Magnetic material loaded with tetrathiomolybdate intercalation layered dihydroxide as well as preparation method and application of magnetic material

By loading magnetic materials with tetrathiomolybdate intercalated layered double hydroxide compounds, the problem of reduced reaction rate and recovery in the transition metal ion-activated persulfate method is solved, and efficient degradation of antibiotic pollutants is achieved, and through magnetic separation Recycling catalysts avoids waste of resources and secondary pollution of water bodies.

CN118767947APending Publication Date: 2024-10-15SOUTH CHINA NORMAL UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410768025.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing technology, the method of activating persulfate with transition metal ions has the problem that the high-valent transition metal accumulated after the reaction inhibits the reaction rate and is difficult to recover, resulting in a waste of resources and secondary pollution of water bodies.

Method used

Using magnetic materials loaded with tetrathiomolybdate intercalated layered double hydroxides, copper and iron transition metals are loaded on the surface of ferric tetroxide nanoparticles in the form of heterogeneous catalysts to synergistically catalytically activate potassium peroxodisulfate. salt, and supports tetrathiomolybdate as an electron donor in the form of an interlayer anion to increase the free radical yield and accelerate the degradation of antibiotics.

Benefits of technology

It achieves efficient and rapid degradation of doxycycline hydrochloride and other antibiotic contaminants. The catalyst can be recovered through magnetic separation to avoid loss, and has wide application value and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767947A_ABST
    Figure CN118767947A_ABST
Patent Text Reader

Abstract

The invention relates to a magnetic material loaded with a tetrathiomolybdate intercalation layered dihydroxide. The layered dihydroxide is loaded on the magnetic material; the layered dihydroxide is a tetrathiomolybdate intercalated copper-iron-aluminum layered metal hydroxide, and the magnetic material comprises ferroferric oxide nanoparticles. According to the magnetic material loaded with the tetrathiomolybdate intercalation layered dihydroxide, the problem that a powder catalyst material is difficult to recycle is solved in the mode that two transition metals, namely copper and iron, are loaded on ferroferric oxide nanoparticles in the form of the layered dihydroxide (LDH); tetrathiomolybdate is intercalated into the interlayer of the layered dihydroxide in an anion exchange form, and the tetrathiomolybdate can be used as an electron donor to improve the rate of activating persulfate, so that the removal rate of organic pollutants, such as doxycycline hydrochloride and other antibiotics, is improved, and the removal rate of the organic pollutants, such as doxycycline hydrochloride and other antibiotics, in water is realized. For example, antibiotics such as doxycycline hydrochloride can be completely degraded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sewage treatment, in particular to a magnetic material loaded with layered double hydroxides, a preparation method and an application thereof. Background Art

[0002] The widespread use of antibiotics has brought significant benefits in medicine and animal husbandry, but it has also brought with it the global problem of antibiotic residues in the environment. Due to their complex chemical structure and special physical and chemical properties, these residues are difficult to effectively remove through the conventional processes of traditional sewage treatment plants, resulting in their continuous accumulation in water bodies, posing a severe challenge to ecosystems and human health. Doxycycline hydrochloride (DOX), as a representative of tetracycline antibiotics, plays a key role in the treatment of a variety of bacterial infections due to its broad-spectrum antibacterial effect. Existing research reports have shown that DOX is frequently detected in a variety of water bodies. Therefore, the development of methods that can efficiently remove DOX from water bodies is of great significance for protecting the environment and maintaining human health.

[0003] In the field of sewage treatment, the main methods used for the treatment of antibiotics such as DOX include physical treatment, biological treatment and advanced oxidation processes (AOPs). Although the physical treatment method is simple and fast to operate, it can only achieve mechanical separation of pollutants rather than complete degradation, and there is a risk of causing secondary pollution. Biological treatment methods are favored for their good selectivity and the safety and stability of the treatment process, but are limited by the applicability of wastewater and strict operating conditions. In contrast, advanced oxidation technology, especially persulfate oxidation, is regarded as a promising environmentally friendly pollutant removal technology because it can efficiently decompose and mineralize difficult-to-degrade organic matter without producing harmful secondary pollutants.

