Method for preparing high-purity quartz sand by deeply purifying natural quartz ore
By optimizing the traditional quartz sand preparation process and combining ultrasonic, transmission sorting, microwave, electric field interference and other technologies, the problems of low quartz sand quality and high impurities in the traditional process have been solved, and the deep purification of high-purity quartz sand has been achieved, which is suitable for many applications. The demand for high-purity quartz products in the field.
Patent Information
- Application Number
- CN202410808659.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional high-purity quartz sand preparation methods are difficult to effectively remove inclusion impurities, resulting in lower quartz sand quality, more gas-liquid inclusions and similar impurities, and quartz sand products prone to bubbles.
By optimizing traditional processes such as crushing, calcined water quenching, crushing, magnetic separation, and flotation, and adding ultrasonic scrubbing, transmission sorting, high-temperature atmosphere, electric field interference, color sorting, microwave calcination and other purification processes, including crushing, ultrasonic scrubbing, color Steps include selection, calcination, quenching, transmission sorting, sand making, magnetic separation, microwave roasting, electric field interference sorting, flotation, leaching, high temperature atmosphere and other steps.
It effectively improves the quality of natural quartz sand, removes primary mud and secondary mud, reduces impurity content, reduces gas-liquid inclusions and the presence of metal elements, and is suitable for quartz products such as high-purity quartz crucibles, quartz drawn tubes, and quartz weights.
Smart Images

Figure CN118771391A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of quartz sand purification, and in particular to a method for preparing high-purity quartz sand by deep purification of natural quartz ore. Background Art
[0002] High-purity quartz sand is the main raw material for the preparation of quartz crucibles, quartz drawn tubes, and quartz ingots. It is widely used in electronic communications, new energy, chemical medicine, aerospace, optics and other fields.
[0003] With the continuous development of photovoltaic, semiconductor, optical fiber, electronic integrated circuit and other fields, the market demand for high-purity quartz sand is gradually increasing. In the early days, natural crystal was mainly used to prepare high-purity quartz sand, but due to the problem of reserves and cost, it is no longer suitable for the current market demand for high-purity quartz sand. At this stage, natural quartz ore (vein quartz, granite pegmatite, quartzite, etc.) can be used, through physical, chemical, biological and other treatment methods, to finally obtain high-purity quartz sand with SiO2 content of more than 3N; among them, high-purity quartz sand for quartz crucible, quartz tube and quartz ingot requires extremely high impurity content, the total impurity element content of quartz tube is less than 70ppm, the impurity element content of quartz ingot is 50ppm, the outer layer purity grade of quartz dry pot is 4N5, and the inner layer of quartz dry pot is pure 4N8 or above. The traditional method for preparing high-purity quartz sand is coarse crushing-calcination water quenching-crushing-pickling-flotation-drying-magnetic separation and other processes. This conventional purification method is difficult to effectively remove inclusion impurities. Therefore, it is of great significance to innovate and optimize the purification process of high-purity quartz sand. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing high-purity quartz sand by deeply purifying natural quartz ore. The high-purity quartz sand prepared from natural quartz ore by traditional processes has low quality, more gas-liquid inclusions and similar impurities, and quartz sand products are prone to bubbles. By optimizing traditional purification processes such as crushing, calcination and water quenching, crushing, magnetic separation, flotation, acid leaching, and adding purification processes such as ultrasonic scrubbing, transmission sorting, high-temperature atmosphere, electric field interference, color sorting, and microwave calcination, the quality of quartz sand is finally improved.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for deeply purifying natural quartz ore to prepare high-purity quartz sand comprises the following steps:
[0007] Crushing, ultrasonic scrubbing, color sorting, calcination, quenching, transmission sorting, sand making, magnetic separation, microwave roasting, electric field interference sorting, flotation, leaching, high temperature atmosphere.
[0008] Furthermore, the natural quartz ore is selected from one of natural vein quartz, granite pegmatite and quartzite; the silicon dioxide content in natural vein quartz and quartzite is not less than 98.5%, and the silicon dioxide content in granite pegmatite is between 15% and 40%.
[0009] Furthermore, during the crushing operation, the feed particle size of the natural quartz ore is 50 to 500 mm, the natural quartz ore is washed with surface water and crushed to a particle size of 1 to 30 mm; the crushing operation equipment can adopt one or more of a jaw crusher, a gyratory crusher, a cone crusher, an impact crusher, an impact crusher, and a double-roll crusher.
[0010] Furthermore, during the ultrasonic scrubbing operation, the ultrasonic frequency is 15 to 60 KHz, the operating temperature is 30 to 60° C., the rotation speed of the drum scrubbing machine is 100 to 1000 r / min, and the ultrasonic scrubbing time is 1 min to 2 h.
[0011] Furthermore, the color sorter system used in the color sorting operation includes a feeding system, a transportation system, an identification system, and an execution system; the color sorter is one or more of a crawler type, a chute type, and a drop type; the applicable particle size for color sorting is 0.1 to 50 mm, and the number of color sorting times is 1 to 3 times; and an air compressor or air compressor station is provided to assist in air supply.
