types of polycrystalline membranes usually requires the careful selection of appropriate ligands, which poses certain challenges in large-scale synthesis. Fortunately, hydrogen-bonded organic frameworks (HOFs) are organic building blocks composed of hydrogen bonds that can be dissolved in organic solvents due to the reversibility of hydrogen bonds. This property allows HOF membranes to be prepared by solution processing methods without the need for complex ligand selection procedures. In addition, while retaining their crystalline nanoporous structure, HOFs offer several interesting advantages over other framework materials, including low cost, ease of purification, and the ability to heal by simple recrystallization. Despite this apparent advantage, there is little research on HOF membranes, which may be due to the difficulty in growing 2D HOFs due to the poor coherence between long-range single crystals and ordered single crystals. Therefore, designing and fabricating an ultrahighly selective hydrogen-bonded organic framework ion rectifying membrane is expected to further promote the development of high-performance energy conversion. Summary of the invention

[0004] Purpose of the invention: The first purpose of the present invention is to provide an ultra-high selectivity hydrogen-bonded organic skeleton ion rectifying membrane, which has stable performance and is green and environmentally friendly. The second purpose of the present invention is to provide a method for preparing a hydrogen-bonded organic skeleton ion rectifying membrane, which is simple to operate, mild in conditions and easy to implement. The third purpose of the present invention is to provide the application of the hydrogen-bonded organic skeleton ion rectifying membrane in salinity gradient osmotic energy conversion. The plasma electron sponge nanochannel composite membrane can be used in reverse electrodialysis technology to capture salinity gradient osmotic energy, and has the advantages of stable performance, high conversion power, and a wide range of applicable environments.

[0005] Technical solution: The present invention discloses a hydrogen-bonded organic skeleton ion rectifying membrane, which comprises a layer of self-assembled hydrogen-bonded organic skeleton porous membrane and a layer of amino-functionalized membrane material with a macroporous structure, wherein the pores in the self-assembled hydrogen-bonded organic skeleton porous membrane correspond to and communicate with part of the macropores in the amino-functionalized membrane material with a macroporous structure.

[0006] Furthermore, the membrane material with a macroporous structure is selected from one of anodized aluminum membrane (AAO), titanium dioxide nanotube array membrane (TNT), polycarbonate membrane (PC), cellulose membrane (NC), polytetrafluoroethylene membrane (PTFE) or polyvinylidene fluoride membrane (PVDF), preferably AAO.

[0007] Furthermore, the pore size of the amino-functionalized membrane material with a macroporous structure is 50-100 nm, preferably 60 nm.

[0008] Furthermore, the hydrogen-bonded organic framework porous membrane is assembled by organic or metal organic building units through intermolecular hydrogen bonding.

[0009] Furthermore, the thickness of the hydrogen-bonded organic skeleton porous membrane is 0.33-1.88 μm, preferably 0.60 μm.

[0010] Furthermore, the diameter of the pores of the hydrogen-bonded organic skeleton porous membrane is 0.8-3.0 nm, preferably 2.5 nm.

[0011] The method for preparing the hydrogen-bonded organic framework ion rectifying membrane of the present invention comprises the following steps:

[0012] (1) dissolving the organic ligand compound in N,N-dimethylformamide (DMF) and subjecting the mixture to ultrasonic treatment to obtain a uniform mixed solution;

[0013] (2) placing the amino-functionalized membrane with a macroporous structure together with the mixed solution in a reaction container, adding a catalyst, and fixing at room temperature to ensure that the formation of the first layer of hydrogen-bonded organic framework porous membrane is completed;

[0014] (3) dissolving the organic ligand compound in a solvent, adding the mixture into a reaction vessel, and heating the mixture for reaction to obtain a yellow continuous hydrogen bond organic framework ion rectifying film.

[0015] Furthermore, the organic ligand compound is a tetradentate carboxylic acid compound.

[0016] Furthermore, the tetradentate carboxylic acid compound is one or more of pyrenetetracarboxylic acid, pyrenyltetrabenzoic acid, pyrenyl-tetraphenyl-benzoic acid, pyrenyl-tetranaphthalene-benzoic acid, biphenyltetracarboxylic acid, and biphenyltetrabenzoic acid.

