Mixed molecular sieve supported gold nanoparticle catalyst, preparation method and propylene gas-phase epoxidation method

By loading a mixed molecular sieve catalyst with a high content of zero-valent gold nanoparticles on titanium-silicon and tin-silicon molecular sieves, the low efficiency problem caused by incomplete reduction of Au in existing catalysts is solved, and the conversion rate of propylene gas-phase epoxidation reaction is significantly improved. and selectivity.

CN118767984AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310372484.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

Existing propylene gas phase epoxidation catalysts are unsatisfactory in terms of propylene conversion rate and propylene oxide selectivity, mainly because the Au nanoparticles are not completely reduced to the 0 valence state, resulting in low catalytic reaction efficiency.

Method used

A mixed molecular sieve is used to load gold nanoparticle catalysts, and titanium silicon and tin silicon molecular sieves are used as carriers to load 0.01-1% by weight of gold nanoparticles to ensure that the proportion of 0-valent Au in the gold nanoparticles exceeds 85%, and control titanium silicon and The molar ratio of tin to silicon is between 0.005-0.04:1, and the particle size is less than 5nm, which improves the catalytic activity.

Benefits of technology

The propylene conversion rate of the propylene gas-phase epoxidation reaction is significantly increased to 8-16%, and the propylene oxide selectivity reaches 85-95%, improving the economy and environmental protection of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767984A_ABST
    Figure CN118767984A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of inorganic chemistry and catalytic chemistry, and discloses a mixed molecular sieve supported gold nanoparticle catalyst, a preparation method and a propylene gas-phase epoxidation method. The catalyst comprises a carrier and gold nanoparticles loaded on the carrier, wherein the carrier is a mixed carrier containing a titanium silicalite molecular sieve and a tin silicalite molecular sieve; wherein on the basis of the total weight of the catalyst, the content of the gold nanoparticles is 0.01 to 1 weight percent; wherein in terms of Au element, the proportion of zero-valence Au in the gold nanoparticles is greater than 85%; wherein in the catalyst, the molar ratio of titanium to silicon is (0.005-0.04): 1, and the molar ratio of tin to silicon is (0.005-0.04): 1. When the catalyst provided by the invention is used for catalyzing propylene gas-phase epoxidation reaction, the catalyst has relatively high catalytic activity, the propylene conversion rate is increased to 8-16%, and the epoxypropane selectivity can reach 85-95%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic chemistry and catalytic chemistry, and in particular to a mixed molecular sieve-loaded gold nanoparticle catalyst and a preparation method thereof, and a method for gas-phase epoxidation of propylene. Background Art

[0002] Propylene oxide (C3H6O) is one of the three major propylene derivatives, along with polypropylene and acrylonitrile, and is mainly used to produce organic chemical raw materials such as polyether polyols and propylene glycol. At present, the industrial production of propylene oxide mainly adopts the chlorohydrin method and the co-oxidation process. However, the chlorohydrin method requires the use of a large amount of highly toxic chlorination reagents, which is very easy to corrode equipment and produce a large amount of wastewater and chlorinated byproducts, which seriously violates the current social demand for green chemistry. In view of the requirements of laws and regulations and the people's increasing environmental awareness, the chlorohydrin method for producing propylene oxide will be gradually eliminated. The co-oxidation method effectively avoids the disadvantages of the chlorohydrin method of polluting the environment and serious corrosion, but the ethylbenzene / isobutane co-oxidation method will produce a large amount of styrene / tert-butyl alcohol products while producing propylene oxide, which greatly restricts the economic efficiency of this process. Based on the unsatisfactory status of the above two production routes, the H2O2 liquid phase epoxidation process for preparing propylene oxide (HPPO method) came into being. At present, researchers have a deep understanding of this reaction mechanism and are committed to industrial production. However, as one of the main raw materials, H2O2 is used in large quantities and has harsh transportation conditions. Therefore, an H2O2 synthesis device must be installed to meet the economic efficiency of the HPPO process, but this will also limit the layout of the HPPO process. To further remove this limitation, the process of preparing propylene oxide by direct epoxidation of propylene in gas phase has received great attention from researchers. This route uses H2 and O2 as raw materials, synthesizes H2O2 in situ, and then oxidizes propylene to propylene oxide. The gas-phase epoxidation process is a gas-solid two-phase reaction, which is easy to operate and the products are easy to separate. It is highly economical and the process is green and environmentally friendly, which has obvious advantages over the HPPO method.

[0003] The occurrence of propylene gas phase epoxidation reaction is mainly driven by catalysts. Au / TS-1 catalyst shows good catalytic effect for this reaction, which is due to the synergistic effect between Au nanoparticles and TS-1 molecular sieve. The Au active site catalyzes H2 and O2 to generate HOOH species in situ, and further, the framework Ti atoms catalyze the oxygenation of propylene double bonds. Among them, the generation of HOOH is the rate-determining step, and this step requires Au 0 Au supported on TS-1 molecular sieve usually exists in an oxidized state, so it is necessary to reduce Au to zero valence through activation. However, due to the interaction of the skeleton atoms on the TS-1 carrier, some of the reduced Au nanoparticles are not completely reduced to zero valence, so the catalytic effect of the propylene gas phase epoxidation catalyst in the prior art is not ideal.

[0004] Therefore, it is necessary to take measures to make the propylene epoxidation catalyst have more zero-valent Au active sites, or to make improvements in other aspects to improve the catalytic reaction effect. Summary of the invention

[0005] The purpose of the present invention is to overcome the problem that the propylene conversion rate and propylene oxide selectivity are low when the propylene epoxidation catalyst in the prior art is used for propylene gas phase epoxidation reaction, and to provide a mixed molecular sieve supported gold nanoparticle catalyst and a preparation method and a method for propylene gas phase epoxidation. When the mixed molecular sieve supported gold nanoparticle catalyst provided by the present invention is used for propylene gas phase epoxidation reaction, the propylene conversion rate is significantly improved, and the catalyst has a high propylene oxide selectivity.

[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a hybrid molecular sieve loaded gold nanoparticle catalyst, which comprises a carrier and gold nanoparticles loaded on the carrier, wherein the carrier is a mixed carrier containing titanium silicon molecular sieve and tin silicon molecular sieve; wherein, based on the total weight of the catalyst, the content of the gold nanoparticles is 0.01-1% by weight, preferably 0.04-0.8% by weight; wherein, calculated as Au element, the proportion of zero-valent Au in the gold nanoparticles is greater than 85%; wherein, in the catalyst, the molar ratio of titanium to silicon is 0.005-0.04:1, and the molar ratio of tin to silicon is 0.005-0.04:1.