[0012] Furthermore, the calcination equipment in the calcination operation is one of a rotary tube furnace, a box muffle furnace, a rotary kiln, and a pot calcination furnace; the calcination temperature is 600-1200°C, and the calcination time is 1-5h; the quenching medium is a liquid or gaseous substance, the liquid medium is one or more of water, oil, brine, and alkaline water, the temperature is 0-50°C, and the gaseous medium is one or more of inert gases such as liquid nitrogen, liquid helium, liquid neon, and liquid argon.
[0013] Furthermore, transmission sorting uses one of X-rays, gamma rays, alpha rays, and beta rays; the detection components used are scintillation counters or scintillation detectors; commonly used equipment includes one or more transmission sorting machines such as X-ray sorting machines, TDS intelligent dry sorting machines, radioactive sorting machines, and X-ray intelligent sorting machines; transmission sorting is applicable to particle sizes of 0.1 to 300 mm, and the number of transmission sorting is 1 to 3 times.
[0014] Furthermore, the particle size of the sand making feed material is 0.5-30 mm, and the qualified particle size of the discharge material is 40-140 mesh material; the sand making method can be wet sand making or dry sand making; the sand making crushing equipment is one or more of a ball mill, a rod mill, a hammer crusher, an impact crusher, a double roller crusher, and a Raymond mill; the sand making screening equipment is one or more of a square swing screen, a linear vibrating screen, a high-frequency vibrating screen, an elliptical vibrating screen, and a circular vibrating screen; the sand making dust removal equipment is one or more of a bag dust collector, a cyclone dust collector, an electrostatic precipitator, and a wet dust collector.
[0015] Furthermore, the magnetic separation methods include dry magnetic separation, wet magnetic separation, and dry-wet combined magnetic separation; the magnetic separation separators include weak magnetic field magnetic separators and strong magnetic field magnetic separators; the weak magnetic field magnetic separators include one or more of permanent magnetic drum magnetic separators, permanent magnetic drum magnetic separators, permanent magnetic roller magnetic separators, and permanent magnetic tape magnetic separators, and the magnetic field strength is 0.4 to 1.5 T; the strong magnetic separators include one or more of electromagnetic dry powder magnetic separators, high gradient electromagnetic magnetic separators, strong magnetic field roller magnetic separators, vertical ring strong magnetic field magnetic separators, and periodic magnetic separators, and the magnetic field strength is 1.5 to 3.6 T.
[0016] Furthermore, in the microwave roasting operation, the microwave frequency is 300MHz-300GHz, the power of the microwave roasting device is 1-15kW; the preheating temperature is 600-850°C, the operating temperature is 600-1700°C, and the operating time is 10min-5h.
[0017] Furthermore, the specific operation of electric field interference sorting is as follows: the quartz sand particles are heated to 30-80°C, and then passed into a high-voltage direct current electric field for loading for 1 min-2 h; the direct current electric field is one or more of an electrostatic field, a corona electric field, and a composite electric field; the high-voltage direct current electric field strength is 2-6 WN / C; the electric separator is one or more of a high-voltage electric separator, a double-roller electric separator, a three-roller high-voltage electric separator, and a Capco high-voltage electric separator.
[0018] Furthermore, the flotation reagents used in the flotation operation include one or more of a pH adjuster, a collector, an inhibitor, an active agent, and a frother; the pH adjuster is one or more of HF, HCl, H2SO4, HNO3, NaOH, KOH, ammonia water, and Na2CO3; the pH of acid flotation is 1 to 6, the pH of alkaline flotation is 9 to 13, and the pH of neutral flotation is 7; the collector is an amine X-NH2, a hydroxyl X-OH, a hydrocarbon oil C n H 2n+2-m , ester RCOOX, sulfhydryl, amino acid RNHR-X or more; the inhibitor is one of phosphate, lignin, starch; the activator is an associated mineral activator or a quartz activator; the foaming agent is one of ethers, alcohols, ether alcohols, esters, ketone alcohols or more; the flotation machine is an air-filled flotation machine or a self-aspirated flotation machine; the flotation reaction temperature is 40-80°C, the flotation reaction time is 10min-2h; the number of flotations is one or more, the pulp mass concentration is 40-60%; the flotation machine stirring speed is 500-1500rpm / min.