[0017] Furthermore, in step (1), the concentration of the organic ligand compound in the mixed solution is 5-30 mmol / L, preferably 15 mmol / L, and the ultrasonic treatment time is 5-20 min.

[0018] Furthermore, in step (2), the catalyst is EDC and NHS.

[0019] Furthermore, in step (2), the mass volume ratio of the catalyst EDC and NHS to the mixed solution is 20-60:5-30:2 mg / mg / mL, preferably 40:10:2 mg / mg / mL.

[0020] Furthermore, in step (2), the reaction liquid in the reactor is immersed in the amino-functionalized macroporous membrane for a fixed time at room temperature of 6-12 hours, preferably 12 hours.

[0021] Furthermore, in step (3), the solvent is one or more of ethanol, acetone, N,N-dimethylformamide and dimethyl sulfoxide. Preferably, the solvent is a mixed solution of ethanol and dimethyl sulfoxide, wherein the volume ratio of ethanol to dimethyl sulfoxide is 3:1.

[0022] Furthermore, in step (3), by controlling the concentration of the organic ligand compound in the solvent, self-assembled hydrogen-bonded organic skeleton porous membranes of different thicknesses can be obtained.

[0023] Furthermore, in step (3), the concentration of the organic ligand compound in the solvent is 10-50 mmol / L, preferably 22 mmol / L.

[0024] Furthermore, in step (3), the heating reaction temperature is 25-100°C, preferably 80°C, and the heating reaction time is 8-48h, preferably 24h.

[0025] The application of the hydrogen-bonded organic framework ion rectifying membrane described in the present invention in salinity gradient energy conversion.

[0026] Furthermore, during the salinity gradient energy conversion process, a salinity difference is formed between the concentrated salt solution and the dilute salt solution, and the salt difference energy is converted into electrical energy.

[0027] Furthermore, the molar concentration of the concentrated salt solution is 0.1-5 mol / L, and the molar concentration of the dilute salt solution is 0.0001-0.01 mol / L.

[0028] Furthermore, the concentrated salt solution and the dilute salt solution are each one of a sodium chloride solution, a potassium chloride solution, a magnesium chloride solution, a lithium bromide solution and a calcium chloride solution.

[0029] Furthermore, the concentrated salt solution and the dilute salt solution are of the same type.

[0030] Furthermore, the preparation of the amino-functionalized membrane material having a macroporous structure comprises the following steps:

[0031] (3-Aminopropyl)triethoxysilane (APTES) was diluted in ethanol, mixed thoroughly, immersed in the macroporous structure membrane material, and allowed to stand overnight to obtain an amino-functionalized macroporous structure membrane material.

[0032] Furthermore, the volume ratio of the APTES solution to the ethanol solution is 1:1-9, preferably 1:9, and the immersion time is more than 12 hours.

[0033] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0034] (1) The hydrogen-bonded organic skeleton ion rectifying membrane of the present invention comprises a self-assembled hydrogen-bonded organic skeleton porous membrane. The hydrogen-bonded organic skeleton ion rectifying membrane has stable performance, is green and environmentally friendly, and has a simple preparation method, mild conditions and is easy to implement, thus overcoming the shortcomings of the prior art of complex process and poor controllability.

[0035] (2) The hydrogen-bonded organic framework ion rectifying membrane of the present invention is applied to salinity gradient osmotic energy conversion and has obvious advantages:

[0036] 1) The amino groups on the surface of the membrane material with a macroporous structure functionalized by amino groups react with the monomer H4TBAPy containing four symmetrical carboxyl groups to form the first layer of HOF membrane on the surface of the membrane material with a macroporous structure. Then, the solvent modulation strategy is used to induce the rearrangement of hydrogen bonds to obtain a uniform and thin HOF membrane on the membrane material with a macroporous structure.

[0037] 2) The presence of a large number of unprotonated carboxyl groups in HOF gives it more surface negative charge and excellent hydrophilicity, which enhances the percharge selectivity for efficient osmotic energy conversion.