[0007] Preferably, in the catalyst, the particle size of the gold nanoparticles is less than 5 nm, preferably less than 3 nm.

[0008] Preferably, the titanium silicon molecular sieve is one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0009] Preferably, the tin-silicon molecular sieve is one or more of Sn-MFI molecular sieve, Sn-USY molecular sieve, Sn-Beta molecular sieve and Sn-MEL molecular sieve.

[0010] The second aspect of the present invention provides a method for preparing the hybrid molecular sieve supported gold nanoparticle catalyst described in the first aspect, the method comprising the following steps:

[0011] S1, mixing titanium silicon molecular sieve, tin silicon molecular sieve and a gold-containing compound aqueous solution, and then adjusting the pH value of the resulting mixture to alkaline, wherein the amount of the gold-containing compound aqueous solution calculated as Au element is 0.05-5% by weight of the total amount of the titanium silicon molecular sieve and the tin silicon molecular sieve;

[0012] S2, performing solid-liquid separation on the product obtained in step S1, and activating the obtained solid product.

[0013] Preferably, in step S1, the weight ratio of the titanium silicon molecular sieve to the tin silicon molecular sieve is 1:0.01-5.

[0014] Preferably, in step S1, the titanium-silicon molar ratio in the titanium-silicon molecular sieve is 0.005-0.04:1.

[0015] Preferably, in step S1, the molar ratio of tin to silicon in the tin-silicon molecular sieve is 0.005-0.04:1.

[0016] Preferably, in step S1, the titanium silicon molecular sieve is selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0017] Preferably, in step S1, the tin-silicon molecular sieve is selected from one or more of Sn-MFI molecular sieve, Sn-USY molecular sieve, Sn-Beta molecular sieve and Sn-MEL molecular sieve.

[0018] Preferably, in step S1, the gold compound aqueous solution is selected from one or more of an aqueous solution of chloroauric acid, an aqueous solution of cesium chloroaurate and an aqueous solution of potassium chloroaurate.

[0019] Preferably, in step S1, the concentration of the gold compound aqueous solution is 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, and more preferably 0.005-0.05 mol / L.

[0020] Preferably, in step S1, the amount of the gold-containing compound aqueous solution calculated as Au element is 0.1-5 wt % of the total amount of the titanium silicon molecular sieve and the tin silicon molecular sieve.

[0021] Preferably, in step S1, the pH value of the mixture is adjusted to 7-10, preferably 7-9.

[0022] Preferably, in step S1, the pH adjuster used to adjust the pH value of the mixture is an alkaline solution.

[0023] Preferably, the alkaline solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, cesium hydroxide solution, urea solution, sodium carbonate solution, sodium bicarbonate solution, potassium carbonate solution, potassium bicarbonate solution, cesium carbonate solution and cesium bicarbonate solution.

[0024] Preferably, in step S2, the activation conditions include: temperature of 150-300°C and time of 1-5 hours.

[0025] The third aspect of the present invention provides a hybrid molecular sieve-loaded gold nanoparticle catalyst prepared by the method described in the second aspect.

[0026] The fourth aspect of the present invention provides a method for gas-phase epoxidation of propylene, the method comprising: in the presence of a protective gas and a catalyst, mixing hydrogen, oxygen and propylene for reaction to obtain propylene oxide; the catalyst is the mixed molecular sieve loaded gold nanoparticle catalyst described in the first aspect or the mixed molecular sieve loaded gold nanoparticle catalyst described in the third aspect.

[0027] Preferably, the reaction conditions include: the volume flow ratio of hydrogen, oxygen and propylene is 0.5-2:0.5-2:1.

[0028] Preferably, the volume flow rate ratio of propylene to protective gas is 1:1-10.

[0029] Preferably, the reaction conditions include: temperature of 100-250° C. and pressure of 0.1-0.7 MPa.

[0030] Preferably, the reaction conditions include: temperature of 120-220° C. and pressure of 0.1-0.5 MPa.

[0031] The mixed molecular sieve supported gold nanoparticle catalyst provided by the present invention adopts a mixture of titanium silicon molecular sieve and tin silicon molecular sieve as a carrier, has a large number of zero-valent gold nanoparticles on the catalyst, and contains a specific titanium silicon molar ratio, a tin silicon molar ratio and a specific content of gold nanoparticles in the catalyst. The catalyst with these characteristics has high catalytic activity when catalyzing propylene gas phase epoxidation reaction, the propylene conversion rate can be increased to 8-16%, and the propylene oxide selectivity can reach 85-95%. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is the XPS spectra of the catalysts prepared in Example 1 and Comparative Example 5;

[0033] Figure 2 is a HAADF-STEM image of the catalyst obtained in Example 1;

[0034] Figure 3 This is the HAADF-STEM image of the catalyst obtained in Comparative Example 5. DETAILED DESCRIPTION

[0035] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0036] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0037] The first aspect of the present invention provides a hybrid molecular sieve supported gold nanoparticle catalyst, the catalyst comprising a carrier and gold nanoparticles supported on the carrier, wherein the carrier is a hybrid carrier containing titanium silicon molecular sieve and tin silicon molecular sieve, wherein the titanium silicon molecular sieve and the tin silicon molecular sieve exist in the form of a physical mixture.

[0038] In the present invention, the use of titanium silicon molecular sieve and tin silicon molecular sieve as a mixed carrier to load gold nanoparticles can improve the catalytic activity of the catalyst and improve the propylene conversion rate of the propylene epoxidation reaction. The inventors have found that Sn and Ti additives can jointly provide electrons to Au to obtain more electron-rich Au. 0 Active sites, thereby effectively promoting the rate-determining step of in-situ synthesis of H2O2 by hydrogen and oxygen, and having a high propylene conversion rate when applied to propylene gas-phase epoxidation reaction.

[0039] According to the present invention, the content of gold nanoparticles, tin-silicon molar ratio, and titanium-silicon molar ratio in the catalyst all have a greater impact on improving propylene conversion and propylene oxide selectivity during catalytic propylene gas phase epoxidation reaction. Wherein, based on the gross weight of the catalyst, the content of the gold nanoparticles can be 0.01-1% by weight, preferably 0.04-0.8% by weight. Wherein, in the catalyst, the titanium-silicon molar ratio can be 0.005-0.04:1, and the tin-silicon molar ratio can be 0.005-0.04:1.

