Precision casting method special for complex thin-wall special-shaped bent pipe component
By adopting wax pattern preparation, silica sol shell coating and vibration shelling process in investment casting, the defect problem of high chromium nickel alloy thin-walled elbow components in the casting process is solved, efficient precision casting is achieved and the yield is improved. and product quality while reducing production costs.
Patent Information
- Application Number
- CN202310363826.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-15
AI Technical Summary
During the investment casting process, high-chromium-nickel high-temperature alloy thin-walled special-shaped bent pipe components are prone to defects such as undercasting, cracks, shrinkage cavities, and porosity, making it difficult to achieve efficient precision casting.
Using wax mold preparation, shell coating of silica sol binder and zirconium powder filler, dewaxing roasting and vibration shelling process, combined with specific process parameters and steps, such as wax injection pressure, temperature, casting time and vibration frequency, Ensure high-quality molding of castings.
It significantly improves the yield of thin-walled special-shaped elbow castings, reduces the production process and manufacturing cycle, reduces equipment and production costs, and improves product quality.
Smart Images

Figure CN118768516A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of precision (investment casting), and in particular to a precision casting method specially used for complex thin-walled special-shaped curved pipe components. Background Art
[0002] With the development of social economy and the continuous improvement of science and technology, modern casting technology is constantly being updated, improved and developed to meet the production needs of large-size components, high precision requirements, thin walls, complex structures, and high metallurgical mechanical properties.
[0003] In the vacuum pressure casting method, after the melt is poured, the subsequent filling step is carried out under the assistance of vacuum. After the filling is completed, the pressure is increased and maintained until the casting is completely solidified. However, the casting cost of this method is quite high and it is difficult to be widely adopted. Investment casting in precision casting has the characteristics of high precision and near net shape casting, which can achieve nearly zero-residue casting blanks, reduce many subsequent machining processes, and reduce production costs. It has received widespread attention in recent years and has been widely used in aerospace, shipbuilding, military and other technical fields.
[0004] High chromium nickel high temperature resistant alloy has high high temperature strength and oxidation resistance, is sensitive to sulfur-containing atmosphere, tends to be brittle at 600℃-800℃, and is suitable for making furnace components. Its tensile strength is 590MPa and hardness is ≤187. It is suitable for making engine high temperature resistant parts and other high temperature resistant parts serving in extreme environments. However, the alloy has high melting temperature, poor fluidity, large shrinkage tendency, thin wall and large curvature of bent pipe parts, and complex structure of some parts. When the above-mentioned investment casting method is used, it is very easy to produce defects such as undercasting, cracks, stress concentration, shrinkage and shrinkage during the casting process.
[0005] In summary, in order to meet production needs, further optimizing the precision casting method has become a key research direction for researchers in this field. Summary of the invention
[0006] The invention provides a precision casting method specially used for complex thin-walled special-shaped bent pipe components to solve the problems of undercasting, cracks, shrinkage cavities and shrinkage that are easily generated during the investment casting process of complex thin-walled special-shaped bent pipe components.
[0007] To achieve the purpose of the present invention, the present invention provides a technical solution: a precision casting method specifically used for complex thin-walled special-shaped curved pipe components, comprising the following steps:
[0008] 1) preparing a wax pattern and cooling it;
[0009] 2) Use an electric soldering iron to seamlessly weld the wax pattern with intact surface and the pouring system together to form a wax pattern assembly tree;
[0010] 3) After cleaning the wax model tree, evenly apply the prepared slurry on the wax model tree, and form a shell on the wax model after drying;
[0011] 4) The wax mold tree with the shell is placed in a dewaxing kettle for roasting and dewaxing to form a shell, and the molten alloy is cast into the shell, cooled and solidified; the shell is removed by vibration, and the casting is obtained after the corresponding pouring system is cut off;
[0012] 5) The castings are ground, shot blasted once, solution treated, shot blasted twice, pickled, passivated and dried, and the surface is inspected and repaired.
[0013] Furthermore, the wax pattern preparation in the above step 1) uses semi-solid paraffin as raw material, and a vertical wax injection machine is used to inject the semi-solid wax into the mold through the wax injection hole on the mold, and the wax injection pressure is 3.5-4MPa; the wax injection time is 22-25s, the wax injection temperature is 57-58°C, and the pressure holding time is 10-13s.
