Application of O-allyl salicylic hydroxamic acid compound in metal ore flotation

By using O-allyl salicylic hydroxamic acid compounds as collectors, the problem of insufficient flotation and selectivity of metal minerals in the prior art is solved, and more efficient metal mineral enrichment and recovery is achieved. Have a commercially feasible preparation process.

CN115228618BActive Publication Date: 2024-11-26CENT SOUTH UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202110448641.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-25
Publication Date
2024-11-26
Estimated Expiration
2041-04-25

AI Technical Summary

Technical Problem

There is still room for improvement in the capture capacity and selectivity of existing hydroxamic acid collectors in metal mineral flotation.

Method used

O-allyl salicylic hydroxamic acid compounds are used as collectors and are prepared by substitution and hydroxamation reaction with salicylate, halopropylene and hydroxylamine to improve the flotation performance of metal minerals.

Benefits of technology

It improves the enrichment and recovery efficiency of valuable metal minerals, shows better capture and selectivity, and the preparation process is simple, economical and efficient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115228618B_ABST
    Figure CN115228618B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of mineral flotation, and specifically discloses an application of an O-allyl salicylic hydroxamic acid compound in the flotation of metal minerals. In the present invention, an O-allyl salicylic hydroxamic acid compound of the structure shown in formula (I) is used as a flotation collector to flotation and recover valuable metal minerals from rare earth, tin, tungsten, titanium, copper, iron and other ores. The collector described in the present invention, based on the intramolecular synergy of the structure and substituent, helps to improve the hydrophobicity of froth flotation, effectively strengthens the flotation enrichment and recovery of rare earth, tin, tungsten, titanium, copper, iron and other minerals, and improves the flotation recovery rate of valuable metal ores.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal ore dressing, and in particular to an O-allyl salicylic hydroxamic acid collector and application thereof in metal ore flotation. Background Art

[0002] The hydroxyl oxygen, oxime oxygen and nitrogen atoms of the hydroxamic acid molecule have abundant lone pair electrons and can react with Pb 2+ 、Co 2+ 、Ti 4+ and Sn 4+ The metal ions undergo chelation reaction to form a five-membered or four-membered ring. Therefore, hydroxamic acid compounds are widely used in the field of mineral flotation, especially in the flotation of rare earth ores, ilmenite, tungsten ore, tin ore, copper oxide ore, iron ore and other metal ores.

[0003] At present, benzohydroxamic acid and salicylic acid are the most commonly used chelating collectors for metal ore flotation. Dong Hongjun and Chen Zhengxue found that salicylic acid flotation of fine-grained ilmenite has the advantages of low dosage and high selectivity (Dong Hongjun, Chen Zhengxue. Research on the flotation of fine-grained ilmenite with salicylic acid, Mining and Metallurgical Engineering, 1991, 11 (1): 19-22). Wu et al. found that benzohydroxamic acid has good flotation selectivity for cassiterite (XQ Wu, JG Zhu. Selective flotation of cassiterite with benzohydroxamic acid. Minerals Engineering, 2006, 19 (14): 1410-1417). Sun Wei et al. studied the performance and mechanism of benzohydroxamic acid flotation of cassiterite (Sun Wei, Ke Lifang, Sun Lei. Application and mechanism of benzohydroxamic acid in cassiterite flotation, Journal of China University of Mining and Technology, 2013, 42(1): 62-68). Jordens et al. believed that benzohydroxamic acid is an efficient collector for flotation of rare earth minerals (Jordens A, Marion C, Grammatikopoulos T, et al. Beneficiation of the Nechalacho rare earth deposit: Flotation response using benzohydroxamic acid. Minerals Engineering, 2016, 99: 158-169). Patent CN112246441A discloses that a composite collector composed of a hydroxamic acid compound and an alcohol has good flotation performance for minerals such as ilmenite and cassiterite (Ma Xin, Zhong Hong, Cao Zhanfang, Wang Shuai. A flotation composite collector, its preparation method and application, CN112246441A, 2021.01.22).

[0004] Although, through the continuous efforts of scientific researchers, the performance of existing hydroxamic acid collectors has been greatly improved, there is still room for improvement in collection capacity and selectivity. Summary of the invention

[0005] The object of the present invention is to provide an application of O-allyl salicylic acid hydroxamic acid compounds in metal mineral flotation, wherein the O-allyl salicylic acid hydroxamic acid compounds can effectively improve the enrichment and recovery efficiency of valuable metal minerals.

[0006] The application of O-allyl salicylic hydroxamic acid compounds in metal ore flotation is to use them as collectors for the flotation of metal minerals.