[0040] In the present invention, the content of gold nanoparticles in the catalyst is measured by ICP. In the present invention, the titanium-silicon molar ratio and the tin-silicon molar ratio are detected and calculated by an X-ray fluorescence spectrometer, wherein the instrument model is a ZSM Primus II X-ray fluorescence spectrometer of Rigaku Corporation, Japan, and the test conditions are a rhodium target, an excitation voltage of 40 kV, and an excitation current of 250 mA.

[0041] In the present invention, in order to improve the catalytic activity of the catalyst in the gas-phase epoxidation reaction of propylene, and to improve the propylene conversion rate and the selectivity of propylene oxide, the catalyst needs to have a higher proportion of zero-valent Au. Wherein, in terms of Au element, the proportion of zero-valent Au in the gold nanoparticles is greater than 85%, which is detected and calculated by XPS.

[0042] According to the present invention, XPS characterization obtains zero-valent Au (Au 0) The center of the characteristic peak is located at 83-84eV; the peak area of ​​0-valent Au peak is more than 85% of the total peak area after peak separation by XPS peak software. The XPS measurement was carried out on the ESCALab250 X-ray photoelectron spectrometer of Thermo Fisher Scientific, with the excitation source being monochromatic Al Kα X-ray, energy of 1486.6eV, power of 150W; the penetration energy used for narrow scanning was 30eV; the basic vacuum during analysis was about 6.5×10 - 8 Pa.

[0043] Research has found that in the present invention, the particle size of the gold nanoparticles has a great influence on improving the catalytic effect of the catalyst. In order to improve the catalytic activity of the catalyst in the gas-phase epoxidation reaction of propylene, improve the propylene conversion rate and the selectivity of propylene oxide, preferably, in the catalyst, the particle size of the gold nanoparticles is less than 5nm, and more preferably less than 3nm. The particle size of the gold nanoparticles is obtained by high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) observation.

[0044] According to the present invention, the type of the titanium silicon molecular sieve is not limited, as long as it is a molecular sieve containing silicon, titanium and oxygen.

[0045] In some preferred embodiments, the titanium silicalite molecular sieve may be selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0046] According to the present invention, the type of the tin-silicon molecular sieve is not limited, as long as it is a molecular sieve containing silicon, tin and oxygen.

[0047] In some preferred embodiments, the tin-silicon molecular sieve is one or more of Sn-MFI molecular sieve, Sn-USY molecular sieve, Sn-Beta molecular sieve and Sn-MEL molecular sieve.

[0048] The second aspect of the present invention provides a method for preparing the hybrid molecular sieve supported gold nanoparticle catalyst described in the first aspect, the method comprising the following steps:

[0049] S1, mixing titanium silicon molecular sieve, tin silicon molecular sieve and an aqueous solution of a gold compound, and then adjusting the pH value of the resulting mixture to alkaline;

[0050] S2, performing solid-liquid separation on the product obtained in step S1, and activating the obtained solid product.

[0051] In the present invention, titanium silicon molecular sieve and tin silicon molecular sieve are used as mixed carriers, and Au is loaded by a deposition precipitation method to obtain the mixed molecular sieve loaded gold nanoparticle catalyst of the present invention. The method is simple and easy to operate.

[0052] In the present invention, too high an amount of the gold compound will lead to the aggregation of gold nanoparticles, which will cause side reactions during the propylene gas phase epoxidation reaction, resulting in a decrease in the selectivity of propylene oxide; too low an amount of the gold compound will lead to a decrease in the catalytic activity of the prepared catalyst, so it is necessary to control the amount of the gold compound so that an appropriate amount of gold nanoparticles is loaded on the mixed molecular sieve. Specifically, in the present invention, the amount of the gold compound aqueous solution in terms of Au element is 0.05-5% by weight of the total amount of the titanium silicon molecular sieve and the tin silicon molecular sieve, preferably 0.1-5% by weight, for example, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5% by weight.

[0053] In order to improve the catalytic performance of the prepared catalyst in the present invention, preferably, in step S1, the weight ratio of the titanium silicon molecular sieve to the tin silicon molecular sieve can be 1:0.01-5.

[0054] According to the present invention, in order to further improve the catalytic activity and selectivity of the prepared catalyst, preferably, in step S1, the molar ratio of titanium to silicon in the titanium silicalite molecular sieve can be 0.005-0.04:1.

[0055] According to the present invention, in order to further improve the catalytic activity and selectivity of the prepared catalyst, preferably, in step S1, the molar ratio of tin to silicon in the tin-silicon molecular sieve is 0.005-0.04:1.

[0056] According to the present invention, the type of the titanium silicon molecular sieve is not limited, as long as it is a molecular sieve containing silicon, titanium and oxygen.

[0057] In some preferred embodiments, the titanium silicalite molecular sieve may be selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0058] According to the present invention, the type of the tin-silicon molecular sieve is not limited, as long as it is a molecular sieve containing silicon, tin and oxygen.

[0059] In some preferred embodiments, the tin-silicon molecular sieve is one or more of Sn-MFI molecular sieve, Sn-USY molecular sieve, Sn-Beta molecular sieve and Sn-MEL molecular sieve.

[0060] In the present invention, the titanium silicon molecular sieve and the tin silicon molecular sieve can be purchased commercially, prepared according to the methods in the prior art, or prepared by oneself.

[0061] In the present invention, the gold-containing compound aqueous solution can be an aqueous solution well known to those skilled in the art. Preferably, in step S1, the gold-containing compound aqueous solution is selected from one or more of chloroauric acid aqueous solution, cesium chloroaurate aqueous solution and potassium chloroaurate aqueous solution.

[0062] The present invention has no particular restrictions on the manner in which the titanium silicon molecular sieve, the tin silicon molecular sieve and the gold-containing compound aqueous solution are mixed. Preferably, the titanium silicon molecular sieve, the tin silicon molecular sieve and the gold-containing compound aqueous solution in the present invention can be mixed by stirring at room temperature. Similarly, adjusting the pH value of the obtained mixture to alkaline can also be achieved by stirring at room temperature.