[0014] Furthermore, the specific steps of the above step 3) are as follows: ① Place the module in a cleaning agent for 2 to 3 seconds at room temperature and then rinse the surface oil in clean water; ② In a slurry barrel, use silica sol as a binder, add 315-325 mesh zirconium powder filler, anti-cracking agent, wetting agent and defoaming agent, stir for 10 to 12 hours, and the viscosity reaches 40Pa·s. Apply the surface layer slurry to the module, sprinkle 110-120 mesh zirconium sand, and dry for 10 to 12 hours; ③ Apply several layers of slurry on the module, sprinkle 60 mesh mullite sand, dry for 10 to 12 hours, apply the back layer slurry on the module, sprinkle 30 mesh mullite sand, dry for 13 to 15 hours, and repeat the back layer slurry shell making process several times, and dry for 13 to 15 hours each time; ④ When sealing the slurry, immerse the module in the silica sol pre-wetting agent, quickly take it out and let it stand, and air dry for 10 to 12 hours.
[0015] Furthermore, the roasting and dewaxing in the above step 4) is specifically to place the mold group including the wax mold with the gate downward after drying in a dewaxing kettle; the pressure in the kettle is 0.7-0.8MPa, the temperature is 160±10°C, and the dewaxing time is 15-20min; after the dewaxing is completed, the mold shell is placed in a roasting furnace and roasted to obtain the mold shell, the roasting time is 40-60min, and the roasting temperature is 1150-1180°C.
[0016] Furthermore, in the above step 4), the temperature of the molten alloy is 1600° C., the casting time is 8 to 12 seconds, the mold shell preheating temperature is 800 to 900° C., and the casting process follows the rule of first slow, then fast, and then slow again.
[0017] Furthermore, in the above step 4), the vibration impact frequency of the vibration shelling is 1200-1300 n / min.
[0018] Furthermore, in the above step 4), the cast alloy is a high-chromium-nickel high-temperature alloy, and its liquidus temperature is 1440°C.
[0019] Furthermore, in the above step 5), the shot blasting time of the first shot blasting treatment is 30 to 50 minutes, and the diameter of the steel shot is 0.6 mm; the second shot blasting treatment time is 30 to 40 minutes, and the diameter of the steel shot is 0.4 mm.
[0020] Furthermore, in the above step 5), the pH of the acid used for pickling is 1-2; during pickling, the pickling liquid level is above the casting, and then the casting is taken out and cleaned after being immersed for 2-5 minutes. During passivation, the casting is taken out after being immersed for 4-6 minutes after being immersed in a hot water pool at 80-100°C and free of impurities for 3-5 minutes, and then taken out and air-dried.
[0021] Furthermore, in the above step 4), after the casting system is removed, the gate is reserved
[0022] 0.2~0.5mm.
[0023] Compared with the prior art, the advantages of the present invention are as follows:
[0024] The present invention is based on the method of investment casting for the special shape and complex morphological structure characteristics of high-chromium-nickel high-temperature alloy thin-walled special-shaped curved pipe components. During the processing of the shell, the mold is coated with a surface slurry with silica sol as a binder, zirconium powder filler, anti-cracking agent, wetting agent and defoaming agent, and zirconium sand is sprinkled on it, so that the thickness is easy to be uniform. At the same time, the mold is immersed in silica sol pre-wetting agent when sealing the slurry, and the shell can be made up to 5 layers. In conjunction with the steps of dewaxing and roasting, specific process parameters are further set, which overcomes the limitations of traditional investment casting in producing high-chromium-nickel high-temperature alloy thin-walled complex curved pipe castings, greatly improves the yield rate of this type of thin-walled special-shaped curved pipe castings, and while improving product quality, reduces production processes, shortens finished product time, shortens manufacturing cycle, effectively reduces equipment and production costs, and maximizes production benefits. Description of the drawings:
[0025] Figure 1 The complex thin-walled special-shaped curved pipe component produced in Example 1;
[0026] Figure 2 This is the complex thin-walled special-shaped curved pipe component produced in Example 2. DETAILED DESCRIPTION
[0027] The technical solution of the present invention will be clearly described below in conjunction with the accompanying drawings and embodiments. It is obvious that the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0028] The thin-walled special-shaped curved pipe component targeted by the present invention has the following basic size ranges: length: 120-130mm; width: 120-130mm; height: 200-225mm, the whole is a curved pipe structure, and is connected by a thin-walled straight pipe, an intermediate flange and an elbow structure. The wall thickness difference between the straight pipe and the flange connection is 0.5mm, more than 70% of the surface of the casting is a thin-walled arc structure with a thickness of 1.5-2mm, and the groove width on both sides of the flange is between 6mm, the wall thickness between the two grooves is 5mm, the thickness of the flange is 16mm, and the mouth of the curved pipe is a flare-like mouth that expands outward by 70°. Except for the flange and the straight pipe part that require a small amount of machining, the rest of the parts require no excess casting.
