Method for preparing high-thermal-conductivity polycrystalline diamond at high temperature and high pressure
By mixing carbon source and catalyst under high temperature and high pressure conditions for powder mixing and pressure forming, the problems of slow growth rate and low thermal conductivity of polycrystalline diamond in traditional methods are solved, and high-efficiency, low-cost high thermal conductivity diamond is achieved. preparation.
Patent Information
- Application Number
- CN202410168117.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-02-06
AI Technical Summary
The growth rate of polycrystalline diamond synthesized by the traditional CVD method is slow, and the polycrystalline diamond prepared by the HPHT method has low thermal conductivity and high cost, and cannot meet the high thermal conductivity requirements.
Under high-temperature and high-pressure conditions, the carbon source and catalyst are mixed and batched, and are pressurized and molded through a mold to form a prefabricated synthetic raw material, which is then subjected to high-temperature and high-pressure treatment in a quasi-static high-pressure equipment to remove the catalyst to obtain polycrystalline diamond with high thermal conductivity. piece.
The growth rate and thermal conductivity of diamond are significantly improved, and the cost of raw materials is reduced. The prepared polycrystalline diamond material has large particle size and high bonding density, and the thermal conductivity reaches ≥600W/K·m.
Smart Images

Figure CN118767804A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of device thermal management materials and electromagnetic shielding material preparation, and more specifically, to a method for preparing high-thermal conductivity polycrystalline diamond under high temperature and high pressure. Background Art
[0002] As the power of semiconductor devices increases, their heat generation increases significantly, which causes the local temperature to continue to rise, causing the actual effective power of the semiconductor devices to decrease due to the temperature rise.
[0003] High thermal conductivity materials can quickly conduct heat away, ensuring the efficient use of high-frequency, high-power devices. Diamond has an intrinsic thermal conductivity of over 2000W / K·W, and polycrystalline diamond produced by chemical vapor deposition (CVD) can have a thermal conductivity of over 1000W / K·W, making high thermal conductivity diamond an ideal heat sink for high-frequency, high-power semiconductor devices.
[0004] For example, Chinese patent CN1274878C discloses a chemical vapor deposition (CVD) polycrystalline diamond composite diamond material and its application, which discloses three structures: 1. A CVD diamond layer with a thickness of more than 0.01 mm is grown on the surface of the polycrystalline diamond to form a CVDD-PCD composite. 2. The CVDD-PCD composite is welded to a cemented carbide substrate to form a CVDD-PCD-wC(Co) three-layer composite. 3. A CVD diamond layer with a thickness of more than 0.01 mm is grown on the surface of the polycrystalline diamond composite sheet to form a CVDD-PCD three-layer composite. However, this method is very slow in synthesizing polycrystalline diamond.
[0005] Chinese patent CN2104947068A discloses a method for preparing a diamond heat sink, addressing the slow growth rate, rough surface, and low thermal conductivity of diamond produced using existing MWCVD methods. The method involves: 1. slicing a silicon wafer and ultrasonically cleaning it to obtain a clean silicon wafer substrate; 2. uniformly coating the clean silicon wafer substrate with nanodiamonds; 3. placing the diamond-coated silicon wafer in an MWCVD apparatus, introducing hydrogen and methane for chemical vapor deposition; and 4. etching the silicon substrate with a mixed solution of HNO3 and HF, followed by cleaning to obtain the diamond heat sink. However, the growth rate of the diamond film obtained using this CVD deposition method is limited to 2-5 μm / h.
[0006] Since the growth rate of polycrystalline diamond synthesized by CVD is usually only 10 microns / hour, the growth rate of single crystal diamond synthesized by CVD, although higher than that of polycrystalline diamond, is still only ≤20μm / h. In addition, due to the size limitation of diamond seed crystal, the current size of synthetic diamond single crystal is usually ≤10mm×10mm, and the cost is high, which seriously restricts its promotion and application.
[0007] In addition to CVD technology, high temperature and high pressure (HPHT) is also a commonly used method for synthesizing diamond. People have always wanted to use the HPHT method to prepare polycrystalline diamond with high thermal conductivity.
[0008] For example, Chinese patent CN115959659A discloses a method for preparing polycrystalline diamond, which involves sintering at least one diamond powder to form polycrystalline diamond.
[0009] For example, Chinese patent CN106694887A discloses a method for preparing a polycrystalline diamond composite sheet, which uses cemented carbide as a matrix, assembles diamond powder with the matrix, and presses it into shape to obtain a blank; the blank is then kept at a pressure of 4 to 5.5 GPa and a temperature of 1100°C to 1600°C for 10 to 180 seconds; the pressure is then increased to 5 to 8 GPa, the temperature is increased to 1400°C to 2000°C, and the temperature is kept at this temperature for 5 to 40 minutes.
[0010] However, since diamond conducts heat via phonons, the continuity of the lattice is key to ensuring its high thermal conductivity. Therefore, the thermal conductivity of polycrystalline diamond materials synthesized using diamond powder and catalyst under HPHT conditions is usually ≤500W / K·W, which cannot meet the high thermal conductivity requirements.
[0011] Figure 1 a is a schematic diagram of the process of traditional HPHT synthetic polycrystalline diamond preparation method. Figure 1 As shown in Figure a, in the traditional HPHT polycrystalline diamond synthesis process, diamond powder is subjected to high-pressure extrusion, causing the particles to break and rearrange, increasing their packing density. Subsequently, with the assistance of a catalyst such as cobalt or transition metals such as iron, nickel, and their alloys, diamond necks form between the diamond particles, ultimately forming a polycrystalline diamond compact with a continuous diamond skeleton structure. The polycrystalline diamond compacts produced by this method have an average diamond grain size of ≤30μm, numerous grain boundaries, a low diamond neck density, and a high amount of residual metal catalyst on the grain boundaries. These factors significantly reduce the thermal conductivity of HPHT-synthesized polycrystalline diamond.
[0012] Based on this, there is an urgent need to find a method for preparing low-cost and high-thermal conductivity polycrystalline diamond. Summary of the Invention
[0013] In view of the above problems, the purpose of the present invention is to provide a method for preparing high thermal conductivity polycrystalline diamond under high temperature and pressure to solve the problems of slow diamond growth rate and low preparation efficiency in the traditional CVD method for synthesizing polycrystalline diamond, as well as small grain size and low necking density in the polycrystalline diamond composite sheets synthesized by traditional HPHT.
[0014] The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure provided by the present invention comprises the following steps:
[0015] Preparation of raw material block: a raw material carbon source and a catalyst are mixed and the mixture is pressurized and formed into a prefabricated synthetic raw material carbon source through a mold; the prefabricated synthetic raw material carbon source and prefabricated assembly components are then assembled together to form an integral synthetic block;
[0016] High temperature and high pressure growth: placing the entire synthetic block into a quasi-static high pressure device and subjecting it to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth;
[0017] Sample post-processing: crushing the entire synthetic block after the high temperature and high pressure treatment to peel off the polycrystalline diamond sheet sample;
[0018] Removing the catalyst: removing the catalyst on the polycrystalline diamond sheet sample to obtain a polycrystalline diamond sheet with high thermal conductivity.
[0019] In addition, a preferred solution is that the raw carbon source includes graphite with a purity of not less than 80%, and the catalyst includes at least one of iron, nickel, cobalt and their alloy powders; the ingredient ratio of the mixed sample is: graphite: catalyst in the range of 20:1 to 1:1.
[0020] In addition, a preferred solution is that the raw carbon source includes diamond micropowder and graphite with a purity of not less than 80%, and the catalyst includes at least one of iron, nickel, cobalt and their alloy powders; the ratio of the mixed sample is: the ratio of graphite: diamond micropowder ranges from 100:1 to 20:1, and the ratio of graphite and diamond mixed carbon source: catalyst ranges from 20:1 to 1:1.
[0021] In addition, a preferred solution is that the prefabricated synthetic raw material is a sheet structure with a thickness of not less than 1 mm.
[0022] In addition, a preferred solution is that the prefabricated assembly elements include thermal insulation sheets, heating sheets, heating plugs and pyrophyllite cubes.