[0004] Compared with the Fenton method dominated by hydroxyl radicals, the sulfate radicals produced by the persulfate oxidation method have higher oxidation potential, longer half-life, stronger oxidizing property, and higher selectivity under complex environment. The methods commonly used to activate persulfate include photoactivation, electroactivation, thermal activation, ultrasonic activation, and transition metal ion activation. Among them, transition metal ion activation has the advantages of low energy consumption, simple operation, and green environmental protection, thus becoming a current research hotspot. Although the rate of electron conduction and the efficiency of persulfate activation can be greatly improved by directly adding metal ions into the pollutant solution, the high-valent transition metals accumulated after the reaction will inhibit the activation of persulfate, resulting in a decrease in the reaction rate, and a large amount of metal ions are difficult to recover, resulting in waste of resources and secondary pollution of water bodies. Therefore, it is urgent to develop a heterogeneous persulfate catalyst with high activation efficiency loaded with metal oxides. Summary of the invention

[0005] Based on the problem that traditional powder materials are difficult to separate and recycle and the accumulation of high-valent transition metals in the process of persulfate activation by layered double hydroxides leads to a decrease in reaction rate, the present invention provides a magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxides, as well as a preparation method and application thereof.

[0006] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0007] A magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxides, wherein the layered double hydroxides are loaded on the magnetic material; the layered double hydroxides are tetrathiomolybdate intercalated copper-iron-aluminum layered double hydroxides.

[0008] Compared with the prior art, the magnetic material of the load tetrathiomolybdate intercalation layered double hydroxide of the present invention solves the problem that powder material is difficult to recycle in the way that layered double hydroxide is loaded on the surface of ferroferric oxide nanoparticles. At the same time, copper and iron two transition metals are loaded thereon in the form of heterogeneous catalysts, and potassium peroxodisulfate can be catalytically activated. In addition, tetrathiomolybdate is loaded in the layered double hydroxide in the form of interlayer anions, and the activation rate of potassium peroxodisulfate can be accelerated as an electron donor, so as to improve the free radical yield, accelerate the degradation rate of target pollutants (antibiotics such as doxycycline hydrochloride), and realize the complete degradation of antibiotics such as doxycycline hydrochloride in water. The catalyst of the present invention can be separated and recovered by magnetic separation means after use, avoiding the problems such as the loss of catalysts during catalytic degradation. In persulfate activation technology, the magnetic material of the load tetrathiomolybdate intercalation layered double hydroxide of the present invention has the versatility of efficient and rapid degradation of doxycycline hydrochloride and removal of antibiotic pollutants. At the same time, the magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide of the present invention can also effectively degrade antibiotic pollutants in complex water bodies, and is a universal catalyst material with great application value, which can efficiently degrade emerging organic pollutants through activated persulfate technology.

[0009] Furthermore, the magnetic material includes ferrosoferric oxide nanoparticles.

[0010] Furthermore, the preparation method of the magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide comprises the following steps: adding the precursor solution of the layered metal hydroxide to a dispersion of ferrosoferric oxide and ammonium tetrathiomolybdate, performing a coprecipitation reaction and then aging to obtain the magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide.

[0011] Furthermore, the molar ratio of iron, aluminum and copper in the precursor solution of the layered metal hydroxide is (2-4): (15-20): (50-70).

[0012] Furthermore, the precursor solution of the layered metal hydroxide is prepared by mixing ferric nitrate: copper nitrate: aluminum nitrate; the ferric nitrate includes ferric nitrate nonahydrate; the copper nitrate includes copper nitrate trihydrate; and the aluminum nitrate includes aluminum nitrate nonahydrate.

[0013] Furthermore, the molar ratio of the ferric nitrate to the ferroferric oxide is 1:4.5-20.

[0014] Furthermore, the ferroferric oxide nanoparticles and ammonium tetrathiomolybdate dispersion are a mixture after ultrasonic dispersion. Specifically, the ferroferric oxide and ammonium tetrathiomolybdate dispersion is prepared by adding ferroferric oxide and ammonium tetrathiomolybdate to a methanol aqueous solution and ultrasonically dispersing the mixture. The concentrations of ferroferric oxide and ammonium tetrathiomolybdate are 2.5 to 5 mg·mL -1 , 0.5~1mg·mL -1 This step can effectively inhibit the agglomeration of ferroferric oxide nanoparticles.

[0015] Furthermore, the ultrasonic dispersion time is 0.5±0.5h.

[0016] Furthermore, the volume ratio of methanol to water in the methanol water is 1:1.

[0017] Furthermore, the step of the coprecipitation reaction is specifically as follows: adding the precursor solution of the layered double hydroxide to the dispersion of ferrosoferric oxide nanoparticles and ammonium tetrathiomolybdate, stirring and mixing, and adjusting the pH to 10-11 using a NaOH solution to obtain the product.

[0018] Furthermore, the aging reaction step is specifically as follows: after the coprecipitation reaction is completed, the mixed solution is placed in a reaction kettle and reacted at 60±10° C. for 20±5 hours.

[0019] Furthermore, the preparation method also includes the following steps: after the aging reaction is completed, the magnetic composite material is separated by magnetic separation, washed with water for 3 to 6 times, the magnetic material is washed to neutrality, and dried at 60±10°C for 20±5h.