[0029] For complex thin-walled special-shaped curved pipe components, the investment casting process steps provided by the present invention are as follows:
[0030] 1) Analyze the mold to find the best steps to remove the wax pattern, prepare the molded wax pattern, and cool the wax pattern:
[0031] The mold coated with release agent is fixed on the hydraulic press platform, and the semi-solid wax is injected into the mold through the wax injection hole on the mold by a vertical wax injection machine. The wax injection pressure is 3.5-4MPa; the wax injection time is 22-25s, the wax injection temperature is 57-58℃, and the pressure holding time is 10-13s; since this type of elbow is complex and has thin walls, it is extremely difficult to remove it during the preparation of the wax mold. Through repeated experiments, the optimal mold removal steps are found, the wax mold with intact surface quality is taken out, and then it is placed in water to cool.
[0032] 2) The prepared wax model and pouring system are seamlessly welded together using an electric soldering iron to form a wax model assembly tree. The wax model assembly tree adopts a conventional side-injection / bottom-column pouring system, which is composed of a pouring cup, a straight runner and a cross runner. The wax pouring system and the wax model casting are seamlessly bonded together by heating with an electric soldering iron.
[0033] 3) After cleaning the wax model tree, evenly apply the prepared slurry on the wax model tree, and form a shell on the wax model after drying:
[0034] ① Place the module in the cleaning agent for 2 to 3 seconds and then rinse the surface oil in clean water; ② In the slurry barrel, use silica sol as a binder, add 315-325 mesh zirconium powder filler, anti-cracking agent, wetting agent and defoaming agent, stir for 10 to 12 hours to fully mix, and the viscosity reaches 40Pa·s. Apply the surface layer slurry to the module, sprinkle 110-120 mesh zirconium sand, and dry for 10 to 12 hours; ③ Apply the second layer of slurry on the module, sprinkle 60 mesh mullite sand, dry for 10 to 12 hours, apply the back layer slurry on the module, sprinkle 30 mesh mullite sand, dry for 13 to 15 hours, and repeat the back layer slurry shell making several times, and dry for 13 to 15 hours each time; ④ When sealing the slurry, immerse the module in the silica sol pre-wetting agent, take it out after 2 seconds, let it stand for 5 seconds, and air dry for 10 to 12 hours. Repeating this process, the reverse replication shell can reach 5 layers with an average wall thickness of 10mm.
[0035] 4) The wax mold tree with the shell is placed in a dewaxing kettle for roasting and dewaxing to form a shell, and the molten alloy is cast in the shell. After cooling, the shell is vibrated and removed, and the casting is obtained after the casting system is cut off:
[0036] During roasting and dewaxing, the mold including the wax pattern is placed downward with the gate facing downward after drying in the dewaxing kettle; the pressure in the kettle is 0.7-0.8MPa, the temperature is 160±10℃, and the dewaxing time is 15-20min. The wax removed from the dewaxing kettle is recovered to the wax treatment room for impurity removal and is ready for reuse; the pressure in the dewaxing kettle is constant during the dewaxing process to prevent the shell from cracking; after dewaxing, the shell is placed in a roasting furnace for roasting for 40-60min at a temperature of 1150-1180℃ to obtain a high-temperature resistant mold shell ready for casting.
[0037] The high-temperature alloy liquid to be cast is a high-chromium-nickel high-temperature alloy with a liquidus temperature of 1440°C. The temperature of the molten alloy is 1600-1700°C, the casting time is 8-12s, the shell preheating temperature is 800-900°C, the casting is placed on the sand table with the shell, and a heat preservation agent is sprinkled on the pouring and riser. After the metal liquid is completely solidified, it is sent to the designated location for placement. The principle of slow first, fast then slow again is followed during the casting process.
[0038] After cooling and solidification, vibration shelling is adopted, and the vibration impact frequency is 1200~1300n / min, and it must be ensured that there is no vibration damage and deformation during the vibration process.