[0023] In addition, a preferred solution is that the high temperature and high pressure treatment is performed using a pre-set synthesis pressure program, including:
[0024] Pressurizing to 5-8 GPa at a pressurizing rate of 0.1-2 GPa / min, then heating to 1200-2000°C at a heating rate of 200-2000K / min; maintaining the temperature at 1200-2000°C for a predetermined time to grow diamond; and,
[0025] After the heat preservation and pressure maintenance growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 20-4000K / min and in a segmented multi-stage pressure relief manner.
[0026] In addition, a preferred solution is that the preset time is 10 to 150 minutes.
[0027] In addition, a preferred solution is to crush and peel off the polycrystalline diamond sheet sample, clean it in a high-temperature water bath, air-dry it to remove moisture, and then grind and polish it.
[0028] In addition, a preferred solution is to remove the catalyst on the polycrystalline diamond sheet sample, comprising:
[0029] placing the polycrystalline diamond sheet sample in an acid solution and heating it to remove the catalyst;
[0030] Using deionized water to ultrasonically clean the surface of the polycrystalline diamond sheet sample to remove residual acid;
[0031] The moisture on the surface of the polycrystalline diamond sheet sample is removed by drying.
[0032] In addition, a preferred solution is that the average particle size of the prepared high thermal conductivity polycrystalline diamond sheet is ≥40 μm, and the thermal conductivity is ≥600 W / K·m.
[0033] On the other hand, the present invention also provides another method for preparing high thermal conductivity polycrystalline diamond at high temperature and high pressure, comprising the following steps:
[0034] Preparation of raw material blocks: Mix the raw carbon source powders and ingredients to form a mixed sample, and pressurize the mixed sample through a mold to prepare a standard carbon source; then assemble the standard carbon source and catalyst together as prefabricated raw materials with assembly components to form an integral synthetic block;
[0035] High temperature and high pressure growth: placing the entire synthetic block into a quasi-static high pressure device and subjecting it to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth;
[0036] Sample post-processing: crushing the entire synthetic block after the high temperature and high pressure treatment to peel off the polycrystalline diamond sheet sample;
[0037] Acid leaching to remove the catalyst: removing the catalyst on the polycrystalline diamond sheet sample to obtain a polycrystalline diamond sheet with high thermal conductivity.
[0038] In addition, a preferred solution is that the raw carbon source is carbon or graphite with a purity greater than 90%, and the catalyst is a transition metal catalyst sheet or a cemented carbide matrix; wherein the graphite and the catalyst sheet or matrix are assembled into a synthetic raw material.
[0039] In addition, a preferred solution is that the raw carbon source includes diamond micropowder and carbon powder with a purity of not less than 90%, and the catalyst is FeCo alloy powder; wherein, the diamond micropowder and the carbon powder are mixed and formulated into a prefabricated standard carbon source, and then mixed with the FeCo alloy powder to form a mixed sample; wherein, the ratio of carbon powder:diamond micropowder ranges from 300:1 to 1:1.
[0040] In addition, a preferred solution is that the prefabricated assembly elements include thermal insulation sheets, heating sheets, heating plugs and pyrophyllite cubes.
[0041] In addition, a preferred solution is to perform high temperature and high pressure treatment using a pre-set synthesis pressure program, including:
[0042] Pressurizing to 5-8 GPa at a pressurizing rate of 0.1-2 GPa / min, then heating to 1200-2000°C at a heating rate of 200-1000 K / min; maintaining the temperature at 1200-2000°C for a predetermined time to grow diamond; and,
[0043] After the heat preservation and pressure maintenance growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 20-400K / min and in a segmented multi-stage pressure relief manner.
[0044] The preset time is 10 to 300 minutes.
[0045] In addition, a preferred solution is to crush and peel off the polycrystalline diamond sheet sample, clean it in a static high-temperature water bath, air-dry it to remove moisture, and then grind and polish it.
[0046] In addition, a preferred solution is that the average particle size of the prepared high thermal conductivity polycrystalline diamond sheet is ≥40 μm, and the thermal conductivity is ≥600 W / K·m.
[0047] The present invention provides a method for producing high-thermal-conductivity polycrystalline diamond (PCD) under high temperature and high pressure. Using various carbon sources as raw materials, the method uses a catalyst to directly convert the carbon sources into PCD under high temperature and high pressure conditions. Compared with traditional PCD production methods, this method significantly reduces raw material costs and enables the rapid and inexpensive production of ultra-high-thermal-conductivity PCD materials.
[0048] To achieve the above and related ends, one or more aspects of the present invention include features that will be described in detail below and particularly pointed out in the claims. The following description and the accompanying drawings set forth certain exemplary aspects of the present invention in detail. However, these aspects are merely indicative of the various ways in which the principles of the present invention may be employed. Furthermore, the present invention is intended to include all such aspects and their equivalents. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] By referring to the following description and claims in conjunction with the accompanying drawings, and with a more complete understanding of the present invention, other objects and results of the present invention will become more apparent and readily understood. In the accompanying drawings:
[0050] Figure 1 Schematic diagram comparing a conventional method for preparing polycrystalline diamond with a method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to an embodiment of the present invention;
[0051] Figure 2 This is a schematic flow chart of a method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to one embodiment of the present invention;
[0052] Figure 3 Schematic diagram of the synthesis process of high thermal conductivity polycrystalline diamond according to an embodiment of the present invention;
[0053] Figure 4 This is a schematic flow chart of a method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to another embodiment of the present invention;
[0054] Figure 5 A schematic diagram of the surrounding morphology of high thermal conductivity polycrystalline diamond prepared according to an embodiment of the present invention;
[0055] Figure 6 Schematic diagram of a high thermal conductivity polycrystalline diamond thermal conductive sheet prepared according to different synthesis conditions of an embodiment of the present invention.
[0056] In the attached drawings, it includes: pyrophyllite 1, dolomite 2, graphite box 3, magnesium oxide 4, salt pipe 5, conductive steel bowl 6, molybdenum sheet 7, carbon sheet 8, and prefabricated synthetic raw material 9.
[0057] The same reference numerals throughout the drawings indicate similar or corresponding features or functions. DETAILED DESCRIPTION
[0058] In the following description, for illustrative purposes, numerous specific details are set forth to provide a comprehensive understanding of one or more embodiments. However, it will be apparent that the embodiments may be practiced without these specific details. In other instances, well-known structures and devices are shown in block diagram form to facilitate description of one or more embodiments.
[0059] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer" and the like indicating directions or positional relationships are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the devices or components referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as limiting the present invention; the terms "first", "second", and "third" are only used for descriptive purposes and should not be understood as indicating or implying relative importance; in addition, unless otherwise expressly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, an indirect connection through an intermediate medium, or it can be internal communication between two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0060] In order to overcome the problems of small grain size and low neck density in traditional HPHT synthetic polycrystalline diamond compacts, the present invention provides a new HPHT method for preparing high thermal conductivity polycrystalline diamond.
[0061] Figure 1 a is a schematic diagram of the traditional polycrystalline diamond preparation method. Figure 1 b is a schematic diagram of a method for preparing high thermal conductivity polycrystalline diamond according to an embodiment of the present invention. Figure 1 a and Figure 1 As shown in Figure 2, conventional polycrystalline diamond production methods involve forming a neck of diamond powder under high temperature and high pressure conditions using a catalyst to produce polycrystalline diamond. The present invention, however, uses various carbon sources as raw materials and, under high temperature and high pressure conditions, uses a catalyst to directly convert the carbon sources into polycrystalline diamond.
[0062] Figure 2 This is a flow chart of a method for preparing high thermal conductivity polycrystalline diamond at high temperature and high pressure according to an embodiment of the present invention. Figure 2 As shown, the method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure provided in this embodiment includes the following steps:
[0063] S110: Raw material block preparation step. This includes: preparing a raw carbon source and a catalyst, and pressurizing the resulting mixture through a mold to prepare a prefabricated synthetic raw material; and then assembling the prefabricated synthetic raw material and prefabricated assembly components together to form an integral synthetic block;
[0064] S120: High temperature and high pressure growth step. This includes placing the entire synthetic block prepared in the raw material block preparation step into a quasi-static high pressure device and performing high temperature and high pressure treatment at a pre-set synthesis pressure program to achieve diamond growth;
[0065] S130: Sample post-processing step. This includes: crushing the entire synthetic block after high temperature and high pressure treatment to peel off the polycrystalline diamond sheet sample;
[0066] S140: Catalyst removal step, which includes: removing the catalyst on the peeled polycrystalline diamond sheet sample to obtain a polycrystalline diamond sheet with high thermal conductivity.