[0007] The O-allyl salicylic hydroxamic acid compound is a compound having formula (I);

[0008]

[0009] Where R is H or C1-C 12 Alkyl; M is H + 、Na + or K + .

[0010] The study found that thanks to the synergy of the collector structure at the molecular level, the capture performance and capture selectivity of metal ores can be unexpectedly improved.

[0011] Preferably, the R is H or methyl.

[0012] The O-allyl salicylic acid hydroxamic acid compound can be prepared simply, economically and efficiently by a one-pot method using salicylic acid ester, halogenated propene and hydroxylamine as raw materials through substitution and hydroxylation reaction. Specifically, in a solvent, salicylic acid ester represented by formula (II) undergoes substitution reaction with halogenated propene (3-haloallyl propane) represented by formula (III) to obtain an O-allyl salicylic acid ester intermediate represented by formula (IV), and then the intermediate undergoes hydroxylation reaction with hydroxylamine to obtain an O-allyl salicylic acid hydroxamic acid compound represented by formula (I), and then the O-allyl salicylic acid hydroxamic acid collector is obtained by desolventizing.

[0013]

[0014]

[0015] Where R is H or C1~C 12 X represents Cl or Br; R' is a C1~C6 alkyl group.

[0016] In the present invention, the reaction solvent is preferably at least one of methanol, ethanol, propanol or isopropanol, preferably methanol. Further preferably, the reaction solvent is preferably recycled.

[0017] Preferably, the molar ratio of salicylic acid ester, propylene halide and hydroxylamine hydrochloride is 1:0.95-1.5:0.95-1.5.

[0018] Preferably, the substitution reaction temperature is 10° C. to 150° C., and the substitution reaction time is preferably 1 to 30 hours.

[0019] In the present invention, the intermediate, hydroxylamine and base (sodium or potassium hydroxide) are subjected to a hydroximation reaction to obtain a target product in which M is Na or K. In order to obtain a product in which M is H, the product of the hydroximation reaction (hydroxamate portion) can be subjected to a conventional acidification treatment.

[0020] Preferably, the hydroximation reaction temperature is 0° C. to 90° C., and the hydroximation reaction time is preferably 1 to 12 hours.

[0021] The metal mineral is preferably at least one of rare earth, tin, tungsten, titanium, copper, iron and the like ores.

[0022] In the present invention, the collector of formula (I) is applied to the flotation field to recover metal minerals in ores.

[0023] The application comprises the following steps:

[0024] Step (1): crushing and slurrying the metal ore to obtain slurry;

[0025] Step (2): adding a flotation agent to the ore pulp of step (1) for flotation, and collecting a flotation concentrate; the flotation agent comprises at least one O-allyl salicylic acid hydroxamic acid compound; the dosage of the O-allyl salicylic acid hydroxamic acid flotation collector is 2-2000 g / t based on the weight of the flotation feed ore.

[0026] Preferably, during the flotation process, the pH of the pulp is 4-10; more preferably 6-10; further preferably 7-8.

[0027] The present invention also provides a flotation agent for metal ore, comprising the O-allyl salicylic hydroxamic acid flotation collector.

[0028] Preferably, other components beneficial to flotation, such as frothers and other flotation components, are allowed to be added to the flotation reagent.

[0029] Beneficial Effects

[0030] (1) The present invention proposes a new use of O-allyl salicylic hydroxamic acid compounds as metal ore flotation collectors. The present invention has found that, thanks to the structure of the collector and the intramolecular synergy of the groups, it can show better capture and selectivity than other similar hydroxamic acid collectors. In the present invention, the introduction of allyl groups into salicylic hydroxamic acid to obtain O-allyl salicylic hydroxamic acid collectors helps to improve the hydrophobicity of froth flotation, effectively enhance the flotation enrichment and recovery of rare earth, tin, tungsten, titanium, copper, iron and other minerals, and improve the flotation recovery rate of valuable metal ores.

