Method for strengthening flotation separation of micro-fine particle rare earth ore
By using a combination of water glass, hydroxamic acid collectors and synergists in the flotation process of rare earth ores, the problems of high energy consumption and poor selective collection ability in the flotation of fine-grained rare earth ores are solved, achieving Efficient, low-cost rare earth mineral recovery and process simplification.
Patent Information
- Application Number
- CN202411238097.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-10-15
AI Technical Summary
The flotation method of fine-grained rare earth ores in the existing technology has problems such as high energy consumption for grinding and high-temperature flotation, complex process operations, and poor selective capture ability of rare earth minerals, which limits the efficient recovery and utilization of rare earth resources.
Water glass is used as an inhibitor, hydroxamic acid compounds are used as collectors, and fatty alcohols, kerosene and polyoxyethylene ethers are used as synergists. Through the processes of grinding, roughing, selection and sweeping, fine particles are achieved. Efficient flotation separation of rare earth ores, reducing temperature and improving collection capacity.
It improves the flotation recovery rate of fine-grained light rare earth minerals, reduces process energy consumption, simplifies the process, reduces chemical consumption, achieves efficient recovery of rare earth minerals, and improves the hydrophobicity difference between target minerals and gangue minerals.
Smart Images

Figure CN118768091A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ore dressing, and in particular relates to a method for strengthening the flotation separation of fine-grained rare earth ores. Background Art
[0002] Rare earths are known as "industrial vitamins" and are extremely important strategic metal resources in the national economy. However, the mineral composition of rare earth ores is complex, and the two main rare earth minerals, bastnaesite and monazite, have similar surface chemical properties to gangue minerals such as fluorite, calcite, and apatite, and their co-existence relationship is complex, resulting in poor flotation separation effects. At the same time, rare earth minerals are fine in size, and fine grinding is required to obtain an ideal monomer dissociation degree. During the flotation process, rare earth minerals are severely lost due to fine grinding and mudification. Therefore, the flotation of fine-grained light rare earth ores is a major technical problem that restricts the efficient recycling of rare earth resources.
[0003] In the prior art, the flotation method of fine rare earth ores includes: (1) The flotation of rare earth ores is carried out by using staged grinding and step grinding and selection processes. This method can reduce over-grinding while ensuring that rare earth minerals reach a high degree of dissociation. It can also effectively improve the collection capacity of hydroxamic acid collectors under high temperature conditions of about 70°C, ultimately achieving a double increase in the grade and recovery rate of rare earth flotation concentrates. However, this method has the problems of high energy consumption for grinding and high-temperature flotation and complex process operation.
[0004] (2) Use flocculants to make fine particles form flocs, increase the apparent diameter of the particles, and reduce the loss of fine particles due to mudification; use fatty acid collectors with strong collection capacity and hydroxamic acid collectors to improve the collection capacity of rare earth minerals. However, the above two methods have the problem of poor selective collection capacity for rare earth minerals, resulting in high floating amount of gangue minerals and low grade of flotation rare earth concentrate.
[0005] Therefore, how to provide a new solution with low cost, simple process and the ability to improve the flotation index of fine rare earth ores is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0006] In order to solve the above technical problems, the present invention proposes a method for strengthening the flotation separation of fine-grained rare earth ores.
[0007] To achieve the above object, the present invention provides the following technical solutions: A method for strengthening the flotation separation of fine rare earth ores comprises grinding, roughing, cleaning and scavenging, using water glass as an inhibitor, hydroxamic acid compounds as collectors, and one or more of fatty alcohols, kerosene and polyoxyethylene ether as synergists to perform flotation separation on ore pulp with a rare earth mineral monomer dissociation degree greater than 80%.
[0008] Preferably, the hydroxamic acid compound is one or any combination of C5-C9 hydroxamic acid, benzohydroxamic acid, naphthohydroxamic acid and salicylic hydroxamic acid; More preferably, the collector is obtained by mixing the following raw materials in percentage by mass: Octylhydroxamic acid 50%~60%, naphthyhydroxamic acid 20%~30% and salicylic hydroxamic acid 10%~30%.
[0009] More preferably, the synergist is obtained by mixing the following raw materials in percentage by mass: Fatty alcohol 10%~30%, kerosene 0~5% and polyoxyethylene ether 65%~90%.
[0010] Preferably, the polyoxyethylene ether is octylphenol polyoxyethylene ether.
[0011] Beneficial effects: The synergist used in the present invention improves the dissolution effect and collection capacity of the hydroxamic acid collector at a lower temperature. The hydroxamic acid collector and the synergist in the present invention are synergistically adsorbed on the surface of the light rare earth mineral through the hydrophobic association of the hydrophobic chain, so that the light rare earth mineral selectively hydrophobically flocculates into particles with a larger apparent diameter, improves the flotation recovery rate of fine light rare earth minerals, increases the hydrophobicity difference between the target mineral and the gangue mineral, and realizes the efficient recovery of fine rare earth minerals.