[0067] In this embodiment, the raw carbon source can include, but is not limited to, carbon, graphite, diamond particles, or graphene and activated carbon, petroleum coke and pitch coke, plant charcoal, and the like. Any one of these materials, or any combination thereof, can be used to form a mixed sample with the catalyst ingredients. The raw carbon source should have a purity of no less than 80%. Furthermore, the ratio of the carbon, graphite, and other base materials to the diamond powder in the raw carbon source is in the range of 300:1 to 1:1, and the ratio of the graphite, other base materials to the diamond mixed carbon source: catalyst is in the range of 20:1 to 1:1.
[0068] In one embodiment of the present invention, the raw carbon source and catalyst are mixed in a powdered form. This allows the raw carbon source and catalyst to mix and fully contact each other, allowing for a full reaction during the HPHT process. This results in multiple diamond nucleation points, growth, and interconnection, thereby producing large-particle polycrystalline diamond. Compared to traditional preparation methods, the high-temperature, high-pressure method for preparing high-thermal-conductivity polycrystalline diamond provided in this embodiment not only offers a low-cost raw carbon source, significantly reducing raw material costs, but also significantly increases inter-particle bonding density and diamond growth rate by subjecting the mixed powders to HPHT treatment.
[0069] In the specific implementation of the present invention, the catalyst may be a transition metal, other metal, or carbonate, including but not limited to the above catalysts, or a combination of one or more thereof; for example, any combination of at least two of iron, nickel, cobalt, and their alloys. The catalyst may be in the form of a sheet, block, or powdered solid, and may also be derived from a composite material, such as the Co in WC(Co) cemented carbide.
[0070] like Figure 1As shown in Figure b, the method for preparing high-thermal-conductivity polycrystalline diamond under high temperature and high pressure, as provided in the present invention, involves encapsulating a raw carbon source and catalyst together. These are then placed into a pyrophyllite cube along with other assembly components, including a thermal insulation sheet, a heater sheet, and a heating plug, to form a monolithic composite block. The raw carbon source and catalyst are first pressurized and formed into a prefabricated composite material having a sheet structure no less than 1 mm thick, which is then encapsulated along with the assembly components.
[0071] Figure 3 Schematic diagram of the structure of the assembled integrated block according to an embodiment of the present invention. Figure 3 As shown, the prefabricated synthetic raw material after pressurization is placed Figure 3 In area 9 (the location of the carbon source and catalyst), a salt tube 5, a magnesium oxide cup 6, a graphite box 3, dolomite 2, talc 1, a carbon sheet 8, a molybdenum sheet 7 and a conductive steel bowl 6 are assembled in sequence on the outside thereof. Accordingly, the structure of the overall synthetic block formed by the combination includes a heat-insulating layer, a heat-conducting layer, an insulating layer, and salt used to balance the pressure.
[0072] In this embodiment, the static high-pressure equipment can be a six-sided top press (e.g., a hinged six-sided top press or a drawbar six-sided constant press). HPHT (5-8 GPa, 1200-2000°C) treatment is performed in the static high-pressure equipment. Under the action of the catalyst and HPHT, the carbon source undergoes multi-point diamond nucleation, growth, and interconnection, transforming into continuous polycrystalline diamond.
[0073] After HPHT treatment, the whole synthetic block needs to be broken to peel off Figure 3 The polycrystalline diamond thermal conductive sheet sample is formed in area 9 in the figure. At this time, since the polycrystalline diamond thermal conductive sheet sample has a catalyst, it is necessary to remove the catalyst on the polycrystalline diamond sheet sample to finally obtain the desired high thermal conductivity polycrystalline diamond sheet.
[0074] Specifically, as an example, the step of removing the catalyst on the polycrystalline diamond sheet sample includes:
[0075] S141: placing the polycrystalline diamond sheet sample in an acid solution and heating it to remove the catalyst;
[0076] S142: using deionized water ultrasonic cleaning to remove residual acid on the surface of the polycrystalline diamond sheet sample;
[0077] S143: Drying to remove moisture from the surface of the polycrystalline diamond sheet sample.
[0078] Experiments have shown that the method of preparing high-thermal conductivity polycrystalline diamond using high temperature and high pressure of the present invention can produce diamond at a growth rate of up to 10 mm / h. The prepared polycrystalline diamond material has an average particle size of ≥40 μm, a high inter-particle bonding density, and a high thermal conductivity of ≥600 W / K·m.
[0079] To further illustrate the preparation process of high thermal conductivity polycrystalline diamond based on the above method, the method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure provided by the present invention is described below in the form of an implementation case.
[0080] Implementation Case 1
[0081] In this embodiment 1, the raw carbon source in the mixed sample is graphite (purity>90%), and the catalyst is iron powder (purity>90%) and cobalt powder (purity>90%).
[0082] The specific preparation steps are as follows:
[0083] (1) Preparation of raw material blocks: The required mixed sample is mixed and formulated according to the ratio of graphite: iron powder: cobalt powder = 10:1:1, and then the mixed sample is pressurized and formed in a mold to prepare a prefabricated synthetic raw material, so that the thickness of the prefabricated synthetic raw material is about 5 mm.
[0084] Figure 2 Schematic diagram of the synthesis process of high thermal conductivity polycrystalline diamond according to an embodiment of the present invention.
[0085] like Figure 2 As shown, the prepared prefabricated synthetic raw material is placed Figure 2 The prefabricated synthetic raw material 9 is located in the position. Subsequently, the salt tube 5, magnesium oxide cup 4, graphite box 3, dolomite 2, pyrophyllite 1, carbon sheet 8, molybdenum sheet 7, and conductive steel bowl 6 are assembled in sequence on the outside of the prefabricated synthetic raw material 9 to form the overall synthetic block required for the subsequent high temperature and high pressure growth process.
[0086] In this embodiment, the structure of the integral synthetic block includes a heat-insulating layer, a heat-conducting layer, an insulating layer, and salt for balancing pressure.
[0087] (2) High temperature and high pressure growth: The assembled assembly blocks are placed in a quasi-static high pressure device (such as a hinged six-sided top press) and subjected to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth.
[0088] Specifically, as an example, the synthetic pressure program includes:
[0089] (2.1) Pressurize to 5-8 GPa at a rate of 0.1-2 GPa / min;
[0090] (2.2) The temperature is then raised to 1573.15 K at a heating rate of 200 to 1000 K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0091] In this embodiment, the time for growing diamond under the conditions of maintaining temperature and pressure is 10 to 100 minutes.
[0092] (2.3) After the heat preservation and pressure growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 240-3500K / min and a multi-stage pressure relief method, and then the integral synthetic block is removed from the six-sided top press.
[0093] It should be noted that the above cooling rate can be selected according to specific needs, and a cooling rate of 20-4000K / min is acceptable.
[0094] (3) Sample post-processing: The whole synthetic block taken out from the six-sided top press is crushed to peel off the Figure 3 The polycrystalline diamond sheet sample at area 9 in the middle is removed. The peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture, thereby obtaining a polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then ground flat on a conventional grinder and polished.
[0095] (4) Acid leaching to remove catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. The residual acid is further ultrasonically cleaned with deionized water and dried to remove surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed. The macroscopic morphology of the high thermal conductivity polycrystalline diamond sheet is as follows: Figure 3 Shown on the right side.
[0096] Implementation Case 2
[0097] In this embodiment 2, the raw carbon source in the mixed sample is graphite (purity of 90%), and the catalyst is iron powder (purity>95%) and cobalt powder (purity>95%).