[0031] (2) The O-allyl salicylic acid hydroxamic acid compounds of the present invention can be prepared simply, economically and efficiently by a one-pot method using salicylic acid ester, halogenated propene and hydroxylamine as raw materials through substitution and hydroxylation reaction. Compared with halogenated alkanes such as halopropane, the halogen atom in the halogenated propene compound is connected to the allyl group, and the reaction activity is higher, and the O-allyl salicylic acid ester compound, which is the intermediate of the O-allyl salicylic acid hydroxamic acid compound, can be prepared efficiently. Therefore, the entire "one-pot method" preparation process is simple, the product yield is high, and the obtained product is used as a collector, and has excellent collection ability and selectivity; the technical solution is commercially feasible. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 O-allyl salicylic acid 1 H NMR spectra;

[0033] Figure 2 The flotation results of cassiterite in Application Example 1 are shown in FIG. 1 , wherein ■ is reagent 1 and ● is reagent 2;

[0034] Figure 3 This is a comparison of the flotation results of cassiterite, malachite and bastnaesite using reagent a and reagent b in Example 2, wherein the bar graph on the left is the flotation result graph of reagent a. DETAILED DESCRIPTION

[0035] The following examples are intended to further illustrate the present invention, but are not intended to limit the scope of the present invention. All parts and percentages in the examples are by weight unless otherwise specified. The flotation process of the minerals in the examples is a conventional process, except that the O-allyl salicylic acid hydroxamic acid compounds of the present invention are used to replace the conventional flotation collector.

[0036] Comparative Synthesis Example: Synthesis of O-allyl Salicylic Hydroxamic Acid

[0037] Potassium O-allyl salicylate was prepared according to the method reported by Pandey SK et al. (Pandey SK, Mishra M., Sharma A., et al. Syntheses of low molecular weight hydroxamates as potent antiprotozoal and antifungalagents. Chemistry & Biology Interface, 2012, 6 (2) 373-393). With tetrahydrofuran as solvent, methyl salicylate (1.0 g, 6.5 mmol) was reacted with allyl bromide (0.5 mL, 6.51 mmol) in the presence of potassium carbonate (0.92 g, 6.57 mmol) and tetrabutylammonium bromide (0.42 g, 1.31 mmol) to obtain colorless oily methyl O-allyl salicylate in a yield of 82% (1.02 g). Then, in methanol solvent, methyl O-allyl salicylate reacts with hydroxylamine hydrochloride (3.25 g, 46.8 mmol) and potassium hydroxide (5.25 g, 93.7 mmol) to obtain white potassium O-allyl salicylate hydroxamate solid with a yield of 75% (0.76 g). Based on methyl salicylate, the yield of potassium O-allyl salicylate hydroxamate is 62%.

[0038] Synthesis Example:

[0039] With methanol as solvent, in the presence of potassium carbonate (27.92g, 0.2mol) and potassium iodide (3.32g, 0.02mol, as catalyst), methyl salicylate (30.74g, 0.2mol) and propylene chloride (17.89g, 0.21mol) were refluxed for 12h to obtain colorless oily O-allyl salicylic acid methyl ester. Then, hydroxylamine hydrochloride (15.52g, 0.22mol) was added at below 20°C, and then sodium hydroxide (17.5g, 0.42mol) was added in batches. After stirring for 30min, the temperature was raised to 55°C, and the reaction was kept warm for 5h. The solvent was removed by reduced pressure distillation to obtain a yellow-white solid of sodium O-allyl salicylate hydroxamate. The yield was 95% based on methyl salicylate. The crude product of sodium O-allyl salicylate hydroxamate obtained can be directly used for metal ore flotation. Sodium O-allyl salicylic acid hydroxamate was purified by acidification, and its H NMR spectrum 1 H NMR Figure 1 .

[0040] Obviously, compared with the comparative synthesis example, the one-pot synthesis process used in the present invention is simple, efficient and economical, and is a preparation route with commercial value.

[0041] Application Example 1 Cassiterite flotation comparison test

[0042] Agent 1: O-allyl salicylic acid (concentration 3×10 -4 mol / L) + foaming agent methyl isobutyl carbinol (MIBC; concentration is 7×10 -4 mol / L);

[0043] Drug 2: Formula A ( The concentration is 3×10 -4 mol / L) + foaming agent methyl isobutyl carbinol (MIBC; concentration is 7×10 -4 mol / L);

[0044] Drug 3: Formula B ( The concentration is 3×10 -4 mol / L) + foaming agent methyl isobutyl carbinol (MIBC; concentration is 7×10 -4 mol / L);

[0045] 1 to 3 reagents were used for flotation. When the N2 flow rate was 300 mL / min, cassiterite with a particle size of 0.038 mm to 0.076 mm was flotated for 3 minutes at pH 4, 6, 8, and 10. The flotation results are shown in Table 1. Figure 2 . Figure 2 It shows that under the same conditions, the capture ability of O-allyl salicylic acid for cassiterite is stronger than that of formula A and formula B; at pH 8, O-allyl salicylic acid has a better flotation effect on cassiterite.