[0039] Use a cutting machine to cut off the pouring system connected to the casting. Ensure that the gate is reserved for 0.2 to 0.5 mm, no burrs are allowed to remain, no abrasions are allowed, and the casting appearance is visually undamaged. Then use an angle grinder to remove excess burrs on the casting surface.
[0040] 5) Grinding, primary shot blasting, solution treatment, secondary shot blasting, pickling, passivation and drying of castings, surface inspection and repair:
[0041] The casting is shot blasted twice. The shot blasting time of the first shot blasting is 30-50 minutes, and the diameter of the steel shot is 0.6mm; the second shot blasting time is 30-40 minutes, and the diameter of the steel shot is 0.4mm.
[0042] The castings after the secondary shot blasting are pickled and passivated. The pH of the acid used for passivation pickling is 1-2. During pickling, the pickling liquid level is above the casting and then soaked for 2-5 minutes, then taken out and cleaned. During passivation, the liquid level is above the casting and then soaked for 4-6 minutes, then taken out, soaked in a hot water pool at 80-100°C and free of impurities for 3-5 minutes, then taken out and air-dried. Visually, there is no trace of pickling liquid and oxide scale on the surface.
[0043] Embodiment 1, a precision casting method specifically used for complex thin-walled special-shaped curved pipe components, specifically comprising the following steps:
[0044] 1) For thin-walled special-shaped elbow castings, fix the mold coated with release agent on the hydraulic press platform, and use a vertical wax injection machine to inject semi-solid wax into the mold through the wax injection hole on the mold. The wax injection pressure is 3.5-4MPa; the wax injection time is 22s, the wax injection temperature is 58℃, and the pressure holding time is 10s. Take out the wax mold with good surface quality and put it into water for cooling.
[0045] 2) The wax model with intact surface and the pouring system are seamlessly welded together using an electric soldering iron to form a wax model assembly tree. The wax model assembly tree is prepared using a bottom pouring system.
[0046] 3) Prepare the shell: ① Place the module in a cleaning agent for 2 to 3 seconds and then rinse the surface oil in clean water; ② In a slurry barrel, use silica sol as a binder, add 315-325 mesh zirconium powder filler, anti-cracking agent, wetting agent and defoaming agent, stir for 10 hours to fully mix, and the viscosity reaches 40Pa·s. Apply the surface layer slurry to the module, sprinkle 110-120 mesh zircon sand, and dry for 12 hours; Apply the second layer of slurry on the module, sprinkle 60 mesh mullite sand, dry for 10 hours, apply the back layer slurry on the module, sprinkle 30 mesh mullite sand, dry for 15 hours, repeat the back layer slurry shell making twice, and dry for 15 hours each time; when sealing the slurry, immerse the module in the silica sol pre-wetting agent, take it out after 2 seconds, let it stand for 5 seconds, and air dry for 12 hours. The reverse copy shell has a total of 5 layers, with an average wall thickness of 10mm.
[0047] 4) Dewaxing and roasting: Place the mold with the wax pattern after drying, with the gate facing downward, in a dewaxing kettle; the pressure in the kettle is 0.7-0.8MPa, the temperature is 160±10℃, and the dewaxing time is 20min. The wax removed from the dewaxing kettle is recovered to the wax treatment room for impurity removal and is ready for reuse; the pressure in the dewaxing kettle is constant during the dewaxing process to prevent the shell from cracking; after dewaxing, place the shell in a roasting furnace for roasting for 40min at a temperature of 1150-1180℃ to obtain a high temperature resistant shell, ready for casting.
[0048] The alloy liquid with the alloy composition shown in Table 1 was cast into the preheated shell mold, the casting alloy liquid temperature was 1600°C, the casting time was 11s, and the shell mold preheating temperature was 900°C.
[0049] Table 1 Chemical composition of casting alloy
[0050]
[0051] After cooling and solidification, the shelling is carried out by vibration, and the vibration impact frequency is 1300n / min to ensure that there is no vibration damage and deformation during the vibration process.
[0052] After cutting off the casting system, a 0.5mm gate is reserved.
[0053] 5) Grinding, primary shot blasting, solution treatment, secondary shot blasting, pickling, passivation and drying of castings, surface inspection and repair:
[0054] In this embodiment, the shot blasting time of the first shot blasting treatment is 30 minutes, and the diameter of the steel shot is 0.6 mm; the second shot blasting treatment time is 40 minutes, and the diameter of the steel shot is 0.4 mm.