[0098] The specific preparation steps are as follows:
[0099] (1) Preparation of raw material blocks: The required mixed sample is mixed and formulated according to the ratio of graphite: iron powder: cobalt powder = 40:1:1, and then the mixed sample is pressurized and formed in a mold to prepare a prefabricated synthetic raw material, so that the thickness of the prefabricated synthetic raw material is less than 8 mm and not less than 1 mm.
[0100] (2) High temperature and high pressure growth: The assembled assembly blocks are placed in a quasi-static high pressure device (such as a hinged six-sided top press) and subjected to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth.
[0101] Specifically, as an example, the synthetic pressure program includes:
[0102] (2.1) Pressurize to 6±2 GPa at a rate of 1±0.3 GPa / min;
[0103] (2.2) The temperature is then raised to 1500±200°C at a heating rate of 300±50K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0104] In this embodiment, the time for growing diamond under the condition of maintaining temperature and pressure is 50±10 minutes.
[0105] (2.3) After the heat preservation and pressure growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 300±10K / min and a segmented multi-stage pressure relief method, and then the integral synthetic block is taken out from the six-sided top press.
[0106] (3) Sample post-processing: The whole synthetic block taken out from the six-sided top press is crushed to peel off the Figure 3 The polycrystalline diamond sheet sample at area 9 in the middle is removed. The peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture, thereby obtaining a polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then ground flat on a conventional grinder and polished.
[0107] (4) Acid leaching to remove the catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. It is further ultrasonically cleaned with deionized water to remove the residual acid solution and dried to remove the surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed.
[0108] Implementation Case 3
[0109] In this embodiment 2, the raw carbon source in the mixed sample is graphite (purity of 80%), and the catalyst is iron powder (purity>99.9%) and cobalt powder (purity>99.9%).
[0110] The specific preparation steps are as follows:
[0111] (1) Preparation of raw material blocks: The required mixed sample is mixed and formulated according to the ratio of graphite: iron powder: cobalt powder = 2:1:1, and then the mixed sample is pressurized and formed in a mold to prepare a prefabricated synthetic raw material, so that the thickness of the prefabricated synthetic raw material is 6±1 mm.
[0112] (2) High temperature and high pressure growth: The assembled assembly blocks are placed in a quasi-static high pressure device and subjected to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth.
[0113] Specifically, as an example, the synthetic pressure program includes:
[0114] (2.1) Pressurize to 5-8 GPa at a rate of 0.1-2 GPa / min;
[0115] (2.2) The temperature is then raised to 1200-2000°C at a heating rate of 200-2000 K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0116] In this embodiment, the time for growing diamond under the condition of maintaining temperature and pressure is 10 to 150 minutes.
[0117] (2.3) After the heat preservation and pressure growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 300±10K / min and a segmented multi-stage pressure relief method, and then the integral synthetic block is taken out from the six-sided top press.
[0118] (3) Sample post-processing: The whole synthetic block removed from the six-sided top press is crushed to peel off the polycrystalline diamond sheet sample; the peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture to obtain a polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then placed on a popular grinder and ground flat, and then polished.
[0119] (4) Acid leaching to remove the catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. It is further ultrasonically cleaned with deionized water to remove the residual acid solution and dried to remove the surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed.
[0120] Implementation Case 4
[0121] In this embodiment, the raw carbon sources in the mixed sample are graphite (purity > 90%) and diamond powder, and the catalysts are iron powder (purity > 95%) and cobalt powder (purity > 95%). The graphite and diamond powder serve as the carbon source and diamond nuclei, respectively, while the iron powder and cobalt powder serve as the catalyst.
[0122] The specific preparation steps are as follows:
[0123] (1) Preparation of raw material block: The required mixed sample is mixed according to the ratio of graphite: diamond powder: iron powder: cobalt powder = 10:2:1:1, and then the mixed sample is pressed into a sheet structure with a thickness of 5±2mm in a mold and placed Figure 2 9 locations in the center. Subsequently, a salt tube 5, magnesium oxide cup 4, graphite box 3, dolomite 2, pyrophyllite 1, carbon sheet 8, molybdenum sheet 7, and conductive steel bowl 6 are sequentially assembled on the outside to form the monolithic composite block required for subsequent high-temperature and high-pressure growth processing. The monolithic composite block structure includes a thermal insulation layer, a heat-conducting layer, an insulating layer, and salt for pressure balance.
[0124] (2) High temperature and high pressure growth: The assembled whole synthetic block is placed in a quasi-static high pressure device (hinged six-sided top press) and treated with high temperature and high pressure according to a pre-set synthetic pressure program to achieve diamond growth.
[0125] Specifically, as an example, the synthetic pressure program includes:
[0126] (2.1) Pressurize to 6 GPa at a rate of 1.5 GPa / min;
[0127] (2.2) The temperature is then raised to 1800°C at a heating rate of 600±50K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0128] In this embodiment, the time for growing diamond under the condition of maintaining temperature and pressure is 40 to 60 minutes.
[0129] (2.3) After the heat preservation and pressure growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 3000±20K / min and a multi-stage pressure relief method, and then the integral synthetic block is taken out from the six-sided top press.
[0130] (3) Sample post-processing: The whole synthetic block taken out from the six-sided top press is crushed to peel off the Figure 3 The polycrystalline diamond sheet sample at area 9 in the middle is removed. The peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture, thereby obtaining a polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then ground flat on a conventional grinder and polished.
[0131] (4) Acid leaching to remove catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. The residual acid is further ultrasonically cleaned with deionized water and dried to remove surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed. The macroscopic morphology of the high thermal conductivity polycrystalline diamond sheet is as follows: Figure 3 Shown on the right side.
[0132] Implementation Case 5
[0133] In this embodiment, the raw carbon sources in the mixed sample include carbon (purity > 99.9%), graphite (purity > 99.9%), and diamond powder, and the catalysts include iron powder (purity > 99.9%) and cobalt powder (purity > 99.9%). The carbon, graphite, and diamond powder serve as the carbon source and diamond nuclei, respectively, while the iron powder and cobalt powder serve as the catalyst.
[0134] The specific preparation steps are as follows:
[0135] (1) Preparation of raw material block: The required mixed sample is mixed according to the ratio of carbon: graphite: diamond powder: iron powder: cobalt powder = 10:10:2:1:1, and then the mixed sample is pressed into a sheet structure with a thickness of 5±2mm in a mold and placed Figure 29. Then, a salt tube 5, a magnesium oxide cup 4, a graphite box 3, dolomite 2, a pyrophyllite 1, a carbon sheet 8, a molybdenum sheet 7, and a conductive steel bowl 6 are sequentially assembled on the outside of the salt tube to form the overall synthetic block required for the subsequent high-temperature and high-pressure growth process.
[0136] (2) High temperature and high pressure growth: The assembled whole synthetic block is placed in a quasi-static high pressure device (hinged six-sided top press) and treated with high temperature and high pressure according to a pre-set synthetic pressure program to achieve diamond growth.
[0137] Specifically, as an example, the synthetic pressure program includes:
[0138] (2.1) Pressurize to 7 GPa at a rate of 1.8 GPa / min;
[0139] (2.2) The temperature is then raised to 1600°C at a heating rate of 800±100 K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0140] In this embodiment, the time for growing diamond under the condition of maintaining temperature and pressure is 50 to 90 minutes.
[0141] (2.3) After the growth under heat and pressure is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 350 K / min and in a segmented multi-stage pressure relief manner, and then the integral synthetic block is taken out from the six-sided top press.
[0142] (3) Sample post-processing: The whole synthetic block taken out from the six-sided top press is crushed to peel off the Figure 3 The polycrystalline diamond sheet sample at area 9 in the middle is removed. The peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture, thereby obtaining a polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then ground flat on a conventional grinder and polished.
[0143] (4) Acid leaching to remove the catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. It is further ultrasonically cleaned with deionized water to remove the residual acid solution and dried to remove the surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed.
[0144] Implementation Case 6
[0145] In this embodiment, the raw carbon sources in the mixed sample are graphite (purity > 80%) and diamond powder, and the catalysts are nickel powder (purity > 99.9%) and cobalt powder (purity > 99.9%). The graphite and diamond powder serve as the carbon source and diamond nuclei, respectively, while the nickel powder and cobalt powder serve as the catalyst.