[0038] 3) The prepared hydrogen-bonded organic skeleton nanochannel membrane has unique ICR characteristics, which effectively suppresses the polarization of ion concentration and further improves its selectivity. Under a 500-fold NaCl gradient, its power density is 75.2 W m -2 , which is better than most nanoporous membranes (7.0-30.0 W m -2 ).

[0039] 4) The hydrogen-bonded organic framework ion rectifying membrane of the present invention exhibits good stability in the application of salinity gradient osmotic energy conversion. After 15 days of testing, the energy conversion power has almost no attenuation, laying a solid foundation for practical application. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 A schematic diagram of the preparation process of the hydrogen-bonded organic framework ion rectifying membrane prepared in Example 1;

[0041] Figure 2 The scanning electron microscope image of the AAO membrane prepared in Example 1; wherein A is the top image of the AAO membrane, and B is the cross-sectional image of the AAO membrane;

[0042] Figure 3The scanning electron microscope image of the hydrogen-bonded organic framework ion rectifying membrane prepared in Example 1; wherein A is a top view of the hydrogen-bonded organic framework ion rectifying membrane, B is a back view of the hydrogen-bonded organic framework ion rectifying membrane, C is a cross-sectional view of the hydrogen-bonded organic framework ion rectifying membrane, and D is an AAO pipeline image of a cross-sectional portion of the hydrogen-bonded organic framework ion rectifying membrane;

[0043] Figure 4 IV curves of the hydrogen-bonded organic framework ion rectifying membrane prepared in Example 1 in KCl solutions of different concentrations;

[0044] Figure 5 This is a schematic diagram of the salinity gradient osmotic energy conversion device in Example 5;

[0045] Figure 6 The current density and external resistance relationship diagrams and the power density and external resistance relationship diagrams obtained in the salinity gradient osmotic energy conversion of hydrogen-bonded organic framework ion rectifying membranes of different thicknesses in Examples 1-5, wherein A is the current density and external resistance relationship diagram, and B is the power density and external resistance relationship diagram;

[0046] Figure 7 This is a comparison diagram of the maximum output power density obtained by the hydrogen-bonded organic framework ion rectifying membrane in Example 1 and the existing membrane material in Comparative Example 1 in salinity gradient osmotic energy conversion;

[0047] Figure 8 This is a graph showing the test results of salinity gradient osmotic energy conversion of the hydrogen-bonded organic framework ion rectifying membrane in Example 5 within 15 days. DETAILED DESCRIPTION

[0048] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0049] Example 1 Preparation of Hydrogen Bond Organic Framework Ion Rectification Membrane

[0050] (1) Preparation of anodized aluminum (AAO) membrane: First, the aluminum foil was ultrasonically cleaned with acetone and 1 mol / L KOH for 10 minutes respectively, and then rinsed with water. The first anodization was carried out with 0.3 mol / L oxalic acid as the electrolyte at 50 V for 30 minutes. In order to eliminate the irregular oxide layer formed, the first anodized aluminum foil was treated with a mixed acid solution consisting of 6 wt% H3PO4 and 1.8 wt% H2CrO4 at 60°C for 40 minutes. Subsequently, the second anodization was carried out for 4 hours, and the other conditions were the same as the first anodization. The aluminum substrate was removed with a saturated SnCl2 solution. The AAO membrane was treated with a 1.8 wt% H3PO4 solution for 40 minutes to remove the barrier layer. The prepared AAO membrane was then immersed in a hydrogen peroxide solution (30% H2O2) and boiled for 30 minutes, and a large number of hydroxyl groups were generated on the channel surface. Finally, the AAO membrane was soaked in water overnight and dried. The pore size of the nanochannels in the anodic aluminum oxide membrane can be controlled by adjusting the oxidation voltage. The AAO membrane prepared in this example was analyzed by scanning electron microscopy. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that the pore size of the AAO membrane is 60 nm and the pores are evenly distributed.

[0051] (2) APTES modified AAO membrane: The AAO membrane was immersed in a 10% APTES solution for more than 12 h, then rinsed with ethanol three times, and placed in an oven for 6 h to obtain an APTES modified AAO membrane, thereby successfully modifying the amino group with AAO.