[0063] In a preferred embodiment, the process of mixing the titanium silicon molecular sieve, the tin silicon molecular sieve and the gold compound aqueous solution can be: firstly prepare the gold compound aqueous solution with water, and then mix the titanium silicon molecular sieve, the tin silicon molecular sieve and the gold compound aqueous solution to obtain a mixture. In this article, unless otherwise specified, room temperature refers to 20-30°C.

[0064] In order to further improve the catalytic performance of the catalyst, improve the propylene conversion rate and the propylene oxide selectivity, under preferred conditions, in step S1, the concentration of the gold compound aqueous solution can be 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, more preferably 0.005-0.05 mol / L, for example 0.005 mol / L, 0.008 mol / L, 0.01 mol / L, 0.015 mol / L, 0.02 mol / L, 0.025 mol / L, 0.03 mol / L, 0.035 mol / L, 0.04 mol / L, 0.045 mol / L or 0.05 mol / L.

[0065] In some preferred embodiments, in step S1, the pH value corresponding to alkalinity may be 7-10, preferably 7-9, such as 7, 7.5, 8, 8.5 or 9. According to the present invention, specifically, after the pH value of the obtained mixture is adjusted to alkalinity, the obtained product is a suspension.

[0066] In the present invention, specifically, the pH adjusting agent used to adjust the pH value of the mixture is an alkaline solution. The type and concentration of the alkaline solution are not specifically limited, as long as the pH value of the mixture can be adjusted to a specific alkalinity. Preferably, the alkaline solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, cesium hydroxide solution, urea solution, sodium carbonate solution, sodium bicarbonate solution, potassium carbonate solution, potassium bicarbonate solution, cesium carbonate solution and cesium bicarbonate solution.

[0067] In the present invention, the solid-liquid separation method of the product obtained in step S1 can be various solid-liquid separation methods well known to those skilled in the art, as long as the solid product and the liquid can be separated. Preferably, the solid-liquid separation method is filtration or centrifugation.

[0068] In some preferred embodiments of the present invention, in order to improve the catalytic performance of the catalyst, further improve the propylene conversion rate and propylene oxide selectivity, in step S2, the activation conditions include: temperature of 150-300°C, for example, 150°C, 180°C, 200°C, 220°C, 250°C, 280°C or 300°C; time of 1-5h, for example, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h. In a preferred embodiment, the activation process includes: calcination at 150-300°C in air atmosphere for 1-5h.

[0069] The third aspect of the present invention provides a hybrid molecular sieve-loaded gold nanoparticle catalyst prepared by the method described in the second aspect.

[0070] In some preferred embodiments of the present invention, the catalyst includes a carrier and gold nanoparticles loaded on the carrier, wherein the carrier is a mixed carrier containing titanium silicon molecular sieve and tin silicon molecular sieve; wherein, based on the total weight of the catalyst, the content of the gold nanoparticles is 0.01-1% by weight, preferably 0.04-0.8% by weight; wherein, calculated as Au element, the proportion of zero-valent Au in the gold nanoparticles is greater than 85%; wherein, in the catalyst, the molar ratio of titanium to silicon is 0.005-0.04:1, and the molar ratio of tin to silicon is 0.005-0.04:1.

[0071] In order to improve the catalytic performance of the catalyst, in the catalyst of the present invention, preferably, the particle size of the gold nanoparticles is less than 5 nm, and more preferably less than 3 nm.

[0072] According to the present invention, the type of the titanium silicon molecular sieve is not limited, as long as it is a molecular sieve containing silicon, titanium and oxygen.

[0073] In some preferred embodiments, the titanium silicalite molecular sieve may be selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0074] According to the present invention, the type of the tin-silicon molecular sieve is not limited, as long as it is a molecular sieve containing silicon, tin and oxygen.

[0075] In some preferred embodiments, the tin-silicon molecular sieve is one or more of Sn-MFI molecular sieve, Sn-USY molecular sieve, Sn-Beta molecular sieve and Sn-MEL molecular sieve.

[0076] The catalyst prepared by the method of the present invention is used in catalyzing propylene gas phase epoxidation reaction, and the propylene conversion rate can reach 8-16%, and the propylene oxide selectivity can reach 85-95%.

[0077] The fourth aspect of the present invention provides a method for gas-phase epoxidation of propylene, the method comprising: in the presence of a protective gas and a catalyst, mixing hydrogen, oxygen and propylene for reaction to obtain propylene oxide; the catalyst is the mixed molecular sieve loaded gold nanoparticle catalyst described in the first aspect or the mixed molecular sieve loaded gold nanoparticle catalyst described in the third aspect.

[0078] According to the present invention, under preferred conditions, the reaction conditions include: the volume flow ratio of the hydrogen, oxygen and propylene is 0.5-2:0.5-2:1.

[0079] More preferably, the volume flow ratio of propylene to protective gas is 1:1-10. In the present invention, the protective gas is nitrogen and / or an inert gas.

[0080] In some preferred embodiments of the present invention, the reaction conditions further include: temperature of 100-250° C. and pressure of 0.1-0.7 MPa; further preferably, temperature of 120-200° C. and pressure of 0.1-0.5 MPa.

[0081] In the present invention, the method for gas-phase epoxidation of propylene can be operated in a continuous manner. Specifically, after the catalyst is loaded into the reactor, a mixture of hydrogen, oxygen, propylene and protective gas is continuously added to carry out the reaction.

[0082] The present invention has no special requirements on the form of the catalyst. The catalyst can be a mixed molecular sieve loaded with gold nanoparticle powder, or it can be further loaded on a carrier for use. Those skilled in the art can choose according to the type of reactor.

[0083] In the present invention, the separation of the propylene gas-phase epoxidation product and the catalyst can be adjusted according to the form of the catalyst and actual needs. For example, when the catalyst is a mixed molecular sieve loaded with gold nanoparticle powder, the product separation and the catalyst recovery and reuse can be achieved by sedimentation, filtration, centrifugation, evaporation, membrane separation and the like; when the catalyst is a mixed molecular sieve loaded with gold nanoparticles (molded catalyst) loaded on a carrier, the molten catalyst can be loaded into a fixed bed reactor, and the catalyst can be recovered after the reaction is completed.

[0084] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto. Unless otherwise specified, the raw materials used in the following examples are all chemically pure reagents.

[0085] In the present invention:

[0086] The content of gold nanoparticles was measured by inductively coupled plasma (ICP).