[0046] Application Example 2 Comparative flotation test of cassiterite, malachite and bastnaesite

[0047] Agent a: O-allyl salicylic acid (concentration 5×10 -4 mol / L) + foaming agent methyl isobutyl carbinol (MIBC; concentration is 7×10 -4 mol / L);

[0048] Agent b: Formula A ( The concentration is 5×10 -4 mol / L) + foaming agent methyl isobutyl carbinol (MIBC; concentration is 7×10 -4 mol / L);

[0049] Cassiterite, malachite and bastnaesite were flotated using reagents a and b. When the N2 gas flow rate was 300 mL / min and the pH was about 8.0, cassiterite, malachite and bastnaesite with a particle size of 0.038 mm to 0.076 mm were flotated for 3 minutes. The flotation results are shown in Table 1. Figure 3 . Figure 3 It shows that under the same conditions, the capture ability of O-allyl salicylic acid for cassiterite, malachite and bastnaesite is stronger than that of formula A.

[0050] Application Example 3: Flotation test of fine cassiterite in shaking table tailings

[0051] The cassiterite shaking table tailings in Yunnan contains SnO20.38%. The flotation process is a primary roughing process, in which the amount of sodium carbonate is 3000g / t, the pH is 8.0, the amount of collector (as shown in Table 1) is 600g / t, and tributyl phosphate is 8g / t. The flotation results are shown in Table 1.

[0052] Table 1 Comparison results of cassiterite shaking table tailings flotation

[0053]

[0054] As can be seen from Table 1, compared with Formula A and Formula B, O-allyl salicylic hydroxamic acid significantly improves the flotation recovery rate of SnO2 in cassiterite shaker tailings; in addition, the technical solution has advantages in terms of synthesis process, efficiency and economy, and has great practical application prospects.

Claims

1. An application of O-allyl salicylic hydroxamic acid compounds in metal ore flotation, characterized in that: As a collector, used for flotation of metal minerals; The O-allyl salicylic hydroxamic acid compound is a compound having formula (I); (I) Where R is H or C1~C 12 Alkyl; M is H + 、Na + or K + .

2. The use according to claim 1, characterized in that: The R is H or methyl.

3. The use according to claim 1, characterized in that: In a solvent, a salicylate represented by formula (II) undergoes a substitution reaction with a halogenated propylene represented by formula (III) to obtain an O-allyl salicylate intermediate represented by formula (IV), and then the intermediate undergoes a hydroxamination reaction with hydroxylamine to obtain an O-allyl salicylic hydroxamic acid compound collector represented by formula (I); (II) (III) (IV) Where R is H or C1~C 12 X represents Cl or Br; R' is a C1~C6 alkyl group.

4. The use according to claim 3, characterized in that: The reaction solvent is at least one of methanol, ethanol, propanol or isopropanol.

5. The use according to claim 4, characterized in that: The reaction solvent is recovered and recycled.

6. The use according to claim 3, characterized in that: The molar ratio of salicylic acid ester, propylene halide and hydroxylamine hydrochloride is 1: 0.95~1.5: 0.95~1.

5.

7. The use according to claim 3, characterized in that: The substitution reaction temperature is 10°C to 150°C, and the substitution reaction time is 1 to 30 hours.

8. The use according to claim 3, characterized in that: The hydroxyoximation reaction temperature is 0°C to 90°C, and the hydroxyoximation reaction time is 1 to 12 hours.

9. The use according to any one of claims 1 to 8, characterized in that: The metal ore is at least one of rare earth, tin, tungsten, titanium, copper and iron ore.

10. The use according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step (1): crushing and slurrying the metal ore to obtain slurry; Step (2): adding a flotation agent to the ore pulp of step (1) to carry out flotation, and collecting the flotation concentrate; the flotation agent comprises the O-allyl salicylic hydroxamic acid compound.

11. The use according to any one of claims 1 to 8, characterized in that: Taking the weight of the flotation feed ore as the calculation standard, the dosage of the O-allyl salicylic hydroxamic acid flotation collector is 2-2000 g / t.

12. A flotation reagent for metal ore, characterized in that: The invention comprises the O-allyl salicylic hydroxamic acid flotation collector described in any one of claims 1 to 11.

Citation Information

Patent Citations

  • Flotation composite collecting agent as well as preparation method and application thereof

    CN112246441A

  • 6-aliphatic hydrocarbon amido hexyl hydroximic acid collecting agent and preparation and application methods thereof

    CN103301952A

  • Nicotinyl hydroximic acid collecting agent and preparing method and application of nicotinyl hydroximic acid collecting agent

    CN107694763A

  • Application of allyl benzene hydroximic acid in ilmenite and bastnaesite flotation

    CN108499742A

  • Decyl salicylhydroxamic acid and application thereof

    CN108554643A