[0020] The invention also provides a method for degrading organic pollutants, comprising the following steps: using the magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide as a catalyst for activating persulfate to degrade organic pollutants in a solution.

[0021] Furthermore, the organic pollutants include antibiotics.

[0022] Furthermore, the antibiotics include at least one of tetracycline, oxytetracycline, chlortetracycline and doxycycline hydrochloride.

[0023] Furthermore, the initial concentration of the antibiotic in the solution is 5 to 50 mg·L -1 .

[0024] Furthermore, the pH of the solution is 5-9.

[0025] Furthermore, the water body of the solution is at least one of purified water, Pearl River water and tap water.

[0026] Furthermore, the persulfate comprises potassium peroxodisulfate.

[0027] Furthermore, the concentration of the potassium peroxodisulfate salt is 1 to 4 mmol·L -1 .

[0028] Furthermore, the catalyst concentration is 0.08 to 0.14 g·L -1 .

[0029] The present invention also provides an application of the magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide in the degradation of emerging organic pollutants.

[0030] In the present invention, these emerging organic pollutants have the characteristics of biological toxicity, persistence in the environment, and accumulation in organisms. Even at low concentrations in the environment, they may pose significant risks to ecosystems and human health.

[0031] Furthermore, the emerging organic pollutants include at least one of endocrine disruptors, drugs and personal care products, perfluorinated compounds, brominated flame retardants and microplastics. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The figure is a schematic flow chart of a method for preparing a magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide;

[0033] Figure 2 The CuFeAl-MoS4 prepared in Example 1 is ferroferric oxide nanoparticles. 2- -LDH@Fe3O4 SEM images, where Figure (a) is the SEM image of ferroferric oxide nanoparticles; Figures (b), (c) and (d) are the SEM images of CuFeAl-MoS4 prepared in Example 1 2- -SEM image of LDH@Fe3O4;

[0034] Figure 3 The CuFeAl-MoS4 prepared in Example 1 is ferroferric oxide nanoparticles. 2- -VSM diagram of LDH@Fe3O4;

[0035] Figure 4 A comparison of the removal rates of DOX within 7 minutes of reaction when the ferrosoferric oxide nanoparticles and the catalyst materials prepared in Examples 1 to 2 are used as catalysts for activating PDS;

[0036] Figure 5 CuFeAl-MoS4 prepared in Example 1 2- -Comparison of DOX removal rates at different catalyst dosages when LDH@Fe3O4 material is used as the catalyst;

[0037] Figure 6 CuFeAl-MoS4 prepared in Example 1 2- -Comparison of DOX removal rates at different PDS dosages when LDH@Fe3O4 material is used as catalyst;

[0038] Figure 7 CuFeAl-MoS4 prepared in Example 1 under different solution initial pH conditions 2- -The effect diagram of LDH@Fe3O4 material activating PDS to degrade DOX;

[0039] Figure 8 When different concentrations of chloride ions exist, the CuFeAl-MoS4 prepared in Example 1 2- -Comparison of the degradation effect of LDH@Fe3O4 materials on DOX;

[0040] Fig. 9 When different concentrations of nitrate ions are present, the CuFeAl-MoS4 prepared in Example 1 2- -Comparison of the degradation effect of LDH@Fe3O4 materials on DOX;

[0041] Fig.10 CuFeAl-MoS4 prepared in Example 1 2- -Degradation effect diagram of LDH@Fe3O4 material on OTC, TC, CTC and DOX;

[0042] Fig.11 CuFeAl-MoS4 prepared in Example 1 2- -Comparison of the degradation effect of DOX in different water bodies by LDH@Fe3O4 materials;

[0043] Fig.12 The CuFeAl-MoS4 prepared in Example 1 2- -ESR spectrum of LDH@Fe3O4 material as a PDS-activated catalyst. DETAILED DESCRIPTION

[0044] In order to solve the problems in the existing transition metal ion activation method for persulfate, such as low single transition metal ion circulation efficiency, resulting in high-valent transition metal accumulated after the reaction inhibiting the activation of persulfate, and difficulty in recovering transition metal ions, resulting in waste of resources and secondary pollution of water bodies, the present invention considers loading transition metal ions as active components of the catalyst and co-catalysts as electron donors on a carrier. When the material is used to activate persulfate, the transition metal ions as active components catalyze the persulfate to generate high-valent transition metal ions, and the co-catalysts as electron donors provide electrons for the high-valent transition metal ions to accelerate their reduction, thereby improving the activation efficiency of the catalyst for persulfate.