[0087] The particle size of gold nanoparticles was observed by high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM).

[0088] The contents of tin, silicon and titanium were analyzed by X-ray fluorescence spectrometry using a ZSM Primus II X-ray fluorescence spectrometer produced by Rigaku Corporation of Japan. The test conditions were a rhodium target, an excitation voltage of 40 kV, and an excitation current of 250 mA.

[0089] The proportion of zero-valent Au in the catalyst was detected and calculated by XPS. XPS determination was performed on an ESCALab250 X-ray photoelectron spectrometer from Thermo Fisher Scientific. The excitation source was monochromatic Al Kα X-rays with an energy of 1486.6 eV and a power of 150 W. The penetration energy used for narrow scanning was 30 eV. The basic vacuum during analysis was approximately 6.5×10 - 8 Pa.

[0090] Preparation Examples 1-3 are used to illustrate the preparation process of tin silicon molecular sieve.

[0091] Preparation Example 1 Preparation of Sn-MFI Molecular Sieve

[0092] Dissolve tin tetrachloride pentahydrate (SnCl4.5H2O) in water, add tetraethyl orthosilicate (TEOS) to the aqueous solution and stir, add tetrapropylammonium hydroxide (TPAOH, 20% aqueous solution) and water under stirring, continue stirring for 30 minutes to obtain a clear liquid with a chemical composition of 0.03SnO2:SiO2:0.45TPA:35H2O, then crystallize at 433K for 2 days, filter the obtained solid, wash with distilled water, dry at 393K for 5 hours, and then calcine at 823K for 10 hours to obtain Sn-MFI molecular sieve. Among them, the amount of TEOS used is 15.31g, the amount of TPAOH used is 33.67g, and the amount of SnCl 4.5 The amount of H2O used was 0.38 g, and the amount of water used was 39.64 g.

[0093] Preparation Example 2 Preparation of Sn-Beta Molecular Sieve

[0094] Dissolve tin tetrachloride pentahydrate (SnCl4.5H2O) in water, add the aqueous solution to tetraethyl orthosilicate (TEOS) and stir, add tetraethylammonium hydroxide (TEAOH) under stirring, stir until TEOS evaporates to obtain alcohol, add hydrogen fluoride (HF) to the clear liquid to form a paste-like thin layer. Finally, add a suspension of dealuminated nano-Beta seeds (20nm) and water to obtain a clear liquid with a chemical composition of 0.03SnO2:SiO2:6TEA:15H2O:10HF, then crystallize at 413K for 10 days, filter the obtained solid, wash with distilled water, dry at 393K for 5 hours, and then calcine at 823K for 10 hours to obtain Sn-Beta molecular sieve. Among them, the amount of TEOS used is 20.81g, the amount of TEAOH used is 88.42g, the amount of SnCl4.5H2O used is 1.05g, the amount of water used is 27.01g, and the amount of HF used is 20g.

[0095] Preparation Example 3 Preparation of Sn-USY Molecular Sieve

[0096] The H-USY molecular sieve was mixed with nitric acid, treated at 85℃ for 8h, the sample was filtered and washed with deionized water, and dried at 120℃ for 12h to obtain a solid sample. The solid sample was mixed with tin tetrachloride pentahydrate (SnCl4.5H2O) for 1h to obtain a mixed liquid with a chemical composition of 0.03SnO2:100SiO2, dried at 100℃ for 12h, and finally calcined at 550℃ for 3h to obtain Sn-USY molecular sieve. Among them, the amount of H-USY used was 2.0g, the amount of nitric acid used was 50mL, and the amount of SnCl4.5H2O used was 0.6g.

[0097] Preparation Examples 4-6 are used to illustrate the preparation process of titanium silicalite molecular sieve.

[0098] Preparation Example 4 Preparation of TS-1 Molecular Sieve

[0099] About 3 / 4 of tetrapropylammonium hydroxide (TPAOH, 20%, purchased from Aldrich, USA) solution is added to tetraethyl orthosilicate (TEOS) solution to obtain a liquid mixture with a pH of about 13, and then the required amount of anhydrous isopropanol solution of n-butyl titanate [Ti(OBu)4] is added dropwise to the obtained liquid mixture under vigorous stirring. After stirring for 15 minutes, a clear liquid is obtained. Finally, the remaining TPAOH is slowly added to the clear liquid and stirred at 348-353K for about 3 hours to obtain a sol with a chemical composition of 0.03TiO2:SiO2:0.36TPA:35H2O. The sol is then crystallized at 443K for 3 days, and then the obtained solid is filtered, washed with distilled water, dried at 373K for 5 hours, and then calcined at 823K for 10 hours to obtain TS-1 molecular sieve. Among them, the amount of TEOS used is 42g, the amount of TPAOH used is 73g, the amount of Ti(OBu)4 used is 2g, the amount of anhydrous isopropanol used is 10g, and the amount of water used is 68g.

[0100] Preparation Example 5 Preparation of TS-2 molecular sieve

[0101] A certain amount of tetrabutylammonium hydroxide solution (TBAOH, 20%) was mixed with tetraethyl orthosilicate (TEOS), and then the required amount of anhydrous isopropanol solution of n-butyl titanate [Ti(OBu)4] was added to the obtained transparent liquid mixture under vigorous stirring, and the hydrolysis was completed after stirring for 30 minutes to obtain a clear liquid. Finally, 2 times the required amount of distilled water was added, and the obtained sol was stirred at 348-353K for 2h to remove alcohol. The chemical composition of the obtained sol is 0.03TiO2:SiO2:0.2TBA:20H2O. The sol was placed at 443K for crystallization for 3 days, and the obtained crystallized product was filtered, washed with water, and dried at 373K for 6h, and then calcined at 823K for 16h to obtain TS-2 molecular sieve. Among them, the amount of TEOS used is 42g, the amount of TBAOH used is 52g, the amount of Ti(OBu)4 used is 2g, the amount of anhydrous isopropanol used is 10g, and the amount of water used is 30g.