[0052] (3) Preparation of hydrogen-bonded organic framework ion rectifying membrane: 1,3,6,8-tetramolecular (p-benzoic acid) pyrene (H4TBAPy; 10 mg, 0.015 mmol) was dissolved in 1 mL of DMF. Then, the solution was ultrasonically treated for 10 min to obtain a uniform system. The mixed system of APTES-modified AAO membrane and H4TBAPy (10 mg) was then placed at the bottom of the reaction vessel. EDC 20 mg and NHS 5 mg were added and fixed at room temperature for 12 h to ensure that the formation of the first layer of HOF membrane was complete. Then, H4TBAPy (30 mg, 0.045 mmol) was dissolved in 2 mL of ethanol / dimethyl sulfoxide mixed solvent (ethanol / dimethyl sulfoxide is v / v = 3 / 1). Continue to add to the bottom of the reaction container and react at 80 °C for 24 h to obtain a yellow continuous HOF membrane, namely a hydrogen-bonded organic framework ion rectifying membrane. The entire preparation process is as follows Figure 1 shown.

[0053] The hydrogen-bonded organic framework ion rectifying film layer prepared in this embodiment was analyzed by scanning electron microscope, and the thickness of the hydrogen-bonded organic framework porous structure of the hydrogen-bonded organic framework ion rectifying film was found to be 0.6 μm. Figure 3 shown. Figure 3The scanning electron microscope image of the hydrogen-bonded organic framework ion rectifying membrane prepared in Example 1, wherein A is the top image of the hydrogen-bonded organic framework ion rectifying membrane, B is the back image of the hydrogen-bonded organic framework ion rectifying membrane, C is the cross-sectional image of the hydrogen-bonded organic framework ion rectifying membrane, and D is the AAO pipeline image of the cross-sectional part of the hydrogen-bonded organic framework ion rectifying membrane. Figure 3 It can be seen that the hydrogen-bonded organic skeleton pores are tightly covered on the top of the AAO nanochannels, indicating the successful preparation of the hydrogen-bonded organic skeleton ion rectifying membrane.

[0054] Example 2 Experimental process of preparing hydrogen bonded organic framework ion rectifying membranes with different thicknesses

[0055] The preparation process is the same as that of Example 1. Compared with Example 1, the concentration of the casting solution of Example 1 (i.e., H4TBAPy dissolved in an ethanol / dimethyl sulfoxide mixed solution) is changed to adjust. H4TBAPy is dissolved in an ethanol / dimethyl sulfoxide mixed solution to obtain mixed solutions containing different concentrations of H4TBAPy (10 g / L, 30 g / L, 90 g / L, 120 g / L), which are slowly added to the surface of the functionalized porous AAO substrate. The reaction is carried out at 80°C for 24 hours to obtain continuous HOF films of different thicknesses. By electron microscopy analysis, the thicknesses of the hydrogen-bonded organic framework porous membranes of the hydrogen-bonded organic framework ion rectifying membranes are 0.33 μm, 0.60 μm, 0.82 μm, and 1.88 μm, respectively.

[0056] Example 3 Application of Hydrogen Bond Organic Framework Ion Rectifier Membrane in Salinity Gradient Osmotic Energy Conversion

[0057] The hydrogen bonded organic framework ion rectifying membrane prepared in Example 1 was sandwiched between two silica gel gaskets and placed in the middle of a H- two-chamber electrochemical cell. In order to study the effect of electrolyte concentration on ion current rectification, KCl solutions of different concentrations of electrolyte were added to the cell. A pair of Ag / AgCl electrodes was used as the transmembrane potential, and a scanning voltage of -1.0V to +1.0V was applied. The results are shown in FIG. Figure 4 shown. Figure 4 The IV curve of HOF / AAO at different KCl concentrations. Figure 4 It can be seen that the ionic current increases with the increase of electrolyte concentration due to the enhancement of ionic strength. Interestingly, with the increase of electrolyte concentration, the ICR ratio first increases and then decreases. The reason for explaining this rule is that KCl is a monovalent salt with the same anion, which causes the surface charge of HOF / AAO to attract counterions and form an electrical double layer (EDL). When the EDL thickness matches the nanochannel radius, the ICR ratio reaches a maximum. The EDL thickness decreases with the increase of electrolyte concentration. When the KCl concentration increases from 0.001mM to 10mM, the ionic strength and current increase, and the ICR ratio increases. However, when the KCl concentration exceeds 10mM, the ICR ratio decreases due to incomplete EDL overlap.

