Production method of ultrahigh-strength 86-grade tire cord steel wire rod

By adopting molten iron pretreatment, BOF converter smelting, LF refining, billet continuous casting and controlled rolling and controlled cooling processes in the production of steel cords, the problems of central segregation and reticular cementite precipitation in grade 86 cord steel are solved. , realizing the production of high-purity and high-strength cord steel wire rods, reducing production costs and meeting the demand for ultra-high-strength steel cords.

CN118768384APending Publication Date: 2024-10-15ANSTEEL BEIJING RES INST CO LTD +2

Patent Information

Application Number
CN202410776812.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult to effectively produce high-strength grade 86 cord steel with existing technology, and there are problems with central segregation and reticular cementite precipitation, resulting in breakage of steel cords during processing. The production cost is high, and the existing method has limited C content control. The difficulty is high, which leads to an increase in inclusions in the molten steel and affects the quality of the cord steel.

Method used

Adopt molten iron pretreatment, BOF converter smelting, LF furnace refining, billet continuous casting, billet heating, controlled rolling and controlled cooling processes. By optimizing the smelting process and rolling conditions, the C content is controlled between 0.84% ​​and 0.88%, and the molten steel is reduced. Nitrogen content, reduce inclusions, adopt full protection casting and low superheat casting, control the heating and cooling process, and ensure the purity and strength of the cord steel.

Benefits of technology

It achieves high purity of cord steel wire rods, sorbite rate ≥95%, no large-level reticulated cementite, and tensile strength of 1120~1260MPa, which reduces production costs and meets the demand for ultra-high-strength steel cords. , improving the safety performance and production efficiency of steel cords.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004895928390000041
    Figure BDA0004895928390000041
  • Figure BDA0004895928390000051
    Figure BDA0004895928390000051
  • Figure BDA0004895928390000052
    Figure BDA0004895928390000052
Patent Text Reader

Abstract

The invention relates to a production method of an ultrahigh-strength 86-grade tire cord steel wire rod. The production method comprises the following steps: (1) a steel billet heating procedure: controlling the time of a preheating section to be 30-55 minutes; the temperature of the first heating section is 700-800 DEG C, and the time is 40-60 minutes; the temperature of the second heating section ranges from 900 DEG C to 1000 DEG C, and the time ranges from 60 min to 90 min; the temperature of a soaking zone is 1100-1150 DEG C, the time is 50-85 minutes, and the initial rolling temperature is 1100-1150 DEG C; 2) a controlled rolling process: the finish rolling temperature is 950-990 DEG C, a high-temperature spinning process is adopted, and the spinning temperature is 925-955 DEG C; and (3) a controlled cooling process is carried out, specifically, cooling is controlled through the Steymole process, the air volume of fans is selected to be 160000 + / -20000m < 3 > / h, 1 #-2 # fans are started by 75%-85%, and after it is ensured that the temperature of the lap joint point of the wire rod at the inlet of the 3 # fan is 670 + / -25 DEG C, the 3 #-6 # fans are started by 45%-55%, the rest fans are all closed, and heat preservation covers of the whole line are all opened. The tire cord steel wire rod has high purity, the sorbite rate is larger than or equal to 95%, large-grade cementite does not exist, the tensile strength is 1120-1260 MPa, the drawing requirement of the ultrahigh-strength steel cord can be met, and the overall production cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, and in particular to a production method of an ultra-high strength 86-grade cord steel wire rod. Background Art

[0002] Steel cord is widely used in passenger car tires, light truck tires, truck tires, construction machinery tires and aircraft tires as the skeleton material of radial rubber tires. The development of high-strength and ultra-high-strength steel cord can effectively improve the strength of tire carcass and belt layer, thereby improving tire safety performance; and can reduce the use of steel cord in tires, reduce production costs, reduce tire quality and rolling resistance, and reduce fuel consumption. Therefore, the development of high-strength and ultra-high-strength steel cord is in line with the development trend of lightweight and green environmental protection in today's automotive industry. Steel cord is made by drawing cord steel wire rods. At present, the mainstream products on the market are grade 72 (i.e., C content is 0.72wt.%) and grade 82 (i.e., C content is 0.82wt.%) cord steel. The development of higher grade and higher strength grade 86 (i.e., C content is 0.86wt.%) cord steel production process has very important practical significance.