[0012] Preferably, the temperatures for roughing, cleaning and scavenging are all 50-60°C.
[0013] Beneficial effects: Conventional flotation often requires a temperature of 65°C or above to achieve flotation separation of rare earth ores, while the present invention changes the reagents used in the conventional method so that the flotation of rare earth ores can be completed at 50-60°C, thereby reducing process energy consumption and greatly saving flotation costs.
[0014] Preferably, the roughing is as follows: after adjusting the pulp concentration to 50% to 60%, a depressant, a collector and a synergist are added in sequence, and then aeration flotation is performed to obtain a roughing concentrate and a roughing tailing.
[0015] More preferably, during the rough selection process, the inhibitor is added and stirred for 2-3 minutes, the collector is then added and stirred for 0.5-1 minute, and finally the synergist is added and stirred for 2-3 minutes.
[0016] During the roughing process, the time of aeration flotation is 3-4 minutes.
[0017] Preferably, in the roughing process, based on the total mass of the original ore, the amount of the inhibitor added is 800g / t~1500g / t, the amount of the collector added is 1000g / t~1500g / t, and the amount of the synergist added is 300g / t~450g / t.
[0018] Preferably, the selection includes primary selection and secondary selection, and specifically includes the following steps: The concentration of the rougher concentrate is adjusted to 35%~45%, and then a depressant is added for aeration flotation to complete the first concentration to obtain the concentrated 1 concentrate and the concentrated 1 middling; The concentration of the selected 1 concentrate is adjusted to 25% to 35%, and blank flotation is performed without adding reagents to complete secondary concentration to obtain selected 2 concentrate and selected 2 middlings.
[0019] More preferably, in the process of the primary concentration, the depressant is added and stirred for 2-3 minutes, and the time of aeration flotation is 3-4 minutes.
[0020] During the secondary concentration process, the time of aeration flotation is 2-3 minutes.
[0021] Preferably, during the primary concentration process, the amount of the inhibitor added is 400-800 g / t based on the total mass of the ore in the roughing concentrate.
[0022] Preferably, the scavenging is as follows: the roughing tailings are ground to a particle size of 90% to 95% of 325 mesh, and after obtaining the reground slurry, an inhibitor, a collector and a synergist are sequentially added, and then aeration flotation is performed to obtain scavenging concentrate and scavenging tailings.
[0023] More preferably, during the scanning process, the inhibitor is added and stirred for 2-3 minutes, the collector is then added and stirred for 0.5-1 minute, and finally the synergist is added and stirred for 2-3 minutes.
[0024] During the sweeping process, the time of aeration flotation is 3-4 minutes.
[0025] Preferably, during the scavenging process, the amount of the inhibitor added is 800 g / t to 1200 g / t based on the total mass of the ore to be reground; The addition amount of the collector is 800g / t~1200g / t; The addition amount of the synergist is 250g / t~350g / t.
[0026] Preferably, the intermediate ore of the concentration 1 and the scavenging concentrate are returned as feed for roughing, and the intermediate ore of the concentration 2 is returned as feed for primary concentration.
[0027] Compared with the prior art, the present invention has the following advantages and technical effects: The present invention uses water glass as an inhibitor, hydroxamic acid compounds as collectors, and one or more of fatty alcohols, kerosene and polyoxyethylene ethers as synergists to conduct a "one coarse and two fine - coarse tail sweeping" flotation separation test of light rare earth ore. The flotation recovery rate of fine light rare earth minerals can be improved, the hydrophobicity difference between target minerals and gangue minerals is increased, and efficient recovery of fine rare earth ore is achieved. The method provided by the present invention has low reagent consumption, simple process flow and reagent system, and is easy to control. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings: Figure 1 It is a schematic diagram of the flotation separation process of light rare earth ore of the present invention. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources; Among them, the REO grade of the iron tailings used as the original ore by a rare earth concentrator in Baotou is 9.58%; The REO grade of rare earth in a tailings pond in Inner Mongolia is 8.47%;
[0032] Example 1 A method for enhancing the flotation separation of fine rare earth ores comprises the following steps: (1) The iron tailings from a rare earth ore dressing plant in Baotou were used as the raw ore. The tailings were finely ground to a particle size of 85% at a grinding concentration of 67% to a particle size of ~325 mesh. The tailings were then placed in a flotation tank and diluted with water to a pulp mass concentration of 55%.