[0058] Example 4 Application of salinity gradient osmotic energy conversion of hydrogen-bonded organic framework ion rectifying membranes of different thicknesses

[0059] 1. Salinity gradient osmotic energy conversion device such as Figure 5 As shown, the salinity gradient osmotic energy conversion device is a homemade H-two-chamber electrochemical cell, the hydrogen-bonded organic framework ion rectifying membrane is sandwiched between the two electrochemical cells, and the entire device is fixed by screws. A concentrated salt solution (0.01M NaCl electrolyte solution) is placed on the large pore end of the composite membrane, i.e., the side of the anodized aluminum membrane, and a dilute salt solution (5M NaCl electrolyte solution) is placed on the small pore end of the composite membrane, i.e., the side of the hydrogen-bonded organic framework porous membrane. The two salt solutions are connected to the circuit through an external electrochemical workstation and a load resistor, and the measurement of the relationship curve between current density, power density and external resistance is achieved by adjusting the change in the external resistance value.

[0060] 2. Salinity gradient osmotic energy conversion of hydrogen-bonded organic framework ion rectifying membranes with different thicknesses

[0061] The salinity gradient osmotic energy conversion device in step 1 was used, and the composite membranes in the salinity gradient osmotic energy conversion device were replaced by the hydrogen-bonded organic framework ion rectifying membranes prepared in Example 1 and Example 2, respectively. Other conditions remained unchanged, and the effect of the thickness of the hydrogen-bonded organic framework ion rectifying membrane on the salinity gradient osmotic energy conversion performance was tested. The results are as follows: Figure 6 shown.

[0062] Figure 6 The current density, power density and external resistance relationship diagrams obtained in the salinity gradient osmotic energy conversion of hydrogen bonded organic framework ion rectifying membranes of different thicknesses in Example 1 and Example 2, wherein (A) is a current density and external resistance relationship diagram, (B) is a power density and external resistance relationship diagram, and Figure 6 It can be found that when the thickness of the hydrogen-bonded organic skeleton porous membrane is 0.33 μm, 0.60 μm, 0.82 μm and 1.88 μm, respectively, under the 0.01M:0.5M NaCl gradient, the corresponding external circuit power density is 42 W / m 2 、75.2W / m 2 、37W / m 2 and 29W / m 2 When the thickness of the hydrogen bonded organic skeleton porous membrane is within 0.60 μm, its salinity gradient osmotic energy conversion output power is the highest. The performance of membranes of these thicknesses meets the commercial standard of 5W / m 2 .

[0063] Comparative Example 1

[0064] The following have been publicly reported:

[0065] UiO-66-NH2@ANM membrane: Y.-C. Liu, Y.-C. Yeh, M.-J. Zheng, M.-J. Wu, Sci. Adv. 2021, 7, 9924;

[0066] BDA-TAM COF membrane: C. Wang, J. Tang, L. Li, J. Wan, Y. Ma, Y. Jin, J. Liu, H. Wang, Q. Zhang, Adv. Funct. Mater. 2022, 32, 2204068;

[0067] TFP-TPACOF@ANM membrane: Y. Sun, K. Zhou, H. Xiao, W. Chen, L. Yang, W. Xin, X.-Y. Kong, Z. Xu, L. Jiang, L. Wen, Nano Energy 2023, 105, 108011;

[0068] BCP membrane: C. Li, L. Wen, X. Sui, Y. Cheng, L. Gao, L. Jiang, Sci. Adv. 2021, 7, 2183;

[0069] CS / SA membrane: G. Bian, N. Pan, Z. Luan, X. Sui, W. Fan, Y. Xia, K. Sui, L. Jiang, Angew. Chem. Int. Ed. 2021, 60, 20294;