[0045] Based on this concept, the present invention designs the structure of the catalyst as a layered double hydroxide prepared by loading a variety of catalytically active metals on the surface of the carrier, and uses the co-catalyst as the interlayer anion to replace the interlayer anions of the original layered double hydroxide. Among them, layered double hydroxide (LDH), as a two-dimensional clay mineral, has attracted much attention due to its unique layered structure. It is composed of positively charged metal hydroxide layers and exchangeable anions between the layers. This structure gives LDH a series of significant properties, such as excellent chemical stability and exchangeability of interlayer anions. Based on this, the present invention first screens out transition metal iron and copper as the active components of the catalyst. Copper ions and iron ions can synergistically activate persulfate to produce a large number of sulfate radicals (SO4 ·- ) and hydroxyl radicals (·OH), improve the activation efficiency of persulfates (including PMS and PDS), and with the help of the structural stability of layered double hydroxides, it can effectively avoid the large-scale dissolution of iron ions and copper ions, making the catalyst stable in a wide pH range. In addition, the toxicity of these two transition metals is low, which can effectively avoid the problem of secondary pollution in the process of degrading organic pollutants.

[0046] Furthermore, the present invention selects tetrathiomolybdate as a co-catalyst of an electron donor to replace the interlayer anions of the original layered double hydroxide, further accelerates the circulation of transition metal ions, and improves the catalytic activity of the catalyst.

[0047] Furthermore, the present invention uses magnetic materials as carriers. After sewage treatment, the used catalyst can be separated and recovered by means of magnetic separation, thereby avoiding the loss of catalysts during catalytic degradation, thereby avoiding waste of resources and secondary pollution of water bodies. Based on this, the present invention selects ferrosoferric oxide as a carrier, which is conducive to the recycling of catalysts.

[0048] In addition, the structural stability of the layered double hydroxide is closely related to its chemical composition, and the catalytic performance of the catalyst is also related to the dispersibility of the active component. The higher the dispersibility of the active component, the higher the catalytic activity of the catalyst. Therefore, the present invention considers introducing a third metal ion to improve the dispersibility of transition metal iron and copper and the stability of the catalyst, thereby further improving the catalytic activity of the catalyst. The present invention selects metal aluminum as the third metal ion, which is one of the main components of typical hydrotalcite clay. The addition of aluminum ions can effectively improve the stability of the layered double hydroxide, thereby improving the stability of the catalyst, which is beneficial to the recycling and reuse of the catalyst, and can also assist the active components to be dispersed on the carrier surface in the form of extremely small nanoparticles and high dispersion. The electronegativity of aluminum is greatly different from that of iron and copper, and can form electron transfer between iron and copper, which is beneficial to the catalytic reaction.

[0049] Based on this, the specific preparation method of the catalyst of the present invention is: mixing the CuFeAl-LDH precursor solution with ferroferric oxide and ammonium tetrathiomolybdate, stirring evenly, aging, and drying.

[0050] The preparation step of the CuFeAl-LDH precursor solution includes mixing and stirring a copper source, an iron source and an aluminum source.

[0051] In order to improve the dispersibility of the active components in the catalyst, the present invention first mixes ferroferric oxide and ammonium tetrathiomolybdate to prepare a dispersion, and then mixes the dispersion with a CuFeAl-LDH precursor solution.

[0052] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0053] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0054] The reagents used in the following examples, unless otherwise specified, are all commercially available; the methods used in the following examples, unless otherwise specified, are all achievable by conventional methods.

[0055] Example 1

[0056] See also Figure 1In this embodiment, the magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide is prepared according to the following steps:

[0057] (1) Preparation of ferroferric oxide and ammonium tetrathiomolybdate dispersion: 0.15 g of ferroferric oxide nanoparticles and 0.0312 g of ammonium tetrathiomolybdate were added to 40 mL of methanol aqueous solution, and the mixture was evenly mixed and then ultrasonically dispersed for 30 min to obtain ferroferric oxide and ammonium tetrathiomolybdate dispersion.

[0058] (2) Preparation of CuFeAl-LDH precursor solution: Dissolve ferric nitrate nonahydrate, copper nitrate trihydrate, and aluminum nitrate nonahydrate in 22 mL of methanol and water and stir for 30 min to make the concentrations of Fe(NO3)3, Cu(NO3)2, and Al(NO3)3 2.9 mmol·L -1 、60mmol·L -1 and 18.8mmol·L -1 , and obtain CuFeAl-LDH precursor solution;

[0059] (3) Loading layered double hydroxides and exchanging interlayer anions: Add the above CuFeAl-LDH precursor solution to the above ferroferric oxide and ammonium tetrathiomolybdate dispersion, stir and mix evenly, adjust the pH of the solution to 10-11 with NaOH solution, place the solution in a polytetrafluoroethylene reactor, and age and react at 60°C for 24 hours. After the reaction is completed, separate the catalyst material by magnetic separation, wash the material with ultrapure water to neutrality, and then vacuum dry it at 60°C for 24 hours to obtain a magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxides, which is named CuFeAl-MoS4. 2- -LDH@Fe3O4.