[0146] The specific preparation steps are as follows:
[0147] (1) Preparation of raw material block: The required mixed sample is mixed and prepared according to the ratio of graphite: diamond powder: nickel powder: cobalt powder = 2000:10:10:5, and then the mixed sample is pressurized in a mold to form a sheet structure with a thickness of 5±2 mm. Subsequently, a salt tube 5, a magnesium oxide cup 4, a graphite box 3, dolomite 2, pyrophyllite 1, a carbon sheet 8, a molybdenum sheet 7, and a conductive steel bowl 6 are assembled in sequence on the outside of the sheet structure to form an integral synthetic block required for the subsequent high temperature and high pressure growth treatment.
[0148] (2) High temperature and high pressure growth: The assembled whole synthetic block is placed in a quasi-static high pressure device (hinged six-sided top press) and treated with high temperature and high pressure according to a pre-set synthetic pressure program to achieve diamond growth.
[0149] Specifically, as an example, the synthetic pressure program includes:
[0150] (2.1) Pressurize to 7 GPa at a rate of 1.8 GPa / min;
[0151] (2.2) The temperature is then raised to 1600°C at a heating rate of 800±100 K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0152] In this embodiment, the time for growing diamond under the condition of maintaining temperature and pressure is 50 to 90 minutes.
[0153] (2.3) After the heat preservation and pressure growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 1000K / min and a multi-stage pressure relief method, and then the integral synthetic block is taken out from the six-sided top press.
[0154] (3) Sample post-processing: The whole synthetic block removed from the six-sided top press is crushed to peel off the polycrystalline diamond sheet sample; the peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture to obtain the polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then placed on a popular grinder and ground flat, and then polished.
[0155] (4) Acid leaching to remove the catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. It is further ultrasonically cleaned with deionized water to remove the residual acid solution and dried to remove the surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed.
[0156] Implementation Case 7
[0157] In this embodiment, the raw carbon sources in the mixed sample are graphite (purity > 85%) and diamond powder, and the catalysts are nickel powder (purity > 95%), iron powder (purity > 95%), and cobalt powder (purity > 95%). The graphite and diamond powder serve as the carbon source and diamond nuclei, respectively, while the nickel powder, iron powder, and cobalt powder serve as catalysts.
[0158] The specific preparation steps are as follows:
[0159] (1) Preparation of raw material blocks: The required mixed sample is mixed and formulated according to the ratio of graphite: diamond powder: nickel powder: iron powder: cobalt powder = 2:1:1:1:1, and then the mixed sample is pressurized in a mold to form a sheet structure with a thickness of 6±2 mm. Subsequently, a salt tube 5, a magnesium oxide cup 4, a graphite box 3, dolomite 2, pyrophyllite 1, a carbon sheet 8, a molybdenum sheet 7, and a conductive steel bowl 6 are assembled in sequence on the outside of the sheet structure to form an integral synthetic block required for the subsequent high-temperature and high-pressure growth treatment.
[0160] (2) High temperature and high pressure growth: The assembled whole synthetic block is placed in a quasi-static high pressure device and treated with high temperature and high pressure according to a pre-set synthetic pressure program to achieve diamond growth.
[0161] The specific synthesis pressure procedure can be found in the description of the aforementioned embodiment.
[0162] (3) Sample post-processing: The whole synthetic block removed from the six-sided top press is crushed to peel off the polycrystalline diamond sheet sample; the peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture to obtain the polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then placed on a popular grinder and ground flat, and then polished.
[0163] (4) Acid leaching to remove the catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. It is further ultrasonically cleaned with deionized water to remove the residual acid solution and dried to remove the surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed.
[0164] The present invention also provides another method for preparing high thermal conductivity polycrystalline diamond at high temperature and high pressure, such as Figure 4 As shown, the method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure includes the following steps:
[0165] S410: Raw material block preparation step. This includes: mixing the raw carbon source powder into a mixed sample, and press-molding the mixed sample into a standard carbon source through a mold; then using the standard carbon source and a catalyst as a prefabricated raw material, and assembling the prefabricated raw material with assembly components to form an integrated synthetic block;
[0166] S420: High temperature and high pressure growth step. This includes placing the entire synthetic block prepared in the raw material block preparation step into a quasi-static high pressure device and performing high temperature and high pressure treatment at a pre-set synthesis pressure program to achieve diamond growth;
[0167] S430: Sample post-processing step, which includes: crushing the entire synthetic block after high temperature and high pressure treatment to peel off the polycrystalline diamond sheet sample;
[0168] S440: Acid leaching to remove the catalyst step, which includes: removing the catalyst on the peeled polycrystalline diamond sheet sample to obtain a polycrystalline diamond sheet with high thermal conductivity.
[0169] In this embodiment, the raw carbon source can include carbon with a purity of no less than 80%, graphite, diamond particles or graphene, activated carbon, petroleum coke, pitch coke, plant charcoal, and the like, including but not limited to the aforementioned materials. Any one of these materials or any combination of these materials can be used to form a mixed sample. The resulting mixed sample is pressurized and formed into a standard carbon source using a mold, which is then combined with a catalyst as a prefabricated raw material. Due to the large number of pores in the prepared standard carbon source, the catalyst melts into a liquid under the HPHT environment and enters the pores of the standard carbon source, allowing for sufficient contact and reaction between the raw carbon source and the catalyst, resulting in multiple diamond nucleation points, growth, and interconnection, thereby producing large-particle polycrystalline diamond ingredients. Compared to traditional preparation methods, the high-temperature and high-pressure method for preparing high-thermal-conductivity polycrystalline diamond using this embodiment not only offers a low-cost raw carbon source, significantly reducing raw material costs, but also significantly increases the inter-particle bonding density and diamond growth rate by subjecting the powders to HPHT treatment after mixing.
[0170] The catalyst in this embodiment can be a transition metal catalyst sheet, other metals or carbonates or cemented carbide matrix, including but not limited to the above catalysts, or one or a combination thereof; the catalyst can be a powder, sheet or block solid, or it can be derived from a certain composite material, for example, Co in WC (Co) cemented carbide.
[0171] To further illustrate the preparation process of high thermal conductivity polycrystalline diamond based on the above method, the method for preparing high thermal conductivity polycrystalline diamond at high temperature and high pressure provided by the present invention is described below in the form of two specific implementation cases.
[0172] Implementation Case 8
[0173] In this embodiment, the raw carbon source in the mixed sample is carbon or graphite (purity>90%), and the catalyst uses a WC (Co) alloy matrix.
[0174] The specific preparation steps are as follows:
[0175] (1) Raw material block preparation: Use carbon with a purity greater than 90% as the raw carbon source, press it into a 5±2 mm thick specification carbon source through a mold, and place it together with the cemented carbide substrate as a catalyst as a prefabricated synthetic raw material. Figure 3 The salt tube 5, magnesium oxide cup 4, graphite box 3, dolomite 2, pyrophyllite 1, carbon sheet 8, molybdenum sheet 7, and conductive steel bowl 6 are then assembled on the outside of the tube to form the monolithic composite block required for subsequent high-temperature and high-pressure growth. The monolithic composite block structure includes a thermal insulation layer, a heat-conducting layer, an insulating layer, and salt for pressure balance.
[0176] (2) High temperature and high pressure growth: The assembled assembly blocks are placed in a quasi-static high pressure device (hinged six-sided top press) and subjected to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth.
[0177] Specifically, as an example, the synthetic pressure program includes:
[0178] (2.1) Pressurize to 7±1 GPa at a rate of 0.8±0.2 GPa / h;
[0179] (2.2) The temperature is then raised to 1573.15 K at a heating rate of 500 ± 100 K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0180] In this embodiment, the time for growing diamond under the condition of maintaining temperature and pressure is 40 to 60 minutes.
[0181] (2.3) After the heat preservation and pressure growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 300±50K / min and a multi-stage pressure relief method, and then the integral synthetic block is taken out from the six-sided top press.