[0070] PlL membrane: Y. Hu, Y. Teng, Y. Sun, P. Liu, L. Fu, L. Yang, X.-Y. Kong, Q. Zhao, L. Jiang, L. Wen, Nano Energy 2022, 97, 107170;

[0071] MoS2 membrane: C. Zhu, P. Liu, B. Niu, Y. Liu, W. Xin, W. Chen, X.-Y. Kong, Z. Zhang, L. Jiang, L. Wen, J. Am. Chem. Soc 2021, 143, 1932;

[0072] bsGOM membrane: Y. Qian, D. Liu, G. Yang, L. Wang, Y. Liu, C. Chen, X. Wang, W. Lei, J. Am. Chem. Soc 2022, 144, 13764;

[0073] BHMXM membrane: L.Ding, M.Zheng, D.Xiao, Z.Zhao, J.Xue, S.Zhang, J.Caro, H.Wang, Angew.Chem.Int.Ed.2022,61,e202206152;

[0074] KANF membrane: L. Ding, D. Xiao, Z. Zhao, Y. Wei, J. Xue, H. Wang, Adv. Sci. 2022, 9, 2202869;

[0075] ICM film: W.Chen, T.Dong, Y.Xiang, Y.Qian, X.Zhao, W.Xin, XYKong, L.Jiang, L.Wen, Adv.Mater.2021,34,2108410;

[0076] SSGOMs membrane: S.H. Liu, D. Zhang, Y.P. Fang, Z.X. Liang, Z.K. Zhao, X.C. Chen, J. Yao, L. Jiang, Adv. Funct. Mater. 2022, 33, 2211532;

[0077] MXene / PS-b-P2VP membrane:

[0078] SPEEK / AAO / ppy membrane: Y.Zhao, J.Wang, X.-Y.Kong, W.Xin, T.Zhou, Y.Qian, L.Yang, J.Pang, L.Jiang, L.Wen, Natl.Sci.Rev.2020,7,1349;

[0079] p-BCPS membrane: C.Li, H.Jiang, P.Liu, Y.Zhai, X.Yang, L.Gao, L.Jiang, J.Am.Chem.Soc2022,144,9472.

[0080] The salinity gradient osmotic energy conversion output power density of the above existing membrane is compared with the salinity gradient osmotic energy collection performance of the hydrogen bonded organic framework ion rectifying membrane (our work) in Example 1. The results are as follows Figure 7 shown. Figure 7This is a comparison chart of the maximum output power density obtained by the hydrogen bond organic framework ion rectifying membrane in Example 1 and the existing membrane material in Comparative Example 1 in salinity gradient osmotic energy conversion. Figure 7 The comparison results show that the existing membrane materials in ratio 1 follow the above order under the salinity gradient of 0.01M:5M, and the corresponding external circuit power density is 7.12W / m 2 、7.33W / m 2 、27.8W / m 2 、22.4W / m 2 、19.4W / m 2 、15.5W / m 2 、15.6W / m 2 、18.8W / m 2 、17.8W / m 2 、15.0W / m 2 、23.6W / m 2 、24.9W / m 2 、12.4W / m 2 、26.2W / m 2 and 30.8W / m 2 , which is much lower than the external circuit power density of 75.2 W / m of the hydrogen bond organic framework ion rectifying membrane in Example 1. 2 .

[0081] Example 5 Stability test of salinity gradient osmotic energy conversion of hydrogen-bonded organic framework ion rectifying membrane

[0082] The hydrogen bond organic skeleton ion rectifying membrane with a thickness of 0.6 μm in Example 1 was placed for 1 day, 3 days, 5 days, 7 days, 9 days, 11 days, and 15 days to perform salinity gradient osmotic energy conversion tests. The process after the test was the same as in Example 3, and other conditions remained unchanged. The results are shown in Figure 8 shown.

[0083] Figure 8 The figure is a test result of the salinity gradient osmotic energy conversion of the hydrogen bond organic framework ion rectifying membrane in Example 1 within 15 days. Figure 8 The experimental results show that the hydrogen-bonded organic framework ion rectifying membrane prepared in Example 1 shows good stability in the application of salinity gradient osmotic energy conversion. After 15 consecutive days of testing, the output power density is less than 10%, which lays a reliable foundation for subsequent practical applications.