[0060] The FeO nanoparticles and the CuFeAl-MoS4 prepared in this embodiment 2- -LDH@Fe3O4 was scanned by electron microscope, and the results are as follows Figure 2 As shown, it can be seen that tetrathiomolybdate intercalated layered double hydroxide is supported on ferrosoferric oxide nanoparticles.

[0061] See also Figure 3 , Figure 3 The CuFeAl-MoS4 prepared in this embodiment is ferroferric oxide nanoparticles. 2- -VSM diagram of LDH@Fe3O4, CuFeAl-MoS4 obtained in this example 2- -LDH@Fe3O4 has certain magnetic properties and a large saturation magnetization intensity.

[0062] Example 2

[0063] This embodiment prepares the magnetic material loaded with layered double hydroxide according to the following steps:

[0064] (1) Preparation of ferroferric oxide dispersion: Add 0.15 g of ferroferric oxide nanoparticles into 40 mL of methanol aqueous solution and disperse by ultrasonic for 30 min to obtain ferroferric oxide dispersion.

[0065] (2 Preparation of CuFeAl-LDH precursor solution: Dissolve ferric nitrate nonahydrate, copper nitrate trihydrate and aluminum nitrate nonahydrate in 22 mL of methanol water and stir for 30 min to make the concentrations of Fe(NO3)3, Cu(NO3)2 and Al(NO3)3 2.9 mmol·L -1 、60mmol·L -1 and 18.8mmol·L -1 , and obtain CuFeAl-LDH precursor solution;

[0066] (3) Loading layered double hydroxide: Add the above CuFeAl-LDH precursor solution to the above ferroferric oxide dispersion, stir and mix evenly, adjust the pH of the solution to 10-11 with NaOH solution, place the solution in a polytetrafluoroethylene reactor, and age and react at 60°C for 24 hours. After the reaction, separate the catalyst material by magnetic separation, wash the material with ultrapure water to neutrality, and then vacuum dry it at 60°C for 24 hours to obtain a magnetic material loaded with layered double hydroxide, which is named CuFeAl-LDH@Fe3O4.

[0067] Application Example 1: PDS activated by the magnetic material prepared in Examples 1 to 2 was used to degrade DOX.

[0068] Measure 50 mL containing 50 mg·L -1 Doxycycline hydrochloride solution simulated wastewater, adding 0.1 g·L -1 Catalysts (Fe3O4, CuFeAl-LDH@Fe3O4 or CuFeAl-MoS4 2- -LDH@Fe3O4), 2mmol·L -1 PDS (peroxydisulfate, potassium peroxydisulfate in this example) was used to perform degradation experiments in a constant temperature shaker at 25°C and 200rpm, with no catalyst added as a blank control. During the degradation process, 1.5 mL of sample was taken at regular intervals, and after filtering the sample with a 0.22 μm filter membrane, 1 mL of the filtrate was added to 0.5 mL of anhydrous ethanol, and the maximum absorbance value of the solution was tested near λ=349 nm by UV-visible spectrophotometry to quantify the residual doxycycline hydrochloride in the solution.

[0069] The effect of ferroferric oxide nanoparticles and the magnetic material prepared in Examples 1 to 2 on the activation of PDS to degrade doxycycline hydrochloride is as follows: Figure 4 As shown, compared with no catalyst added, Fe3O4, CuFeAl-LDH@Fe3O4 and CuFeAl-MoS4 2- -LDH@Fe3O4 significantly improved the removal rate of doxycycline hydrochloride by 6.0%, 78.4% and 89.3% within 7 minutes. 2- As the interlayer anion of LDH, MoS4 2- Fully contact with transition metal ions promotes the circulation of multivalent transition metal ions, thereby improving the catalytic activity of magnetic materials on PDS.

[0070] Application Example 2: Catalyst Dosage Optimization

[0071] Referring to Application Example 1, the CuFeAl-MoS4 prepared in Example 1 2- -LDH@Fe3O4 was used as the catalyst for activating PDS. Other parameters remained unchanged and the ratios of catalyst mass to total solution volume were controlled to be 0.08, 0.1, 0.12, and 0.14 g·L -1 Perform degradation experiments.