[0182] (3) Sample post-processing: The whole synthetic block taken out from the six-sided top press is crushed to peel off the Figure 3 The polycrystalline diamond sheet sample at area 9 in the middle is removed. The peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture, thereby obtaining a polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then ground flat on a conventional grinder and polished.
[0183] (4) Acid leaching to remove catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. The residual acid is further ultrasonically cleaned with deionized water and dried to remove surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed. The macroscopic morphology of the high thermal conductivity polycrystalline diamond sheet is as follows: Figure 3 Shown on the right side.
[0184] Implementation Case 9
[0185] In this embodiment, the raw carbon source in the mixed sample is graphite (purity>95%), and the catalyst is a transition metal catalyst sheet.
[0186] The specific preparation steps are as follows:
[0187] (1) Preparation of raw material block: Isostatic graphite with a density of 1.7 g / cm3 is used as the raw carbon source, and is pressed and formed into a 5 mm thick carbon source through a mold. It is placed together with a transition metal catalyst sheet as a prefabricated synthetic raw material. Figure 3 The salt tube 5, magnesium oxide cup 4, graphite box 3, dolomite 2, pyrophyllite 1, carbon sheet 8, molybdenum sheet 7, and conductive steel bowl 6 are then assembled on the outside of the tube to form the monolithic composite block required for subsequent high-temperature and high-pressure growth. The monolithic composite block structure includes a thermal insulation layer, a heat-conducting layer, an insulating layer, and salt for pressure balance.
[0188] (2) High temperature and high pressure growth: The assembled assembly blocks are placed in a quasi-static high pressure device (hinged six-sided top press) and subjected to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth.
[0189] Specifically, as an example, the synthetic pressure program includes:
[0190] (2.1) Pressurize to 6 GPa at a rate of 1.6 GPa / min;
[0191] (2.2) The temperature is then raised to 1573.15 K at a heating rate of 1600 K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0192] In this embodiment, the time for growing diamond under the condition of maintaining temperature and pressure is 50±10 minutes.
[0193] (2.3) After the heat preservation and pressure maintenance growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 300 K / min and a multi-stage pressure relief method, and then the integral synthetic block is taken out from the six-sided top press.
[0194] (3) Sample post-processing: The whole synthetic block taken out from the six-sided top press is crushed to peel off the Figure 3 The polycrystalline diamond sheet sample at area 9 in the middle is removed. The peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture, thereby obtaining a polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then ground flat on a conventional grinder and polished.
[0195] (4) Acid leaching to remove the catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. It is further ultrasonically cleaned with deionized water to remove the residual acid solution and dried to remove the surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed.
[0196] Implementation Case 10
[0197] In this embodiment, the raw carbon source in the mixed sample is a mixture of carbon (purity>80%) and graphite (purity>80%), and the catalyst is a transition metal catalyst sheet.
[0198] The specific preparation steps are as follows:
[0199] (1) Preparation of raw material block: A mixture of carbon (purity>80%) and graphite (purity>80%) is used as the raw carbon source, which is pressurized and formed into a 5mm thick carbon source through a mold, and is placed together with a transition metal catalyst sheet as a prefabricated synthetic raw material. Figure 3 Then, a salt tube 5, a magnesium oxide cup 4, a graphite box 3, dolomite 2, pyrophyllite 1, a carbon sheet 8, a molybdenum sheet 7, and a conductive steel bowl 6 are sequentially assembled on the outside of the salt tube to form the overall synthetic block required for the subsequent high-temperature and high-pressure growth process.
[0200] (2) High temperature and high pressure growth: The assembled assembly blocks are placed in a quasi-static high pressure device (hinged six-sided top press) and subjected to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth.
[0201] Specifically, as an example, the synthetic pressure program includes:
[0202] (2.1) Pressurize to 8 GPa at a rate of 2 GPa / min;
[0203] (2.2) The temperature is then raised to 1800±100°C at a heating rate of 1800 K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0204] In this embodiment, the time for growing diamond under the condition of maintaining temperature and pressure is 60±10 minutes.
[0205] (2.3) After the heat preservation and pressure maintenance growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 300 K / min and a multi-stage pressure relief method, and then the integral synthetic block is taken out from the six-sided top press.
[0206] (3) Sample post-processing: The whole synthetic block removed from the six-sided top press is crushed to peel off the polycrystalline diamond sheet sample; the peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture to obtain the polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then placed on a popular grinder and ground flat, and then polished.
[0207] (4) Acid leaching to remove the catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. It is further ultrasonically cleaned with deionized water to remove the residual acid solution and dried to remove the surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed.
[0208] Implementation Case 11
[0209] In this embodiment, the raw carbon sources in the mixed sample are carbon powder (purity>90%) and diamond powder, and the catalyst is FeCo alloy powder.
[0210] The specific preparation steps are as follows:
[0211] (1) Preparation of raw material block: The raw material carbon source in the required mixed sample is mixed according to the ratio of carbon powder: diamond powder = 10:1, and is pressurized into a 5 mm thick standard carbon source through a mold. FeCo alloy powder is used as a catalyst and placed together with the standard carbon source. Figure 3 9. Then, a salt tube 5, a magnesium oxide cup 4, a graphite box 3, dolomite 2, a pyrophyllite 1, a carbon sheet 8, a molybdenum sheet 7, and a conductive steel bowl 6 are sequentially assembled on the outside of the salt tube to form the overall synthetic block required for the subsequent high-temperature and high-pressure growth process.
[0212] In other specific embodiments of the present invention, the ratio of carbon powder to diamond powder can be flexibly selected between 300:1 and 1:1 according to specific needs.
[0213] (2) High temperature and high pressure growth: The assembled assembly blocks are placed in a quasi-static high pressure device (hinged six-sided top press) and subjected to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth.
[0214] Specifically, as an example, the synthetic pressure program includes:
[0215] (2.1) Pressurize to 6 GPa at a rate of 1.0 GPa / min;
[0216] (2.2) The temperature is then raised to 1600 K at a heating rate of 600 K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0217] In this embodiment, the time for growing diamond under the conditions of maintaining temperature and pressure is 200±20 minutes.
[0218] (2.3) After the heat preservation and pressure growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 80±20K / min and a multi-stage pressure relief method, and then the integral synthetic block is taken out from the six-sided top press.
[0219] It should be noted that the above cooling rate can be selected according to specific needs, and a cooling rate of 20-4000K / min is possible.
[0220] (3) Sample post-processing: The whole synthetic block removed from the six-sided top press is crushed to peel off the polycrystalline diamond sheet sample; the peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture to obtain the polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then placed on a popular grinder and ground flat, and then polished.
[0221] (4) Acid leaching to remove the catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. It is further ultrasonically cleaned with deionized water to remove the residual acid solution and dried to remove the surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed.
[0222] Implementation Case 12
[0223] In this embodiment, the raw carbon sources in the mixed sample are carbon powder (purity>95%) and diamond powder, and the catalyst is FeCo alloy sheet.
[0224] The specific preparation steps are as follows:
[0225] (1) Preparation of raw material block: The raw material carbon source in the required mixed sample is mixed according to the ratio of carbon powder: diamond powder = 9:2, and is pressurized into a standard carbon source with a thickness of 8 mm by a mold. FeCo alloy sheet is used as a catalyst and placed together with the standard carbon source. Figure 3 9. Then, a salt tube 5, a magnesium oxide cup 4, a graphite box 3, dolomite 2, a pyrophyllite 1, a carbon sheet 8, a molybdenum sheet 7, and a conductive steel bowl 6 are sequentially assembled on the outside of the salt tube to form the overall synthetic block required for the subsequent high-temperature and high-pressure growth process.
[0226] (2) High temperature and high pressure growth: The assembled assembly blocks are placed in a quasi-static high pressure device (hinged six-sided top press) and subjected to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth.
[0227] Specifically, as an example, the synthetic pressure program includes:
[0228] (2.1) Pressurize to 8 GPa at a rate of 1.6 GPa / min;
[0229] (2.2) The temperature is then raised to 1500±200°C at a heating rate of 800K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0230] In this embodiment, the time for growing diamond under the condition of maintaining temperature and pressure is 50 to 80 minutes.