[0102] Preparation Example 6 Preparation of Ti-Beta Molecular Sieve

[0103] A certain amount of tetraethyl orthosilicate (TEOS) is added to a solution of tetraethylammonium hydroxide solution (TEAOH, 20%) and hydrogen peroxide, and hydrolyzed for 2 hours under stirring. Then, a weighed anhydrous isopropanol solution of tetrabutyl titanate [Ti(OBu)4] is added to the hydrolyzed solution of tetrabutyl titanate, and stirring is continued for 3 hours to remove alcohol, and finally a sol with a chemical composition of TiO2: 60SiO2: 33TEA: 400H2O: 20H2O2 is obtained. Finally, the P-type molecular sieve seed after dealuminization is added and stirred vigorously (the amount of seed added is based on silicon dioxide in the sol, and 4g seed is added to 100g silicon dioxide). After the obtained mixture is crystallized at 413K for 14 days, the obtained slurry is filtered, washed with water, and dried at 373K for 6 hours, and then calcined at 823K for 12 hours to obtain Ti-Beta molecular sieve. Among them, the amount of TEOS used is 42g, the amount of TEAOH used is 81g, the amount of Ti(OBu)4 used is 1.16g, the amount of anhydrous isopropanol used is 10g, and the amount of hydrogen peroxide used is 7.5g.

[0104] Preparation Example 7

[0105] This preparation example is used to illustrate the preparation process of S-1 molecular sieve.

[0106] Tetrapropylammonium hydroxide (TPAOH, 20%, purchased from Aldrich, USA) solution was added to tetraethyl orthosilicate (TEOS) solution to obtain a liquid mixture with a pH of about 13, and stirred at 348-353K for about 3 hours to obtain a sol with a chemical composition of SiO2:0.36TPA:35H2O, and then crystallized at 443K for 3 days, after which the obtained solid was filtered, washed with distilled water, dried at 373K for 5 hours, and then calcined at 823K for 10 hours to obtain S-1 molecular sieve. Among them, the amount of TEOS used was 42g, the amount of TPAOH used was 73g, and the amount of water used was 68g.

[0107] Test Example 1

[0108] The molar ratios of titanium to silicon and tin to silicon of the molecular sieves prepared in Preparation Examples 1-7 were tested, and the results are shown in Table 1.

[0109] Table 1

[0110]

[0111]

[0112] Examples 1-12 and Comparative Examples 1-7 are used to illustrate the preparation process of the catalyst.

[0113] Example 1

[0114] TS-1 molecular sieve and Sn-MFI molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the TS-1 molecular sieve and the Sn-MFI molecular sieve is 1:0.5, the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the total amount of the TS-1 molecular sieve and the Sn-MFI molecular sieve, and then sodium hydroxide solution is added to adjust the pH value of the obtained mixture to 7.7 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 200°C for 2h to obtain a catalyst.

[0115] Example 2

[0116] TS-1 molecular sieve and Sn-Beta molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the TS-1 molecular sieve and the Sn-Beta molecular sieve is 1:0.5, the concentration of the chloroauric acid aqueous solution is 0.05 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the total amount of the TS-1 molecular sieve and the Sn-Beta molecular sieve, and then potassium hydroxide solution is added to adjust the pH value of the obtained mixture to 8.1 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 150°C for 3h to obtain a catalyst.

[0117] Example 3

[0118] TS-1 molecular sieve and Sn-USY molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the TS-1 molecular sieve and the Sn-USY molecular sieve is 1:0.5, the concentration of the chloroauric acid aqueous solution is 0.08 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the total amount of the TS-1 molecular sieve and the Sn-USY molecular sieve, and then a cesium hydroxide solution is added to adjust the pH value of the obtained mixture to 8.0 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 120°C for 4 hours to obtain a catalyst.

[0119] Example 4

[0120] TS-2 molecular sieve and Sn-MFI molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the TS-2 molecular sieve and the Sn-MFI molecular sieve is 1:0.5, the concentration of the chloroauric acid aqueous solution is 0.005 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the total amount of the TS-2 molecular sieve and the Sn-MFI molecular sieve, and then urea solution is added to adjust the pH value of the obtained mixture to 7.6 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 220°C for 1.5 hours to obtain a catalyst.

[0121] Example 5

[0122] Ti-Beta molecular sieve and Sn-MFI molecular sieve are mechanically mixed, and then a chloroauric acid aqueous solution is added and mixed to obtain a mixture, wherein the weight ratio of the Ti-Beta molecular sieve and the Sn-MFI molecular sieve is 1:0.5, the concentration of the chloroauric acid aqueous solution is 0.008 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the total amount of the Ti-Beta molecular sieve and the Sn-MFI molecular sieve, and then a sodium carbonate solution is added to adjust the pH value of the obtained mixture to 7.4 to obtain a second suspension; then the second suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 250°C for 1h to obtain a catalyst.

[0123] Example 6

[0124] TS-1 molecular sieve and Sn-MFI molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the TS-1 molecular sieve and the Sn-MFI molecular sieve is 1:0.2, the concentration of the chloroauric acid aqueous solution is 0.01 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the total amount of the TS-1 molecular sieve and the Sn-MFI molecular sieve, and then sodium bicarbonate solution is added to adjust the pH value of the obtained mixture to 7.5 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 200°C for 2.5 hours to obtain a catalyst.

[0125] Example 7

[0126] TS-1 molecular sieve and Sn-MFI molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the TS-1 molecular sieve and the Sn-MFI molecular sieve is 1:1, the concentration of the chloroauric acid aqueous solution is 0.09 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the total amount of the TS-1 molecular sieve and the Sn-MFI molecular sieve, and then potassium bicarbonate solution is added to adjust the pH value of the obtained mixture to 8.1 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 180°C for 2h to obtain a catalyst.

[0127] Example 8

[0128] TS-1 molecular sieve and Sn-MFI molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the TS-1 molecular sieve and the Sn-MFI molecular sieve is 1:0.05, the concentration of the chloroauric acid aqueous solution is 0.0008 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the total amount of the TS-1 molecular sieve and the Sn-MFI molecular sieve, and then a cesium carbonate solution is added to adjust the pH value of the obtained mixture to 7.9 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 200°C for 2h to obtain a catalyst.

[0129] Example 9

[0130] TS-1 molecular sieve and Sn-MFI molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the TS-1 molecular sieve and the Sn-MFI molecular sieve is 1:2, the concentration of the chloroauric acid aqueous solution is 0.002 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the total amount of the TS-1 molecular sieve and the Sn-MFI molecular sieve, and then a cesium bicarbonate solution is added to adjust the pH value of the obtained mixture to 8.3 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 200°C for 2h to obtain a catalyst.