[0072] The removal effect of different catalyst dosages on doxycycline hydrochloride Figure 5 As shown, the catalyst dosage is 0.08, 0.1, 0.12 and 0.14 g·L -1 When the PDS dosage was 2.5, the removal rates of doxycycline hydrochloride within 7 min were 83.4%, 89.3%, 85.6% and 87.2% respectively. Application Example 3: Optimization of PDS dosage

[0073] Referring to Application Example 1, the CuFeAl-MoS4 prepared in Example 1 2- -LDH@Fe3O4 was used as the catalyst for activating PDS. Other parameters remained unchanged and the PDS concentrations were controlled to be 1, 2, 3 and 4 mmol·L -1 Perform degradation experiments.

[0074] Under different PDS dosage conditions, CuFeAl-MoS4 2- -LDH@Fe3O4 removal effect on doxycycline hydrochloride Figure 6 As shown, the PDS dosage was 1, 2, 3 and 4 mmol·L -1 When , the removal rates of doxycycline hydrochloride within 7 min were 82.7%, 89.0%, 94.2% and 94.4% respectively.

[0075] Application Example 4: Effect of the initial pH value of the solution on the degradation effect of doxycycline hydrochloride

[0076] Referring to Application Example 1, the CuFeAl-MoS4 prepared in Example 1 2- -LDH@Fe3O4 was used as a catalyst to activate PDS. Other parameters remained unchanged and the initial pH of the simulated wastewater was controlled to be 3, 5, 7 and 9 for degradation experiments.

[0077] CuFeAl-MoS4 under different solution initial pH conditions 2- -LDH@Fe3O4 removal effect on doxycycline hydrochloride Figure 7 As shown, when the initial pH of the solution was 3, 5, 7 and 9, the removal rates of doxycycline hydrochloride within 7 min were 39.0%, 93.2%, 88.5% and 90.3%, respectively.

[0078] Application Example 5: Effect of the Presence of Chloride Ions in the Solution on the Degradation of Doxycycline Hydrochloride

[0079] Referring to Application Example 1, the CuFeAl-MoS4 prepared in Example 1 2- -LDH@Fe3O4 was used as the catalyst for activating PDS. Other parameters remained unchanged and the chloride ion concentrations in the solution were controlled to be 0, 2, 5 and 8 mmol·L -1 Perform degradation experiments.

[0080] Under the conditions of different concentrations of chloride ions in the solution, CuFeAl-MoS4 2- -LDH@Fe3O4 removal effect on doxycycline hydrochloride Figure 8 As shown, the chloride ion concentration is 0, 2, 5 and 8 mmol·L -1 When , the removal rates of doxycycline hydrochloride within 30 min were 90.7%, 90.6%, 93.3% and 91.9% respectively.

[0081] Application Example 6: Effect of the Presence of Nitrate Ions in the Solution on the Degradation of Doxycycline Hydrochloride

[0082] Referring to Application Example 1, the CuFeAl-MoS4 prepared in Example 1 2- -LDH@Fe3O4 was used as the catalyst for activating PDS. Other parameters remained unchanged and the nitrate ion concentrations in the solution were controlled to be 0, 2, 5 and 8 mmol·L -1 Perform degradation experiments.

[0083] Under the condition of different concentrations of nitrate ions in the solution, CuFeAl-MoS4 2- -LDH@Fe3O4 removal effect on doxycycline hydrochloride Fig. 9 As shown, the nitrate concentration is 0, 2, 5 and 8 mmol·L -1When , the removal rates of doxycycline hydrochloride within 30 min were 90.7%, 87.9%, 89.9% and 88.5% respectively.

[0084] Application Example 7: Application of Magnetic Materials Loaded with Tetrathiomolybdate-Intercalated Layered Double Hydroxides in Degradation of Tetracycline Antibiotics

[0085] Referring to Application Example 1, the CuFeAl-MoS4 prepared in Example 1 2- -LDH@Fe3O4 was used as the catalyst for activating PDS. Other parameters remained unchanged. The antibiotics in the simulated wastewater were controlled to be 5 mg·L -1 Tetracycline (TC), 5 mg·L -1 Oxytetracycline (OTC), 5 mg·L -1 Chlortetracycline (CTC) or 5 mg·L -1 The degradation experiment of doxycycline hydrochloride (DOX) was carried out. At the same time, 5 mg·L -1 Tetracycline (TC), 5 mg·L -1 Oxytetracycline (OTC), 5 mg·L -1 Chlortetracycline (CTC), 5 mg·L -1 A mixed solution of doxycycline hydrochloride (DOX) was used as simulated wastewater for degradation experiments.