Claims

1. A hydrogen-bonded organic framework ion rectifying membrane, characterized in that: The hydrogen-bonded organic skeleton ion rectifying membrane comprises a layer of self-assembled hydrogen-bonded organic skeleton porous membrane and a layer of amino-functionalized membrane material with macroporous structure. The pores in the self-assembled hydrogen-bonded organic skeleton porous membrane correspond to and communicate with part of the macropores in the amino-functionalized membrane material with macroporous structure.

2. The hydrogen-bonded organic framework ion rectifying membrane according to claim 1, characterized in that: The membrane material with a macroporous structure is selected from one of an anodic aluminum oxide membrane, a titanium dioxide nanotube array membrane, a polycarbonate membrane, a cellulose membrane, a polytetrafluoroethylene membrane or a polyvinylidene fluoride membrane, and the pore size of the amino-functionalized membrane material with a macroporous structure is 50-100 nm.

3. The hydrogen-bonded organic framework ion rectifying membrane according to claim 1, characterized in that: The hydrogen-bonded organic framework porous membrane is composed of organic or metal organic building units assembled through intermolecular hydrogen bonding. The thickness of the hydrogen-bonded organic framework porous membrane is 0.33-1.88 μm, and the diameter of the pores of the hydrogen-bonded organic framework porous membrane is 0.8-3.0 nm.

4. The method for preparing the hydrogen-bonded organic framework ion rectifying membrane according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) dissolving the organic ligand compound in N,N-dimethylformamide (DMF) and subjecting the mixture to ultrasonic treatment to obtain a uniform mixed solution; (2) placing the amino-functionalized membrane with a macroporous structure together with the mixed solution in a reaction container, adding a catalyst, and fixing at room temperature to ensure that the formation of the first layer of hydrogen-bonded organic framework porous membrane is completed; (3) dissolving the organic ligand compound in a solvent, adding the mixture into a reaction vessel, and heating the mixture for reaction to obtain a hydrogen bonded organic framework ion rectifying membrane.

5. The preparation method according to claim 4, characterized in that: The organic ligand compound is a tetradentate carboxylic acid compound. In step (1), the concentration of the organic ligand compound in the mixed solution is 5-30 mmol / L, and the ultrasonic treatment time is 5-20 min.

6. The preparation method according to claim 4, characterized in that: In step (2), the catalyst is EDC and NHS, the mass volume ratio of the catalyst EDC and NHS to the mixed solution is 20-60:5-30:2 mg / mg / mL, the reaction liquid in the reactor immerses the amino-functionalized membrane with a macroporous structure, and the fixed time at room temperature is 6-12 hours.

7. The preparation method according to claim 4, characterized in that: In step (3), the solvent is one or more of ethanol, acetone, N,N-dimethylformamide and dimethyl sulfoxide. By controlling the concentration of the organic ligand compound in the solvent, a self-assembled hydrogen-bonded organic skeleton porous membrane of different thicknesses can be obtained. The concentration of the organic ligand compound in the solvent is 10-50 mmol / L, the temperature of the heating reaction is 25-100°C, and the time of the heating reaction is 8-48h.

8. Application of the hydrogen-bonded organic framework ion rectifying membrane according to any one of claims 1 to 3 in salinity gradient energy conversion.

9. The use according to claim 8, characterized in that: During the salinity gradient energy conversion process, a salinity difference is formed between the concentrated salt solution and the dilute salt solution, and the salt difference energy is converted into electrical energy. The molar concentration of the concentrated salt solution is 0.1-5 mol / L, and the molar concentration of the dilute salt solution is 0.0001-0.01 mol / L.

10. The use according to claim 8, characterized in that: The concentrated salt solution and the dilute salt solution are both one of sodium chloride solution, potassium chloride solution, magnesium chloride solution, lithium bromide solution and calcium chloride solution, and the concentrated salt solution and the dilute salt solution are of the same type.

Citation Information

Cited By

  • Humidity sensor based on hydrogen bond organic framework material and preparation method

    CN119936135A

  • Humidity sensor based on hydrogen-bonded organic framework material and preparation method thereof

    CN119936135B