[0003] In order to increase the strength, the C content of grade 86 cord steel is significantly increased compared with grade 82 and grade 72. However, the increase in C content leads to an increase in the tendency of central segregation and network cementite precipitation. Network cementite is one of the main reasons for the pull-out fracture during the processing of cord steel. In addition, hard inclusions and surface quality defects can also cause the cord steel to break during pull-out. In view of this situation, the present invention discloses a production process for grade 86 cord steel, and the obtained wire rod has a troostite rate of ≥95%, no large-scale network cementite, high purity, and a tensile strength of 1120 to 1260 MPa.

[0004] Patent document No. 201510548160.4 discloses a low-cost cord steel wire rod and a method for controlling its nitrogen content. The method effectively improves the smelting quality of cord steel by optimizing the refining process and properly controlling the contents of C, S and O. However, the C content of the cord steel described in the method is 0.79% to 0.83%, which belongs to grade 80 or 82 cord steel.

[0005] The patent document with application number 202011105232.5 discloses a method for controlling segregation and carbon network of 86-grade high-strength cord steel wire rod. The specific production process includes molten iron pretreatment, BOF converter smelting, LF furnace refining, continuous casting, billet surface cleaning, billet heating and controlled rolling and cooling, etc. However, the C content of the cord steel described in the patent is 0.85-0.90%, the upper limit is too high, and segregation and network cementite are not easy to control. Therefore, the heating furnace temperature of the patent is high and the time is long (190min-300min), resulting in high production costs and high energy consumption per ton of steel.

[0006] The patent application with application number 202110822163.8 discloses a low-cost grade 86 cord steel and its preparation process. The spacing of the lamellar pearlite in the cross-sectional metallographic structure of the cord steel produced is 155-165nm, and the troostitization rate is 95-98%, which ensures the strength and plasticity of the cord steel wire rod. However, the application adopts composite microalloying, and the cord steel composition contains a certain amount of Nb and V elements, which increases the difficulty of production.

[0007] The patent application with application number 202011338862.7 discloses a method for producing grade 90 and above cord steel. The production method includes processes such as molten steel smelting, continuous casting, blanking, grinding, rolling and temperature-controlled cooling. This production method is a two-fired material forming process, which has the disadvantages of a long process route and high cost. Summary of the invention

[0008] The present invention provides a method for producing an ultra-high strength 86-grade cord steel wire rod, which has high purity, a troostite rate of ≥95%, no large-scale cementite, and a tensile strength of 1120-1260 MPa, can meet the ultra-high strength steel cord drawing requirements, and has a low overall production cost.

[0009] To achieve the above object, the present invention adopts the following technical solutions:

[0010] A production method of ultra-high strength 86-grade cord steel wire rod, including molten iron pretreatment, BOF converter smelting, LF furnace refining, (150±10) mm×(150±10) mm square billet continuous casting, billet heating, controlled rolling, and controlled cooling, specifically including:

[0011] 1) Hot metal pretreatment process: spray passivation magnesium powder and lime powder into the hot metal ladle for desulfurization, apply mechanical stirring to remove the sulfur content in the hot metal, and then scrape off the desulfurization slag in the ladle to ensure that the sulfur content of the hot metal after treatment is ≤0.003%.

[0012] 2) BOF converter smelting process: adopt oxygen top and bottom combined blowing, and the steel tapping temperature is 1580-1595℃; the final high carbon, [C] content is preferably 0.55-0.65%, the target first pouring furnace P≤0.012%, avoid secondary spot blowing; if spot blowing is performed twice, perform the cover drop treatment. Perform ladle alloying: add lime and ferroalloy for deoxidation and alloying when 1 / 4-1 / 3 of the steel is tapped, and blow argon throughout the tapping process; the target amount of alloy added per ton of steel: 2.6-3.5kg / t of silicon manganese, 1.2-1.8kg / t of low-calcium ferrosilicon. Ensure that the final carbon content and temperature are hit once, the ladle and alloy are fully baked, the ladle is pre-blown with argon for 3-4 minutes, the slag is blocked for tapping, and slag is prevented. The steel tapping process maintains a circular flow, prohibits the scattered flow of molten steel, and the tapping time is controlled at 4-6 minutes. The static argon blowing time is ≥5min, the temperature before the static argon blowing treatment is 1505-1530°C, and the temperature after the static argon blowing treatment is 1480-1510°C.