[0231] (2.3) After the growth under heat and pressure is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 260±20K / min and a multi-stage pressure relief method, and then the integral synthetic block is removed from the six-sided top press.
[0232] (3) Sample post-processing: The whole synthetic block removed from the six-sided top press is crushed to peel off the polycrystalline diamond sheet sample; the peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture to obtain the polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then placed on a popular grinder and ground flat, and then polished.
[0233] (4) Acid leaching to remove the catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. It is further ultrasonically cleaned with deionized water to remove the residual acid solution and dried to remove the surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed.
[0234] Implementation Case 13
[0235] In this embodiment, the raw carbon sources in the mixed sample include carbon powder (purity>99.9%), graphite powder (purity>99.9%) and diamond powder, and the catalyst includes FeCo alloy sheet.
[0236] The specific preparation steps are as follows:
[0237] (1) Preparation of raw material block: The raw material carbon source in the required mixed sample is mixed according to the ratio of carbon powder: graphite powder: diamond powder = 9:10:2, and is pressurized into a standard carbon source with a thickness of 8 mm by a mold. FeCo alloy sheets are used as catalysts and placed together with the standard carbon source. Figure 3 9. Then, a salt tube 5, a magnesium oxide cup 4, a graphite box 3, dolomite 2, a pyrophyllite 1, a carbon sheet 8, a molybdenum sheet 7, and a conductive steel bowl 6 are sequentially assembled on the outside of the salt tube to form the overall synthetic block required for the subsequent high-temperature and high-pressure growth process.
[0238] (2) High temperature and high pressure growth: The assembled assembly blocks are placed in a quasi-static high pressure device (hinged six-sided top press) and subjected to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth.
[0239] Specifically, as an example, the synthetic pressure program includes:
[0240] (2.1) Pressurize to 7 GPa at a rate of 2 GPa / min;
[0241] (2.2) The temperature is then raised to 1600±200°C at a heating rate of 700 K / min, and the temperature and pressure are maintained at the above pressure and temperature to allow diamond growth.
[0242] In this embodiment, the time for growing diamond under the condition of maintaining temperature and pressure is 70 minutes.
[0243] (2.3) After the growth under heat and pressure is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 240±20K / min and a multi-stage pressure relief method, and then the integral synthetic block is removed from the six-sided top press.
[0244] (3) Sample post-processing: The whole synthetic block removed from the six-sided top press is crushed to peel off the polycrystalline diamond sheet sample; the peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture to obtain the polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then placed on a popular grinder and ground flat, and then polished.
[0245] (4) Acid leaching to remove the catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. It is further ultrasonically cleaned with deionized water to remove the residual acid solution and dried to remove the surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed.
[0246] Implementation Case 14
[0247] In this embodiment, the raw carbon sources in the mixed sample are carbon powder (purity>99.9%) and diamond powder, and the catalyst is FeCo alloy sheet.
[0248] The specific preparation steps are as follows:
[0249] (1) Preparation of raw material block: The raw material carbon source in the required mixed sample is mixed according to the ratio of carbon powder: diamond powder = 200:1, and is pressurized into a standard carbon source with a thickness of 8 mm by a mold. FeCo alloy sheet is used as a catalyst and placed together with the standard carbon source. Figure 3 9. Then, a salt tube 5, a magnesium oxide cup 4, a graphite box 3, dolomite 2, a pyrophyllite 1, a carbon sheet 8, a molybdenum sheet 7, and a conductive steel bowl 6 are sequentially assembled on the outside of the salt tube to form the overall synthetic block required for the subsequent high-temperature and high-pressure growth process.
[0250] (2) High temperature and high pressure growth: The assembled assembly blocks are placed in a quasi-static high pressure device (hinged six-sided top press) and subjected to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth.
[0251] The specific synthesis pressure procedure can be found in the description of the aforementioned embodiment.
[0252] (3) Sample post-processing: The whole synthetic block removed from the six-sided top press is crushed to peel off the polycrystalline diamond sheet sample; the peeled polycrystalline diamond sheet sample is cleaned in a high-temperature water bath and air-dried to remove moisture to obtain the polycrystalline diamond thermal conductive sheet. The obtained polycrystalline diamond thermal conductive sheet is then placed on a popular grinder and ground flat, and then polished.
[0253] (4) Acid leaching to remove the catalyst: The polycrystalline diamond sheet sample after flat grinding and polishing is placed in aqua regia and heated to remove the catalyst. It is further ultrasonically cleaned with deionized water to remove the residual acid solution and dried to remove the surface moisture. The preparation of high thermal conductivity polycrystalline diamond sheet is completed.
[0254] Figure 5 The microscopic morphology of the high thermal conductivity polycrystalline diamond sheet prepared by the method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure of the present invention is shown. Figure 5 As shown in the figure, ① on the left and ② on the right are microscopic morphology images under optical microscope and scanning electron microscope respectively. Figure 5 As can be seen in the figure, the diamond grains grow in an oriented manner, appearing as elongated strips. Each elongated grain has a width ≥40μm and a length ≥100μm, with clear bonds between the grains. In the area marked by the red rectangle, the grains have sintered to form necks, and nearby grains are closely connected. The high thermal conductivity of the polycrystalline diamond thermal conductive sheet produced by the high-temperature and high-pressure method of producing high-thermal conductivity polycrystalline diamond according to the present invention can be attributed to the large size of the grown diamond grains and the good necking formed between the diamond grains.
[0255] To investigate the thermal conductivity of polycrystalline diamond sheets produced using the high-temperature, high-pressure method for producing high-thermal-conductivity polycrystalline diamond (PCD) according to the present invention, the thermal diffusivity of the PCD sheets obtained under different synthesis conditions was measured using a laser flash thermal tester. The thermal diffusivity was calculated as shown in Formula 1. The density of the synthesized PCD sheets was measured using a water displacement density tester. The specific heat capacity of the PCD sheets was measured using a synchronous thermal analyzer. The thermal conductivity of the sheets was calculated using Formula 2.
[0256]
[0257] D×ρ×CC=enter formula 2
[0258] The parameters have the following meanings: Indicates half heating time (ms),
[0259] d represents thickness (mm),
[0260] D represents the thermal diffusivity (mm^2 / s);
[0261] ρ represents density (g·cm-3);
[0262] C represents specific heat capacity (J / (kg·k));
[0263] λ represents thermal conductivity (W / (m·K)).
[0264] Through Examples 1-14, the assembled monolithic composite block was placed in a quasi-static high-pressure equipment at HPHT parameters of 5-8 GPa and 1200-2000°C for approximately 15 to 80 minutes. The temperature and pressure were then reduced, and the synthesized samples were removed. Acid washing was used to remove residual metals and salts from the surface. The resulting polycrystalline diamond sheet samples were then smoothed using a grinding wheel and diamond grinding disc. The thermal conductivity of the polycrystalline diamond thermally conductive sheets produced under different synthesis conditions was measured and calculated using a laser flash thermal tester, as shown in Table 1 below.
[0265] Figure 6 ①-④ in the figure are macroscopic photos of the four prepared polycrystalline diamond thermal conductive sheets in Table 1. Figure 6 As shown in the figure, the macroscopic morphology of the surface of the polycrystalline diamond thermal conductive sheet is shown. Under the irradiation of the same bias light source, the refraction area of the sample to light increases, which shows that the better the diamond growth quality, the higher the thermal conductivity obtained.
[0266]
[0267] Table 1 Thermal conductivity calculation table
[0268] From the above specific embodiments, it can be seen that the method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure provided by the present invention has at least the following advantages:
[0269] 1. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure provided by the present invention uses different forms of carbon sources as raw materials, mixes them with catalyst powder and ingredients, and then performs high temperature and high pressure growth treatment. This can directly convert the carbon source into polycrystalline diamond, and the raw material cost is greatly reduced compared with the traditional method of preparing polycrystalline diamond.
[0270] 2. Using the high-temperature and high-pressure method provided by the present invention to prepare high-thermal-conductivity polycrystalline diamond, the carbon source, under catalytic and HPHT conditions, causes diamonds to nucleate, grow, and then connect with each other at multiple points. The prepared polycrystalline diamond material has a large particle size (average particle size ≥ 40 μm) and can bring about higher thermal conductivity.