[0086] High performance liquid chromatography was used to determine the concentrations of four tetracycline antibiotic pollutants. Specifically, a gradient elution method was used to quantify multiple tetracycline target pollutants simultaneously: the mobile phase was 0.01 mol·L -1 Oxalic acid aqueous solution (A) and methanol acetonitrile solution (V 甲醇 :V 乙腈 =1:1, B) mixed solution, flow rate is 1.0mL·min -1 , the volume percentages of mobile phase B at 0.0min, 9.5min, 10.0min and 18.0min were 30%, 50%, 30% and 30% respectively. The concentrations of multiple tetracycline target pollutants were simultaneously determined by HPLC at a wavelength of 355nm, with a column temperature of 27℃, an injection volume of 25μL, and a C18 column. The elution peaks of OTC, TC, CTC and DOX were around 4.2, 4.5, 7.2 and 8.6min respectively.

[0087] Degradation results such as Fig.10 As shown, within 7 minutes, CuFeAl-MoS4 2- The degradation rates of OTC, TC, CTC and DOX by -LDH@Fe3O4 material were 98.5%, 96.9%, 92.9% and 98.6%, respectively; CuFeAl-MoS4 2-The simultaneous degradation rates of OTC, TC, CTC and DOX by -LDH@Fe3O4 material were 94.5%, 91.0%, 92.0% and 91.2%, respectively. Application Example 8: Application of the magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide to the degradation of pollutants in actual water samples

[0088] Referring to Application Example 1, the CuFeAl-MoS4 prepared in Example 1 2- -LDH@Fe3O4 was used as the catalyst for activating PDS. Other parameters remained unchanged and the concentrations of doxycycline hydrochloride in the solution were controlled to be 5, 10 and 20 mg·L -1 , the water bodies in the reaction solution are purified water, Pearl River water and tap water. The quantitative method of doxycycline hydrochloride in actual water samples is referred to Application Example 7.

[0089] Degradation results such as Fig.11 As shown, within 7 minutes, CuFeAl-MoS4 2- -LDH@Fe3O4 material was used in Pearl River water, tap water and ultrapure water to test 5mg·L -1 The removal rates of doxycycline hydrochloride were 97.7%, 99.4% and 98.6% respectively; CuFeAl-MoS4 2- -LDH@Fe3O4 material was used in Pearl River water, tap water and ultrapure water to measure 10 mg·L -1 The removal rates of doxycycline hydrochloride were 99.4%, 100.0% and 95.6% respectively; CuFeAl-MoS4 2- -LDH@Fe3O4 material was used in Pearl River water, tap water and ultrapure water to test 20mg·L -1 The removal rates of doxycycline hydrochloride were 99.1%, 100.0% and 95.9%, respectively.

[0090] Application Example 9:

[0091] CuFeAl-MoS4 prepared in Example 1 2- -LDH@Fe3O4 was used as the catalyst material, and 2 mmol·L -1 PDS and 0.1 g·L -1 DMPO (5,5-dimethyl-1-pyrroline-N-oxide) was added to the catalyst solution as a free radical scavenger. The concentration of DMPO was 20 mmol·L -1 After reacting for 2 minutes, 1 mL of the solution was taken and filtered through a 0.22 μm filter membrane. The free radical types contained in the system were tested using an electron spin resonance spectrometer (ESR) according to conventional methods.

[0092] The results are as follows Fig.12As shown, there are obvious 1:2:2:1 quadruple signal peaks and 1:1:1:1:1 sextuple signal peaks in the EPR spectrum, which belong to DMPO / ·OH and DMPO / SO4, respectively. ·- The characteristic peaks of the composite prove that the CuFeAl-MoS4 2- -LDH@Fe3O4 as a catalyst material in the Fenton-like reaction of CuFeAl-MoS4 2- -LDH@Fe3O4 activates PDS to produce free radicals, thereby degrading the target pollutants.

[0093] In summary, the present invention has the following advantages compared with the prior art:

[0094] 1. CuFeAl-MoS4 of the present invention 2- -LDH@Fe3O4, by loading layered double hydroxides on the surface of ferroferric oxide nanoparticles, reduces ion leakage and solves the problem of difficult recycling of powder materials. The used catalyst is separated and recycled by magnetic separation, avoiding problems such as catalyst loss during catalytic degradation.

[0095] 2. In the present invention, two transition metals, copper and iron, are loaded on the surface of ferroferric oxide nanoparticles in the form of heterogeneous catalysts. The two transition metals, copper and iron, synergistically catalyze and activate potassium peroxodisulfate salt: that is, both copper and iron transition metals can activate peroxodisulfate salt to generate a large number of sulfate free radicals and hydroxyl free radicals.