[0131] Example 10

[0132] The method of Example 1 was followed, except that the amount of the chloroauric acid aqueous solution used, calculated as Au element, was 0.05 wt % of the total amount of the TS-1 molecular sieve and the Sn-MFI molecular sieve.

[0133] Embodiment 11

[0134] The method of Example 1 was followed, except that the amount of the chloroauric acid aqueous solution used, calculated as Au element, was 5 wt % of the total amount of the TS-1 molecular sieve and the Sn-MFI molecular sieve.

[0135] Example 12

[0136] The method of Example 1 was followed, except that potassium carbonate solution was added to adjust the pH value of the resulting mixture.

[0137] Comparative Example 1

[0138] The TS-1 molecular sieve and the S-1 molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the TS-1 molecular sieve and the S-1 molecular sieve is 1:1, the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the total amount of the TS-1 molecular sieve and the S-1 molecular sieve, and then sodium hydroxide solution is added to adjust the pH value of the obtained mixture to 7.7 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 200°C for 2h to obtain a catalyst.

[0139] Comparative Example 2

[0140] Add TS-1 molecular sieve to chloroauric acid aqueous solution and mix them to obtain a mixture, wherein the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the amount of TS-1 molecular sieve, and then add sodium hydroxide solution to adjust the pH value of the obtained mixture to 7.7 to obtain a suspension; then filter the suspension, and activate the obtained filter residue, and the activation conditions include: air atmosphere, roasting at 200°C for 2h to obtain a catalyst.

[0141] Comparative Example 3

[0142] The S-1 molecular sieve and the Sn-MFI molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the S-1 molecular sieve and the Sn-MFI molecular sieve is 1:1, the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the total amount of the TS-1 molecular sieve and the Sn-MFI molecular sieve, and then sodium hydroxide solution is added to adjust the pH value of the obtained mixture to 7.7 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 200°C for 2h to obtain a catalyst.

[0143] Comparative Example 4

[0144] Sn-MFI molecular sieve is added to a chloroauric acid aqueous solution and mixed to obtain a mixture, wherein the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the amount of the Sn-MFI molecular sieve, and then sodium hydroxide solution is added to adjust the pH value of the obtained mixture to 7.7 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 200°C for 2h to obtain a catalyst.

[0145] Comparative Example 5

[0146] TS-1 molecular sieve and Sn-MFI molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the TS-1 molecular sieve and the Sn-MFI molecular sieve is 1:0.5, the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 6 weight % of the total amount of the TS-1 molecular sieve and the Sn-MFI molecular sieve, and then sodium hydroxide solution is added to adjust the pH value of the obtained mixture to 7.7 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 200°C for 2h to obtain a catalyst.

[0147] Comparative Example 6

[0148] TS-1 molecular sieve and Sn-MFI molecular sieve are mechanically mixed and then added into a chloroauric acid aqueous solution for mixing to obtain a mixture, wherein the weight ratio of the TS-1 molecular sieve and the Sn-MFI molecular sieve is 1:0.5, the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 0.005 weight % of the total amount of the TS-1 molecular sieve and the Sn-MFI molecular sieve, and then sodium hydroxide solution is added to adjust the pH value of the obtained mixture to 7.7 to obtain a suspension; then the suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 200°C for 2h to obtain a catalyst.

[0149] Test Example 2

[0150] The content of Au element in the catalysts prepared in Examples 1-12 and Comparative Examples 1-6 was tested, and the results are shown in Table 2. The test method is: according to the ASTM D5185 standard method, using SPECTRO ACROSS inductively coupled plasma (ICP) for determination.

[0151] XPS was used to detect the characteristic peak positions of Au elements in the catalysts prepared in Examples 1-12 and Comparative Examples 1-6, and the proportion of zero-valent Au was calculated. The results are shown in Table 2. The XPS spectra of the catalysts prepared in Example 1 and Comparative Example 5 are shown in Table 2. Figure 1 shown.

[0152] The molar ratio of tin to silicon and the molar ratio of titanium to silicon in the catalysts prepared in Examples 1-12 and Comparative Examples 1-6 were analyzed and calculated using X-ray fluorescence spectroscopy. The results are shown in Table 2.

[0153] The particle sizes of the gold nanoparticles in the catalysts prepared in Examples 1-12 and Comparative Examples 1-6 were observed by high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM), and the results are shown in Table 2. High-angle annular dark field scanning transmission electron microscopy photos of the catalysts prepared in Example 1 and Comparative Example 5 are shown in Table 2. Figure 2 and Figure 3 shown.

[0154] Table 2

[0155]

[0156]

[0157] Test Example 3

[0158] This test example is used to illustrate the reaction effect of the catalysts prepared in Examples 1-12 and Comparative Examples 1-6 of the present invention for the gas-phase epoxidation of propylene. The reagents used in this test example are all commercially available chemically pure reagents. The concentration of each substance after the reaction is quantitatively analyzed using gas chromatography. The instruments used are a 6890 gas chromatograph produced by Agilent, molecular sieve 5A and PoraBOND U chromatographic columns, and FID and TCD detectors.

[0159] In each embodiment and comparative example:

[0160] Propylene conversion % = (the number of moles of propylene in the feedstock - the number of moles of propylene in the product) / the number of moles of propylene in the feedstock × 100%;

[0161] Propylene oxide selectivity % = number of moles of propylene oxide in the product / total number of moles of the product × 100%.

[0162] The test process is as follows: the catalyst samples prepared in the above-mentioned embodiment and comparative example are taken respectively, loaded into a tubular reactor with an inner diameter of 8 mm, and then heated to 180°C in a N2 atmosphere, and hydrogen, oxygen, and propylene are introduced to start the reaction. After the reaction for 1 hour, the product is analyzed online; wherein, the amount of catalyst is 0.4 g, the flow rates of hydrogen, oxygen, propylene and nitrogen are 2 mL / min, 2 mL / min, 2 mL / min and 14 mL / min, respectively, the reaction pressure is 0.1 MPa, and the catalytic reaction results are shown in Table 3.