[0271] 3. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure provided by the present invention can rapidly generate polycrystalline diamond (growth rate up to 10 mm / h) due to the full fusion of carbon source and catalyst.
[0272] 4. The polycrystalline diamond prepared by the method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure provided by the present invention has a high density of inter-particle bonding and a high thermal conductivity of ≥600W / K·m.
[0273] As above Figures 1 to 6 The method for producing high-thermal-conductivity polycrystalline diamond under high pressure and high temperature according to the present invention is described by way of example. However, those skilled in the art will appreciate that various modifications may be made to the method for producing high-thermal-conductivity polycrystalline diamond under high pressure and high temperature according to the present invention without departing from the scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the contents of the appended claims.
Claims
1. A method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure, characterized in that: The steps include: Preparation of raw material block: raw material carbon source and catalyst are mixed, and the mixed sample obtained by mixing is pressed and molded into a prefabricated synthetic raw material through a mold; and then the prefabricated synthetic raw material and prefabricated assembly components are assembled together to form an integral synthetic block; High temperature and high pressure growth: placing the whole synthesis block into a quasi-static high pressure device and subjecting it to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth; Sample post-processing: crushing the whole synthetic block after the high temperature and high pressure treatment to peel off the polycrystalline diamond sheet sample; Removing the catalyst: removing the catalyst on the polycrystalline diamond sheet sample to obtain a polycrystalline diamond sheet with high thermal conductivity.
2. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure as claimed in claim 1, characterized in that: The raw carbon source includes graphite with a purity of not less than 80%, and the catalyst includes at least one of iron, nickel, cobalt and alloys thereof; the mixing ratio of the mixed sample is: graphite: catalyst in the range of 20:1 to 1:
1.
3. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure as claimed in claim 1, characterized in that: The raw carbon source includes diamond powder and graphite with a purity of not less than 80%, and the catalyst includes at least one of iron, nickel, cobalt and their alloys; the ratio of the mixed sample is: the ratio of graphite: diamond powder ranges from 300:1 to 1:1, and the ratio of graphite and diamond mixed carbon source: catalyst ranges from 20:1 to 1:
1.
4. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to any one of claims 1 to 3, characterized in that: The prefabricated synthetic raw material is a sheet structure with a thickness of not less than 1 mm.
5. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to any one of claims 1 to 3, characterized in that: The prefabricated assembly elements include a heat insulating sheet, a heating sheet, a heating plug and a pyrophyllite cube.
6. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to any one of claims 1 to 3, characterized in that: The high temperature and high pressure treatment according to a preset synthesis pressure program includes: Pressurizing to 5-8 GPa at a pressure increase rate of 0.1-2 GPa / min, and then heating to 1200-2000°C at a heating rate of 200-2000K / min; maintaining the temperature and pressure at 1200-2000°C for a preset time to grow diamond; and, After the heat and pressure maintenance growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 20-4000K / min and in a segmented multi-stage pressure relief manner.
7. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure as claimed in claim 6, characterized in that: The preset time is 10 to 150 minutes.
8. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to any one of claims 1 to 3, characterized in that: The polycrystalline diamond sheet samples peeled off by the crushing process are cleaned in a high-temperature water bath, air-dried to remove moisture, and then ground and polished.
9. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to any one of claims 1 to 3, characterized in that: Removing the catalyst on the polycrystalline diamond sheet sample comprises: placing the polycrystalline diamond sheet sample in an acid solution and heating it to remove the catalyst; Using deionized water to ultrasonically clean and remove residual acid on the surface of the polycrystalline diamond sheet sample; The moisture on the surface of the polycrystalline diamond sheet sample is removed by drying.
10. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to any one of claims 1 to 3, characterized in that: The average particle size of the prepared high thermal conductivity polycrystalline diamond sheet is ≥40μm, and the thermal conductivity is ≥600W / K·m.
11. A method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure, characterized in that: The steps include: Preparation of raw material block: the raw material carbon source is mixed and powdered to form a mixed sample, and the mixed sample is pressed and molded into a standard carbon source through a mold; then the standard carbon source and the catalyst are used as prefabricated synthetic raw materials and assembled together with assembly components to form an integral synthetic block; High temperature and high pressure growth: placing the whole synthesis block into a quasi-static high pressure device and subjecting it to high temperature and high pressure treatment according to a pre-set synthesis pressure program to achieve diamond growth; Sample post-processing: crushing the whole synthetic block after the high temperature and high pressure treatment to peel off the polycrystalline diamond sheet sample; Acid leaching to remove catalyst: removing the catalyst on the polycrystalline diamond sheet sample to obtain a polycrystalline diamond sheet with high thermal conductivity.
12. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure as claimed in claim 11, characterized in that: The raw carbon source is carbon or graphite with a purity of not less than 80%, and the catalyst is a transition metal catalyst sheet or a hard alloy matrix; wherein, The carbon or graphite is assembled with a catalyst sheet or a matrix into a prefabricated synthetic raw material.
13. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure as claimed in claim 11, characterized in that: The raw carbon source includes diamond powder and carbon powder with a purity of not less than 90%, and the catalyst is FeCo alloy powder; wherein, The diamond micropowder and the carbon powder are mixed and formulated into a prefabricated standard carbon source, and then mixed with the FeCo alloy powder to form a mixed sample; wherein the ratio of carbon powder to diamond micropowder is in the range of 300:1 to 1:
1.
14. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to any one of claims 11 to 13, characterized in that: The prefabricated assembly elements include a heat insulating sheet, a heating sheet, a heating plug and a pyrophyllite cube.
15. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to any one of claims 11 to 13, characterized in that: The high temperature and high pressure treatment according to a preset synthesis pressure program includes: Pressurizing to 5-8 GPa at a pressure increase rate of 0.1-2 GPa / min, and then heating to 1200-2000°C at a heating rate of 200-1000 K / min; maintaining the temperature at 1200-2000°C for a preset time to grow diamond; and, After the heat and pressure maintenance growth is completed, the pressure is reduced to normal temperature and pressure at a cooling rate of 20-4000K / min and in a segmented multi-stage pressure relief manner.
16. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure as claimed in claim 15, characterized in that: The preset time is 10 to 300 minutes.
17. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to any one of claims 11 to 13, characterized in that: The polycrystalline diamond sheet samples peeled off by the crushing process are cleaned in a high-temperature water bath, air-dried to remove moisture, and then ground and polished.
18. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to any one of claims 11 to 13, characterized in that: The average particle size of the prepared high thermal conductivity polycrystalline diamond sheet is ≥40μm, and the thermal conductivity is ≥600W / K·m.
19. The method for preparing high thermal conductivity polycrystalline diamond under high temperature and high pressure according to any one of claims 11 to 13, characterized in that: Removing the catalyst on the polycrystalline diamond sheet sample comprises: placing the polycrystalline diamond sheet sample in an acid solution and heating it to remove the catalyst; Using deionized water to ultrasonically clean and remove residual acid on the surface of the polycrystalline diamond sheet sample; The moisture on the surface of the polycrystalline diamond sheet sample is removed by drying.
Citation Information
Patent Citations
Method for explosive synthesizing nano polycrystal diamond and special-purpose explosive device
CN101164682A
Superhard material cutting tool and preparation method thereof
CN101502926A
Polycrystalline diamond-tungsten carbide rigid alloy composite anvil for generating ultrahigh pressure
CN102671578A
Use of nonmetal catalyst in synthetic diamond
CN105013400A
Diamond production process relating to cubic hydraulic press
CN112808169A
Cited By
Diamond surface etching method
CN119954152A
Lightweight nanopore diamond and preparation method thereof
CN120423542A
Diamond ball or diamond composite material ball and preparation method thereof
CN121159253A
Method for preparing high-quality boron-doped polycrystalline diamond at high temperature and high pressure as well as product and application thereof
CN121466921A
A method for preparing high-quality boron-doped polycrystalline diamond at high temperature and high pressure, and products and applications thereof