[0055] The pH of the acid used for passivation pickling is 1-2. During pickling, put the casting into the pickling tank, soak it for 2 minutes after the pickling liquid level is above the casting, then take it out and clean it. During passivation, soak it for 6 minutes after the liquid level is above the casting, then take it out and soak it in a hot water tank at 80℃ without impurities for 5 minutes, then take it out and air dry it. Visually observe that there is no trace of pickling liquid and oxide scale on the surface, and the casting is obtained. Figure 1 shown.
[0056] Embodiment 2, a precision casting method specifically used for complex thin-walled special-shaped curved pipe components, specifically comprising the following steps:
[0057] 1) For thin-walled special-shaped elbow castings, fix the mold with release agent on the hydraulic press platform, and use a vertical wax injection machine to inject semi-solid wax into the mold through the wax injection hole on the mold. The wax injection pressure is 3.5-4MPa; the wax injection time is 25s, the wax injection temperature is 57℃, and the pressure holding time is 13s; take out the wax mold with good surface quality and put it into water for cooling.
[0058] 2) The wax model with intact surface and the pouring system are seamlessly welded together using an electric soldering iron to form a wax model assembly tree. The wax model assembly tree is prepared using a side-injection pouring system.
[0059] 3) Prepare the shell: ① Place the module in a cleaning agent for 2 to 3 seconds and then rinse the surface oil in clean water; ② In a slurry barrel, use silica sol as a binder, add 315-325 mesh zirconium powder filler, anti-cracking agent, wetting agent and defoaming agent, stir for 11 hours to fully mix, and the viscosity reaches 40Pa·s. Apply the surface layer slurry to the module, sprinkle 110-120 mesh zircon sand, and dry for 11 hours; Apply the second layer of slurry on the module, sprinkle 60 mesh mullite sand, dry for 11 hours, apply the back layer slurry on the module, sprinkle 30 mesh mullite sand, dry for 14 hours, repeat the back layer slurry shell making twice, and dry for 13 hours each time; when sealing the slurry, immerse the module in the silica sol pre-wetting agent, take it out after 2 seconds, let it stand for 5 seconds, and then air dry for 12 hours. The reverse copy shell has a total of 5 layers, with an average wall thickness of 10mm.
[0060] 4) Dewaxing and roasting: Place the mold with the wax pattern after drying, with the gate facing downward, in a dewaxing kettle; the pressure in the kettle is 0.7-0.8MPa, the temperature is 160±10℃, and the dewaxing time is 15min. The wax removed from the dewaxing kettle is recovered to the wax treatment room for impurity removal and is ready for reuse; during the dewaxing process, the pressure in the dewaxing kettle is constant to prevent the shell from cracking; after dewaxing, place the shell in a roasting furnace for roasting for 60min at a temperature of 1150-1180℃ to obtain a high temperature resistant shell, ready for casting.
[0061] The alloy liquid with the alloy composition shown in Table 2 was cast into the preheated shell mold, the casting alloy liquid temperature was 1600°C, the casting time was 12s, and the shell mold preheating temperature was 900°C.
[0062] Table 2 Chemical composition of casting alloy
[0063]
[0064] After cooling and solidification, the shelling is carried out by vibration, and the vibration impact frequency is 1200-1300n / min to ensure that there is no vibration damage and deformation during the vibration process.
[0065] After cutting off the casting system, a gate is reserved with a width of 0.2 mm.
[0066] 5) Grinding, primary shot blasting, solution treatment, secondary shot blasting, pickling, passivation and drying of castings, surface inspection and repair:
[0067] In this embodiment, the shot blasting time of the first shot blasting treatment is 50 minutes, and the diameter of the steel shot is 0.6 mm; the second shot blasting treatment time is 30 minutes, and the diameter of the steel shot is 0.4 mm.
[0068] The pH of the acid used for passivation pickling is 1-2. During pickling, put it into the pickling tank, soak it for 5 minutes after the pickling liquid level is above the casting, then take it out and clean it. During passivation, soak it for 4 minutes after the liquid level is above the casting, then take it out and soak it in a hot water tank at 100°C without impurities for 3 minutes, then take it out and air dry it. Visually observe that there is no trace of pickling liquid and oxide scale on the surface, and obtain the casting, such as Figure 2 shown.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. It should be pointed out that any improvements made by ordinary technicians in this technical field without departing from the principle of the present invention should be regarded as the protection scope of the present invention.