[0033] (2) The slurry was heated to 50°C, and 1000 g / t of water glass was added based on the total mass of the original ore. The mixture was stirred for 2 minutes, and then 1300 g / t of a collector (50% octylhydroxamic acid, 30% naphthohydroxamic acid, and 20% salicylic hydroxamic acid) was added. The mixture was stirred for 0.5 minutes. Finally, 400 g / t of a synergist (10% fatty alcohol and 90% octylphenol polyoxyethylene ether) was added. The mixture was stirred for 2 minutes, and then aerated flotation was performed for 4 minutes to obtain a rougher concentrate and a rougher tailings.
[0034] (3) The concentration of the rougher concentrate is adjusted to 40%. Based on the total mass of the ore of the rougher concentrate, 800 g / t of depressant water glass is added to the rougher concentrate obtained in step (2), and the mixture is stirred for 2 minutes and aerated flotation is performed for 4 minutes to obtain a concentrated 1 concentrate and a concentrated 1 middling. The concentration of the concentrated 1 concentrate is adjusted to 30%. The concentrated 1 concentrate is subjected to blank flotation without adding reagents to obtain a concentrated 2 concentrate and a concentrated 2 middling.
[0035] (4) The rougher tailings obtained in step (2) are finely ground to a mass concentration of 90% to 95% of ~325 mesh particles to obtain a reground slurry, and then 800 g / t of water glass as an inhibitor is added based on the total mass of the reground ore, stirred for 2 minutes, and then 1000 g / t of a collector is added, stirred for 0.5 minutes, and finally 300 g / t of a synergist is added. After stirring for 2 minutes, aeration flotation is performed for 4 minutes to obtain a scavenged concentrate and scavenged tailings.
[0036] (5) The intermediate ore of Concentrated 1 obtained in step (3) is returned as feed for roughing, the intermediate ore of Concentrated 2 is returned as concentrate for Concentrated 1, the scavenging concentrate obtained in step (4) is returned as feed for roughing, and the above steps (3) to (5) are repeated.
[0037] Comparative Example 1 A method for flotation separation of rare earth ores, which differs from Example 1 only in that: In step (2), the ore pulp is heated to 65° C., and 1000 g / t of water glass, 1500 g / t of collector, and 75 g / t of frother pine oil are added in sequence based on the total mass of the original ore. In step (3), based on the total mass of the rough concentrate ore, 800 g / t of water glass, 1250 g / t of collector, and 45 g / t of frother pine oil were added in sequence; In step (4), based on the total mass of the reground ore, 1000 g / t of water glass, 1300 g / t of collector, and 75 g / t of frother pine oil were added in sequence.
[0038] The test results of the above two schemes are shown in Table 1. It can be seen from the test results that the reagent system of the scheme of the present invention achieves better rare earth flotation indicators than the conventional reagent system, and the flotation temperature is lower and the reagent consumption is less.
[0039] Table 1 Rare earth ore flotation results (%)
[0040] Example 2 A method for enhancing the flotation separation of fine rare earth ores comprises the following steps: (1) The rare earth samples from a tailings pond in Inner Mongolia were used as the raw ore. The raw ore was finely ground to a particle size of 325 mesh at a grinding concentration of 67%, accounting for 85% of the total particle size. The raw ore was then placed in a flotation tank and diluted with water to a pulp mass concentration of 50%.
[0041] (2) The slurry was heated to 55°C, and 1000 g / t of water glass was added based on the total mass of the original ore. The mixture was stirred for 2 minutes, and then 1200 g / t of a collector (50% octylhydroxamic acid, 30% naphthohydroxamic acid, 20% salicylic hydroxamic acid) was added. The mixture was stirred for 0.5 minutes. Finally, 350 g / t of a synergist (20% fatty alcohol, 2% kerosene, 78% octylphenol polyoxyethylene ether) was added. The mixture was stirred for 2 minutes, and then aerated flotation was performed for 4 minutes to obtain a rougher concentrate and a rougher tailings.
[0042] (3) The concentration of the rougher concentrate is adjusted to 40%. Based on the total mass of the ore of the rougher concentrate, 1000 g / t of depressant water glass is added to the rougher concentrate obtained in step (2), and the mixture is stirred for 2 minutes and aerated flotation is performed for 4 minutes to obtain a concentrated 1 concentrate and a concentrated 1 middling. The concentration of the concentrated 1 concentrate is adjusted to 30%. The concentrated 1 concentrate is subjected to blank flotation without adding reagents to obtain a concentrated 2 concentrate and a concentrated 2 middling.