[0013] 3) LF furnace refining process: Use micro-positive pressure and strengthen argon blowing to reduce the chance of molten steel inhalation. The pressure in the furnace under micro-positive pressure operation is 40-70kPa. During production, smoke is emitted from the furnace mouth and electrode mouth to avoid inhalation. During the refining process, except for slag dissolution, large argon blowing is prohibited, and the exposed diameter of molten steel is less than 400mm. After slag dissolution, use low-speed high current to heat up, and avoid using high-speed low current to heat up repeatedly, which will lead to long power-on time and air ionization and nitrogen increase. LF refining time is 60-80min, and the full analysis temperature is 1530℃~1550℃. Amount of auxiliary materials added per ton of steel: active lime 3.3-3.6kg / t, quartz sand 3.0-3.2kg / t, carbide slag 0.4-0.67kg / t, carbonized rice husk 0.50-1.0kg / t, medium carbon ferromanganese 0.8-1.2kg / t, low calcium ferrosilicon 0.85-1.35kg / t; soft blowing time ≥15min.

[0014] Through molten iron pretreatment, converter smelting and LF furnace refining, the nitrogen content of molten steel can be minimized, the TiN inclusions in the molten steel can be reduced, the purity of the molten steel can be improved, and the inclusions in the cord steel can be reduced.

[0015] 4) (150±10)mm×(150±10)mm small square billet continuous casting process: adopt the whole process protection casting process and clean the tundish with argon before casting. The argon purge of the tundish should be no less than 2min before starting the machine; during the pouring process, the tundish should be filled with argon throughout the process (after the roaster is lifted, argon is passed until the argon is turned off after the entire pouring); the argon pressure is ≥0.6MPa, and the liquid level should not flip. Attention should also be paid to the air intake during the pouring process. Before pouring, it is required to check whether the protective pouring argon is normal and whether there is any leakage in the pipeline. If there is any abnormality, it must be handled in time to ensure the protective pouring effect. During pouring, the large ladle falls to the bottom and the insertion depth of the protective sleeve is ≥200mm; the sleeve must ensure that the sealing ring is installed and it is vertical, and the molten steel cannot be exposed to the liquid surface. Crystallizer electromagnetic stirring and end electromagnetic stirring are used during continuous casting. The crystallizer electromagnetic stirring current is 280~320A, frequency is 4~6Hz, forward and reverse; the end electromagnetic stirring current is 280~320A, frequency is 6~10Hz, continuous rotation. The platform temperature is 1540±5℃, the middle package temperature is 1495℃~1515℃, low superheat casting is adopted, the superheat is maintained at 20℃~35℃, and the constant pulling speed is 2.0~2.3m / min. The crystallizer protection slag uses square billet high carbon steel protection slag; the billet is slowly cooled down after it is off the line.

[0016] 5) Billet heating process: The continuous casting billet is heated by a regenerative walking beam heating furnace. The preheating time is controlled to be 30-55min; the temperature of the first heating stage is 700-800℃, the time is 40-60min; the temperature of the second heating stage is 900-1000℃, the time is 60-90min; the temperature of the soaking stage is 1100-1150℃, the time is 50-85min, and the rolling temperature is 1100-1150℃; the heating furnace is heated in a reducing atmosphere, and the air-fuel ratio is controlled to be 0.4-0.5. In order to control the thickness of the decarburized layer of the cord steel, the billet heating temperature should be reduced as much as possible under the condition of meeting the rolling and wire drawing temperature requirements, or the lower limit of the billet heating temperature should be selected for steel production. At the same time, the temperature of the preheating section is below 800℃, and the heating section and soaking section should be heated quickly; the heating atmosphere and air-fuel ratio are controlled in the heating furnace.

[0017] 6) Controlled rolling process: The rolling process includes 6 rough rolling passes, 8 intermediate rolling passes, 6 pre-finishing rolling passes and 10 finishing rolling passes. The finishing rolling temperature is 950-990℃, and the high temperature wire laying process is adopted. The wire laying temperature is 925-955℃, which inhibits the precipitation of the core network cementite and optimizes the thickness of the iron oxide scale to 10-15μm, which is easy to remove the iron oxide scale by mechanical shelling of the wire rod. The final wire rod diameter is 5.5-6.5mm.

[0018] 7) Cooling control process: Use Steinmore process to control cooling, and select fan air volume of 160000±20000m 3 / h, 1 # —2 #The fan is turned on 75% to 85%, ensuring 3 # When the temperature of the wire rod overlap point at the fan inlet reaches 670±25℃, # -6 # The fans are turned on at 45% to 55%, and the remaining 5 fans are all turned off. The insulation covers of the entire line are opened to control the cooling speed of the air cooling. # —2 # The fan uses a large air volume to quickly reduce the temperature of the wire rod, crossing the cementite transformation temperature range, and avoiding the formation of harmful network cementite structure inside the wire rod. # —6 # The fans use a lower air volume and the remaining 5 fans are turned off, so that the wire rod stays in the pearlite transformation temperature range for a longer time and fully generates the required pearlite structure.