Claims
1. A precision casting method specifically used for complex thin-walled special-shaped curved pipe components, characterized in that: The following steps are involved: Prepare wax pattern and cool; Use an electric soldering iron to seamlessly weld the wax pattern with intact surface and the pouring system together to form a wax pattern assembly tree; After cleaning the wax model tree, evenly apply the prepared slurry on the wax model tree, and form a shell on the wax model after drying; The wax mold tree with the shell is placed in a dewaxing kettle for roasting and dewaxing to form a shell, and the molten alloy is cast into the shell, cooled and solidified; the shell is removed by vibration, and the casting is obtained after the corresponding pouring system is cut off; The castings are ground, shot blasted once, solution treated, shot blasted twice, pickled, passivated and dried, and the surface is inspected and repaired.
2. A precision casting method for complex thin-walled special-shaped curved pipe components according to claim 1, characterized in that: The wax pattern preparation in step 1) uses semi-solid paraffin as raw material, and a vertical wax injection machine is used to inject the semi-solid wax into the mold through the wax injection hole on the mold. The wax injection pressure is 3.5~4MPa; the wax injection time is 22~25s, the wax injection temperature is 57~58℃, and the pressure holding time is 10~13s.
3. A precision casting method specifically for complex thin-walled special-shaped curved pipe components according to claim 2, characterized in that: The specific steps of step 3) are: ①Put the module in the cleaning agent at room temperature for 2-3 seconds, then rinse the surface oil in clean water; ②In a slurry barrel, use silica sol as a binder, add 315-325 mesh zirconium powder filler, anti-cracking agent, wetting agent and defoaming agent, and stir for 10-12 hours until the viscosity reaches 40Pa·s. Apply the surface slurry to the module, sprinkle 110-120 mesh zirconium sand, and dry it for 10-12 hours; Apply several layers of slurry on the module, sprinkle 60 mesh mullite sand, dry for 10-12 hours, apply back layer slurry on the module, sprinkle 30 mesh mullite sand, dry for 13-15 hours, repeat the back layer slurry coating several times, and dry for 13-15 hours each time; When sealing, immerse the module in silica sol pre-wetting agent, quickly take it out and let it stand, and air-dry for 10-12 hours.
4. A precision casting method specifically for complex thin-walled special-shaped curved pipe components according to claim 3, characterized in that: The roasting and dewaxing in step 4) is specifically as follows: placing the mold group including the wax mold with the gate downward after drying in a dewaxing kettle; the pressure in the kettle is 0.7~0.8MPa, the temperature is 160±10℃, and the dewaxing time is 15~20min; after the dewaxing is completed, placing the mold shell in a roasting furnace and roasting it to obtain the mold shell, the roasting time is 40~60min, and the roasting temperature is 1150~1180℃.
5. A precision casting method for complex thin-walled special-shaped curved pipe components according to any one of claims 1 to 4, characterized in that: In the step 4), the temperature of the molten alloy is 1600-1700° C., the casting time is 8-12 seconds, the mold shell preheating temperature is 800-900° C., and the casting process follows the rule of first slow, then fast, and then slow again.
6. A precision casting method specifically for complex thin-walled special-shaped curved pipe components according to claim 5, characterized in that: In the step 4), the vibration impact frequency of the vibration shelling is 1200-1300 n / min.
7. A precision casting method specifically for complex thin-walled special-shaped curved pipe components according to claim 6, characterized in that: In the step 4), the cast alloy is a high-chromium-nickel high-temperature alloy, and its liquidus temperature is 1440°C.
8. A precision casting method specifically used for complex thin-walled special-shaped curved pipe components according to claim 7, characterized in that: In the step 5), the shot blasting time of the first shot blasting treatment is 30-50 minutes, and the diameter of the steel shot is 0.6 mm; the second shot blasting treatment time is 30-40 minutes, and the diameter of the steel shot is 0.4 mm.
9. A precision casting method specifically for complex thin-walled special-shaped curved pipe components according to claim 8, characterized in that: In the step 5), the pH of the acid used for pickling is 1-2; during pickling, the pickling liquid level is above the casting, and then the casting is soaked for 2-5 minutes before being taken out and cleaned; during passivation, the liquid level is above the casting, and then the casting is soaked for 4-6 minutes before being taken out, and then soaked in a hot water pool at 80-100°C and free of impurities for 3-5 minutes before being taken out and air-dried.