[0096] 3. The present invention loads tetrathiomolybdate in the layered double hydroxide in the form of interlayer anions, and uses it as an electron donor to increase the activation rate of potassium peroxodisulfate, thereby increasing the free radical yield, accelerating the degradation rate of organic pollutants, such as antibiotics such as doxycycline hydrochloride, and achieving complete degradation of antibiotics such as doxycycline hydrochloride in water.

[0097] 4. In the persulfate activation technology, the magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide of the present invention has the versatility of efficiently and rapidly degrading doxycycline hydrochloride and removing antibiotic pollutants: in the process of removing organic pollutants, the magnetic material of the present invention can activate PDS to produce a large number of sulfate radicals and hydroxyl radicals. Both sulfate radicals and hydroxyl radicals have strong oxidation ability, which can oxidize and degrade difficult-to-degrade organic pollutants into small molecular compounds until they are completely mineralized. At the same time, the magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide of the present invention can also effectively degrade organic pollutants such as antibiotics in complex water bodies. It is a universal catalyst material with great application value, which can efficiently degrade emerging organic pollutants by activating persulfate technology.

[0098] 5. The present invention uses CuFeAl-LDH as a precursor to prepare the catalyst. The addition of Al makes the metal elements such as Cu, Fe, and Al highly dispersed at the atomic level, effectively avoiding the phenomenon of agglomeration of active component nanoparticles in the material prepared by the loading method. In addition, the electronegativity of Al is greatly different from that of Cu and Fe, and can form electron transfer with the loaded metal, which is beneficial to the catalytic reaction and can also improve the structural stability of the catalyst.

[0099] 6. The magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide of the present invention can not only catalytically remove pollutants with high efficiency, but also maintain good stability, overcoming the problem that conventional technologies are seriously affected by inorganic anions such as chloride ions and carbonate ions. The magnetic material of the present invention has strong catalytic activity in the pH range of 5 to 9 and has a wide range of applications. It can also have a good removal effect at low dosage and low PDS concentration. The preparation method is simple, one-step synthesis, low price, and low toxicity.

[0100] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0101] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide, characterized in that: The layered double hydroxide is supported on a magnetic material; The layered double hydroxide is a copper-iron-aluminum layered metal hydroxide intercalated with tetrathiomolybdate.

2. The magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide according to claim 1, characterized in that: The magnetic material includes ferrosoferric oxide nanoparticles.

3. A method for preparing a magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide, characterized in that: The following steps are involved: The precursor solution of the layered metal hydroxide is added to the dispersion of ferroferric oxide and ammonium tetrathiomolybdate, and then aged after a coprecipitation reaction to obtain the magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide.

4. The preparation method according to claim 3, characterized in that: The pH value in the coprecipitation reaction is 10-11, and the aging time is 20±5h.

5. The preparation method according to claim 3, characterized in that: The method for preparing the ferroferric oxide and tetrathiomolybdate dispersion is as follows: adding ferroferric oxide and ammonium tetrathiomolybdate to a methanol aqueous solution and ultrasonically dispersing the mixture, wherein the concentrations of ferroferric oxide and ammonium tetrathiomolybdate are 2.5 to 5 mg·mL -1 , 0.5~1mg·mL -1 .

6. The preparation method according to claim 3, characterized in that: The molar ratio of iron, aluminum and copper in the precursor solution of the layered metal hydroxide is (2-4): (15-20): (50-70).

7. The preparation method according to claim 6, characterized in that: The precursor solution of the layered metal hydroxide is prepared by mixing ferric nitrate, copper nitrate and aluminum nitrate; the molar ratio of the ferric nitrate to the ferrosoferric oxide is 1:4.5-20.

8. A method for degrading organic pollutants, characterized in that: The method comprises the following steps: using the magnetic material loaded with tetrathiomolybdate intercalated layered double hydroxide according to any one of claims 1 or 2 as a catalyst for activating persulfate to degrade organic pollutants in a solution.

9. The method according to claim 8, characterized in that The organic pollutants include at least one of antibiotics, endocrine disruptors, drugs and personal care products, perfluorinated compounds, brominated flame retardants and microplastics.

10. The method according to claim 8, characterized in that: The concentration of the catalyst is 0.08 to 0.14 g·L -1 The concentration of the persulfate is 1 to 4 mmol·L -1 , the pH of the solution is 5-9.

Citation Information

Patent Citations

  • Method for synthesizing molybdenum disulfide single-layer nanometer sheets by space limited range method

    CN108394935A

  • Ternary iron-magnesium-zinc layered double hydroxide catalyst with tetrathiomolybdate intercalation as well as preparation method and application of ternary iron-magnesium-zinc layered double hydroxide catalyst

    CN121927623A