[0019] The chemical composition of the ultra-high strength 86 grade cord steel wire rod is calculated by weight percentage as follows: C 0.84%~0.88%, Si0.15%~0.28%, Mn 0.45%~0.55%, P≤0.010%, S≤0.010%, Cr≤0.08%, Ni≤0.06%, Cu≤0.08%, Als≤0.005%, [O]≤0.0030%, [H]≤0.0003%, [N]≤0.0050%, and the balance is Fe and unavoidable impurities.

[0020] The cord steel wire rod has high purity, a troostite rate of ≥95%, a network cementite of ≤1.0 grade, a tensile strength of 1120-1260 MPa, and an elongation of ≥35%.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The cord steel wire rod obtained by the method provided by the present application has a troostite content of ≥95%, a network cementite of ≤1.0 grade, no martensite, a decarburized layer depth of ≤50μm, and a wire rod with high strength and high toughness, meeting the user's drawing and use requirements. The method provided by the present invention adopts a one-fire material forming process, has low production cost and low energy consumption, can enhance the competitiveness of enterprises, and create better profit margins. DETAILED DESCRIPTION

[0023] In order to more clearly explain the objectives of the present application, the technical means adopted and their advantages, the specific embodiments in the present application will be described in detail below. It should be clear that the enumerated embodiments only represent a part of the practical application of the present application, rather than all applications. The description of these embodiments is intended to help understand the core ideas and practical applications of the present invention, but should not be interpreted as limiting the scope of protection of the present invention. Based on the embodiments disclosed in the present application, any other embodiments derived by any technician in the field without involving creative work should be deemed to be included in the scope of protection of the present application.

[0024] A method for producing ultra-high strength 86-grade cord steel wire rod adopts a small square billet-fire material process, specifically comprising the following steps: molten iron pretreatment → BOF converter smelting → LF refining → 150mm×150mm small square billet continuous casting → billet heating → controlled rolling → controlled cooling → inspection and packaging. The chemical composition of the embodiment is shown in Table 1; the molten iron pretreatment and BOF converter smelting process of the cord steel wire rod of the embodiment are shown in Table 2; the LF refining process of the cord steel wire rod of the embodiment is shown in Table 3; the continuous casting process of the cord steel wire rod of the embodiment is shown in Table 4; the controlled rolling process of the cord steel wire rod of the embodiment is shown in Table 5; the controlled cooling process of the cord steel wire rod of the embodiment is shown in Table 6.

[0025] Table 1 Chemical composition of the steel wire rod of the embodiment (wt%)

[0026]

[0027]

[0028] Table 2 Example of molten iron pretreatment and BOF converter smelting process of cord steel wire rod

[0029]

[0030] Table 3 LF refining process of cord steel wire rod of example

[0031]

[0032]

[0033] Table 4 Continuous casting process of cord steel wire rod

[0034]

[0035] Table 5 Controlled rolling process of the cord steel wire rod of the embodiment

[0036]

[0037]

[0038] Table 6 Controlled cooling process of the cord steel wire rod of the embodiment

[0039]

[0040] The present invention adopts reasonable design of converter steelmaking, LF refining, billet continuous casting and rolling process, and produces hot-rolled wire rods with high purity, high troostitization rate, and no large-scale network cementite, which can meet the requirements of ultra-high strength steel cord drawing. The cord steel wire rods of Examples 1 to 10 are tested for their microstructures and properties, and the results are shown in Table 7.

[0041] Table 7 Mechanical properties and metallographic structures of the embodiments of the present invention

[0042]

[0043]

[0044] The above is only a preferred specific implementation of the present invention. However, the protection scope of the present invention is not limited thereto, and any technical method obtained by equivalent replacement or simple conversion of the technical solution and its concept by any technician familiar with the technical field within the technical scope of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for producing ultra-high strength 86-grade cord steel wire rod, comprising molten iron pretreatment, BOF converter smelting, LF furnace refining, continuous casting, billet heating, controlled rolling, and controlled cooling, characterized in that: Specifically include: 1) Billet heating process: preheating time is controlled to 30-55min; The temperature of the first heating stage is 700-800℃, and the time is 40-60min; the temperature of the second heating stage is 900-1000℃, and the time is 60-90min; the temperature of the soaking stage is 1100-1150℃, and the time is 50-85min, and the rolling temperature is 1100-1150℃; 2) Controlled rolling process: the finishing rolling temperature is 950-990°C, the high temperature spinning process is adopted, and the spinning temperature is 925-955°C; 3) Cooling control process: Use Steinmore process to control cooling, and select fan air volume of 160000±20000m 3 / h, 1 # —2 # The fan is turned on 75% to 85%, ensuring 3 # When the temperature of the wire rod overlap point at the fan inlet reaches 670±25℃, # -6 # The fans are turned on at 45% to 55%, the remaining fans are all turned off, and the insulation covers of the entire line are opened.