[0043] (4) The rougher tailings obtained in step (2) are finely ground to a mass concentration of 90% to 95% of ~325 mesh particles to obtain a reground slurry, and then 800 g / t of water glass as an inhibitor is added based on the total mass of the reground ore, stirred for 2 minutes, and then 1000 g / t of a collector is added, stirred for 0.5 minutes, and finally 300 g / t of a synergist is added. After stirring for 2 minutes, aeration flotation is performed for 4 minutes to obtain a scavenged concentrate and scavenged tailings.
[0044] (5) The intermediate ore of Concentrated 1 obtained in step (3) is returned as feed for roughing, the intermediate ore of Concentrated 2 is returned as concentrate for Concentrated 1, the scavenging concentrate obtained in step (4) is returned as feed for roughing, and the above steps (3) to (5) are repeated.
[0045] Comparative Example 2 A method for flotation separation of rare earth ores, which differs from Example 2 only in that: In step (2), the ore pulp is heated to 65°C, and 1360 g / t of water glass, 1450 g / t of collector, and 75 g / t of frother pine oil are added in sequence based on the total mass of the original ore; In step (3), based on the total mass of the rough concentrate ore, 800 g / t of water glass, 1000 g / t of collector, and 45 g / t of frother pine oil are added in sequence; In step (4), based on the total mass of the reground ore, 800 g / t of water glass, 1000 g / t of collector, and 75 g / t of frother pine oil are added in sequence.
[0046] The test results of the above two schemes are shown in Table 2. It can be seen from the test results that the reagent system of the scheme of the present invention achieves better rare earth flotation indicators than the conventional reagent system, and the flotation temperature is lower and the reagent consumption is less.
[0047] Table 2 Rare earth ore flotation results (%)
[0048] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for strengthening the flotation separation of fine rare earth ores, comprising: Grinding, roughing, cleaning and scavenging, characterized in that water glass is used as an inhibitor, hydroxamic acid compounds are used as collectors, and one or more of fatty alcohols, kerosene and polyoxyethylene ethers are used as synergists to flotation separate the pulp with a rare earth mineral monomer dissociation degree greater than 80%; The temperatures for roughing, cleaning and sweeping are all 50-60°C; The roughing process comprises: adjusting the pulp concentration to 50% to 60%, sequentially adding a depressant, a collector and a synergist, and then aerating flotation to obtain a roughing concentrate and a roughing tailing; The selection includes primary selection and secondary selection, and specifically includes the following steps: The concentration of the rougher concentrate is adjusted to 35%~45%, and then a depressant is added for aeration flotation to complete the first concentration to obtain the concentrated 1 concentrate and the concentrated 1 middlings; The concentration of the selected 1 concentrate is adjusted to 25% to 35%, and blank flotation is performed without adding reagents to complete secondary concentration to obtain selected 2 concentrate and selected 2 middlings; The scavenging process comprises: grinding the roughing tailings to a particle size of 90% to 95% of 325 mesh, obtaining a reground pulp, sequentially adding a depressant, a collector and a synergist, and then performing aeration flotation to obtain a scavenging concentrate and scavenging tailings.
2. The method for enhancing the flotation separation of fine rare earth ores according to claim 1, characterized in that: The hydroxamic acid compound is one or any combination of C5-C9 hydroxamic acid, benzohydroxamic acid, naphthohydroxamic acid and salicylic hydroxamic acid.
3. The method for enhancing the flotation separation of fine rare earth ores according to claim 1, characterized in that: In the roughing process, based on the total mass of the original ore, the added amount of the inhibitor is 800g / t~1500g / t, the added amount of the collector is 1000g / t~1500g / t, and the added amount of the synergist is 300g / t~450g / t.
4. The method for enhancing the flotation separation of fine rare earth ores according to claim 1, characterized in that: During the primary concentration process, the amount of the inhibitor added is 500-1000 g / t based on the total mass of the ore in the roughing concentrate.
5. The method for enhancing the flotation separation of fine rare earth ores according to claim 1, characterized in that: During the scavenging process, the amount of the inhibitor added is 800 g / t to 1200 g / t based on the total mass of the ore to be reground; The addition amount of the collector is 800g / t~1200g / t; The addition amount of the synergist is 250g / t~350g / t.
Citation Information
Patent Citations
A floatation separation method of hamartite misch metal mine high containing mengite
CN101444761A
Method for flotation of rare earth from Baiyunebo tailings
CN102319631A
Rare earth ore beneficiation method
CN103962232A
Complex multi-metal rare earth ore beneficiation separation and enrichment method
CN111530620A
Flotation method for alkaline granite type rare earth ore
CN111530634A
Cited By
Composite collecting agent for rare earth ore and application of composite collecting agent in flotation
CN119259268A
A composite collector for rare earth minerals and its application in flotation
CN119259268B
Synergist for rare earth flotation collecting agent and method for carrying out rare earth flotation by utilizing synergist
CN119838761A