[0163] Table 3

[0164] serial number Propylene conversion rate / % Propylene oxide selectivity / % Example 1 10.5 90.2 Example 2 10.6 91.4 Example 3 10.8 90.7 Example 4 11.1 91.1 Example 5 9.9 90.1 Example 6 9.5 94.5 Example 7 15.7 90.1 Example 8 9.2 93.8 Example 9 15.1 89.4 Example 10 8.3 92.5 Embodiment 11 14.3 86.8 Example 12 11.1 91.2 Comparative Example 1 5.6 78.5 Comparative Example 2 6.0 77.9 Comparative Example 3 3.1 65.2 Comparative Example 4 3.3 67.1 Comparative Example 5 7.2 50.5 Comparative Example 6 2.1 86.7

[0165] As can be seen from Table 3, the propylene conversion rate of the catalyst provided in the embodiment of the present invention for the propylene gas-phase epoxidation reaction is significantly higher than that of the comparative example, and the propylene oxide selectivity of the catalyst provided in the embodiment of the present invention for the propylene gas-phase epoxidation reaction is also maintained at a high level.

[0166] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A hybrid molecular sieve loaded with gold nanoparticle catalyst, It is characterized in that The catalyst comprises a carrier and gold nanoparticles loaded on the carrier, wherein the carrier is a mixed carrier containing titanium silicon molecular sieve and tin silicon molecular sieve; Wherein, based on the total weight of the catalyst, the content of the gold nanoparticles is 0.01-1% by weight, preferably 0.04-0.8% by weight; wherein, calculated as Au element, the proportion of zero-valent Au in the gold nanoparticles is greater than 85%; wherein, in the catalyst, the molar ratio of titanium to silicon is 0.005-0.04:1, and the molar ratio of tin to silicon is 0.005-0.04:

1.

2. The catalyst according to claim 1, It is characterized in that In the catalyst, the particle size of the gold nanoparticles is less than 5 nm, preferably less than 3 nm.

3. The catalyst according to claim 1 or 2, It is characterized in that The titanium silicon molecular sieve is one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve; Preferably, the tin-silicon molecular sieve is one or more of Sn-MFI molecular sieve, Sn-USY molecular sieve, Sn-Beta molecular sieve and Sn-MEL molecular sieve.

4. A method for preparing a hybrid molecular sieve loaded with gold nanoparticle catalyst, It is characterized in that The method comprises the following steps: S1, mixing titanium silicon molecular sieve, tin silicon molecular sieve and a gold-containing compound aqueous solution, and then adjusting the pH value of the resulting mixture to alkaline, wherein the amount of the gold-containing compound aqueous solution calculated as Au element is 0.05-5% by weight of the total amount of the titanium silicon molecular sieve and the tin silicon molecular sieve; S2, performing solid-liquid separation on the product obtained in step S1, and activating the obtained solid product.

5. The method according to claim 4, It is characterized in that In step S1, the weight ratio of the titanium silicon molecular sieve to the tin silicon molecular sieve is 1:0.01-5.

6. The method according to claim 4 or 5, It is characterized in that In step S1, the titanium-silicon molecular sieve has a titanium-silicon molar ratio of 0.005-0.04:1; Preferably, in step S1, the molar ratio of tin to silicon in the tin-silicon molecular sieve is 0.005-0.04:

1.

7. The method according to any one of claims 4 to 6, It is characterized in that In step S1, the titanium silicon molecular sieve is selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve; Preferably, in step S1, the tin-silicon molecular sieve is selected from one or more of Sn-MFI molecular sieve, Sn-USY molecular sieve, Sn-Beta molecular sieve and Sn-MEL molecular sieve.

8. The method according to any one of claims 4 to 7, It is characterized in that In step S1, the gold compound aqueous solution is selected from one or more of an aqueous solution of chloroauric acid, an aqueous solution of cesium chloroaurate and an aqueous solution of potassium chloroaurate.

9. The method according to any one of claims 4 to 8, It is characterized in that In step S1, the concentration of the gold compound aqueous solution is 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, and more preferably 0.005-0.05 mol / L.

10. The method according to any one of claims 4 to 9, It is characterized in that In step S1, the amount of the gold-containing compound aqueous solution calculated as Au element is 0.1-5 weight % of the total amount of the titanium silicon molecular sieve and the tin silicon molecular sieve.

11. The method according to any one of claims 4 to 10, It is characterized in that In step S1, the pH value of the mixture is adjusted to 7-10, preferably 7-9.

12. The method according to any one of claims 4 to 11, It is characterized in that In step S1, the pH adjusting agent used to adjust the pH value of the mixture is an alkaline solution; Preferably, the alkaline solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, cesium hydroxide solution, urea solution, sodium carbonate solution, sodium bicarbonate solution, potassium carbonate solution, potassium bicarbonate solution, cesium carbonate solution and cesium bicarbonate solution.

13. The method according to any one of claims 4 to 12, It is characterized in that In step S2, the activation conditions include: temperature of 150-300°C and time of 1-5h.

14. A hybrid molecular sieve-supported gold nanoparticle catalyst prepared by the method described in any one of claims 4 to 13.

15. A method for gas phase epoxidation of propylene, It is characterized in that The method comprises: mixing hydrogen, oxygen and propylene for reaction in the presence of protective gas and catalyst to obtain propylene oxide; The catalyst is the hybrid molecular sieve-supported gold nanoparticle catalyst according to any one of claims 1 to 3 or the hybrid molecular sieve-supported gold nanoparticle catalyst according to claim 14.

16. The method according to claim 15, It is characterized in that The reaction conditions include: the volume flow ratio of hydrogen, oxygen and propylene is 0.5-2:0.5-2:1; Preferably, the volume flow rate ratio of propylene to protective gas is 1:1-10.

17. The method according to claim 15 or 16, It is characterized in that The reaction conditions include: temperature of 100-250°C and pressure of 0.1-0.7MPa; Preferably, the reaction conditions include: temperature of 120-220° C. and pressure of 0.1-0.5 MPa.

Citation Information

Patent Citations

  • Catalyst for direct epoxidation of propylene in presence of hydrogen gas and oxygen gas and preparation method

    CN101804360A

  • Tin-titanium-silicon molecular sieve and preparation method and application thereof, and method for hydroxylation of phenol

    CN105217645A

  • Tin-titanium-silicon molecular sieve as well as preparation method and application thereof, and thioether oxidation method

    CN110642263A

  • Tin-titanium-silicon molecular sieve as well as preparation method and application thereof

    CN114105158A

  • Preparation method and application of Au-TS-1 nano-microsphere catalyst for propylene gas-phase epoxidation

    CN115845916A