2. The method for producing an ultra-high strength 86 grade cord steel wire rod according to claim 1, characterized in that: The molten iron pretreatment process includes: spraying passivation magnesium powder and lime powder into the molten iron ladle for desulfurization, applying mechanical stirring to remove the S content in the molten iron, and then scraping off the desulfurization slag in the ladle to ensure that the S content of the molten iron after treatment is ≤0.003%.

3. The method for producing an ultra-high strength 86 grade cord steel wire rod according to claim 1, characterized in that: The BOF converter smelting process includes: using oxygen top and bottom combined blowing, the steel tapping temperature is 1580-1595°C; pre-blowing argon in the ladle for 3-4 minutes, slag blocking steel tapping, the steel tapping time is controlled at 4-6 minutes, the static argon blowing time is ≥5 minutes, the temperature before the static argon blowing treatment is 1505-1530°C, and the temperature after the static argon blowing treatment is 1480-1510°C.

4. The method for producing an ultra-high strength 86 grade cord steel wire rod according to claim 1, characterized in that: The LF furnace refining process includes: the furnace pressure of the micro-positive pressure operation is 40-70kPa, the LF refining time is 60-80min, the full analysis temperature is 1530℃-1550℃, and the soft blowing time is ≥15min.

5. The method for producing an ultra-high strength 86 grade cord steel wire rod according to claim 1, characterized in that: The continuous casting process includes: purging the tundish with argon for no less than 2 minutes before starting the machine; during the pouring process, argon is passed through the tundish throughout the entire process; the argon pressure is ≥0.6MPa, and the liquid level is not flipped. During continuous casting, electromagnetic stirring of the crystallizer and electromagnetic stirring of the end are adopted, the platform temperature is 1540±5℃, the temperature of the tundish is 1495-1515℃, the superheat is maintained at 20-35℃, and the constant pulling speed is 2.0-2.3m / min.

6. The method for producing an ultra-high strength 86 grade cord steel wire rod according to claim 5, characterized in that: The crystallizer electromagnetic stirring current is 280-320A, the frequency is 4-6Hz, and it is forward and reverse; the end electromagnetic stirring current is 280-320A, the frequency is 6-10Hz, and it is continuously rotated.

7. The method for producing an ultra-high strength 86 grade cord steel wire rod according to claim 1, characterized in that: The diameter of the wire rod is 5.5-6.5 mm.

8. The method for producing an ultra-high strength 86 grade cord steel wire rod according to claim 1, characterized in that: The chemical composition of the steel is calculated by weight percentage: C 0.84%~0.88%, Si 0.15%~0.28%, Mn 0.45%~0.55%, P≤0.010%, S≤0.010%, Cr≤0.08%, Ni≤0.06%, Cu≤0.08%, Als≤0.005%, [O]≤0.0030%, [H]≤0.0003%, [N]≤0.0050%, and the balance is Fe and unavoidable impurities.

9. The method for producing an ultra-high strength 86 grade cord steel wire rod according to claim 1, characterized in that: The cord steel wire rod has a troostite rate of ≥95%, a tensile strength of 1120-1260 MPa, and an elongation of ≥35%.

Citation Information

Patent Citations

  • Production method of hot rolled high-carbon steel wire rod for rope manufacturing

    CN105441787A

  • Control method for segregation and net carbon of 86-grade high-strength cord steel wire rod

    CN112359277A

  • Wire rod for ultrahigh-strength hot-dip galvanized steel wire rope and production method of wire rod

    CN117089763A

  • Nitrogen-controlled production process for tire cord steel

    CN117165832A

  • Method for manufacturing carbon steel wire rods for tire cord

    KR1020030042998A

Cited By

  • Production method for inhibiting martensite transformation in 80-grade tire cord steel wire rod

    CN119307802A

  • Rolling method of high-carbon hard wire rod

    CN120619050A

  • High-plasticity extra-high-strength tire cord steel wire rod and production process thereof

    CN122344686A

  • High plasticity super high strength cord steel wire rod and production process thereof

    CN122344686B