[0019] Furthermore, the leaching method is one or more of alkali leaching, acid leaching and salt leaching; the chemical reagent used for alkali leaching is one or more of sodium hydroxide, potassium hydroxide and ammonia water, the alkali dosage is 0.1-1wt%, the alkali leaching temperature is 20-40°C, and the alkali leaching time is 0-10min; the chemical reagent used for acid leaching is one or more of hydrofluoric acid, hydrochloric acid, nitric acid, sulfuric acid, oxalic acid, glacial acetic acid, phosphoric acid and citric acid, the acid dosage is 1-5wt% of quartz sand, the acid leaching temperature is 40-80°C, and the acid leaching time is 4-24h; the chemical reagent used for salt leaching is one or more of sodium carbonate, sodium bicarbonate, sodium dihydrogen phosphate and sodium bisulfate, the salt dosage is 0.1-1wt% of quartz sand, the salt leaching temperature is 40-80°C, and the salt leaching time is 0-4h; the alkali leaching, acid leaching and salt leaching steps are not in order, and each leaching is cleaned with pure water; the mass concentration of the leached slurry is 40-60%.
[0020] Furthermore, the high-temperature atmosphere generating device is one of a rotating atmosphere tubular furnace and a fluidized bed high-temperature atmosphere tubular furnace, and the reaction chamber is made of a high-temperature resistant and corrosion-resistant material such as a platinum tube, a quartz glass tube, a ceramic tube, a tantalum-tungsten alloy tube, etc.; the reaction temperature is 500-1000°C, and the calcination time is 1-5h; the tubular furnace purification gas before the reaction is one of helium, neon, argon, krypton, and xenon, and the tube is subjected to oxygen pressure reduction treatment; the high-temperature atmosphere reactants are one or more of halogen elements and halides, including Cl2, F2, Br2, I2, HF, HCl, HBr, HI, NH4F, NH4HF2, NH4Cl, NH4Br, etc.; the reactant content does not exceed 0.1-10% of the mass of the quartz sand, and the tail gas needs to be collected and treated as waste gas.
[0021] Beneficial effects of the present invention:
[0022] The present invention can effectively improve the quality of natural quartz sand, wherein ultrasonic scrubbing can remove most of the primary mud and secondary mud to ensure the quality of the selected ore; color sorting can select most of the non-ferrous associated ores to reduce the impurity content; transmission sorting can use the transmission wave feedback signal to strip the quartz ore with a high impurity content through air blowing; microwave roasting can increase the cracks to facilitate subsequent process purification; electric field interference sorting can affect the electrical properties of the particles and discard the miscellaneous ores according to the conductivity deviation; in the high-temperature atmosphere under the oxygen reduction environment, some impurity elements are combined with halogen factors and volatilized and removed, ultimately reducing the gas-liquid inclusions and metal elements in the quartz sand. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention will be further described below in conjunction with the accompanying drawings.
[0024] Figure 1 It is a process step diagram of the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] like Figure 1 The figure shows the process steps of the invention, and the following embodiments are all operated according to the process steps.
[0027] Example 1
[0028] A method for preparing high-purity quartz sand by deep purification of natural quartz ore, the specific steps are as follows:
[0029] The natural vein quartz with a particle size of 200-300mm and a SiO2 mass content of 98.9% is washed with clean water and then crushed to -30mm by a jaw crusher; the crushed material is passed into an ultrasonic scrubber, the ultrasonic frequency is adjusted to 30KHz, the scrubbing temperature is 40°C, the motor speed is 500r / min, the operation time is 15min, and then clean water is passed for several times; the scrubbed material is dried and passed into a crawler color sorter for color sorting twice; the color-sorted concentrate is passed into a calcining furnace at 800°C for calcination for 2h, and then the quartz in a high temperature state is quickly passed into pure water at about 20°C for quenching; After quenching, the material is dried by the residual heat, and then passed into the X-ray transmission sorter for transmission sorting 3 times; after transmission sorting, the concentrate is passed into the vertical impact crusher for sand making, and then the circular vibrating screen is used to screen out qualified products of 40-140 meshes, and the qualified products are passed into the permanent magnetic tape magnetic separator with a magnetic field strength of 1T and the high-gradient electromagnetic magnetic separator with a magnetic field strength of 2T for magnetic separation 2-3 times; the material after magnetic separation is passed into the microwave calcining furnace for microwave calcination treatment for 2h, the microwave treatment temperature is 800℃, and the microwave frequency is 2.45GHz; the material after microwave treatment is kept at a residual temperature of about 60℃, and is directly passed into the high-voltage DC electric separator for loading for 30min, and the electric The field strength is 5WN / C; the electrostatic concentrate is put into a self-priming flotation machine for flotation operation, the mass concentration of the flotation slurry is 50%, the flotation temperature is 50°C, the stirring speed of the flotation machine is 1000r / min, H2SO4 with a mass concentration of 10% is added to adjust the slurry pH to 2, and 1.2kg / t oleic acid and 1.2kg / t dodecylamine are added for flotation for 20 minutes, followed by washing with pure water for several times and filtering the water; the flotation concentrate is alkali-leached at a slurry mass concentration of 50%, and NaOH is added at 0.1wt%, the alkali leaching time is 5min, the alkali leaching temperature is 60°C, and then washed and filtered with 60°C pure water; the quartz after alkali leaching is The sand was acid-leached at a pulp mass concentration of 40%, and HF and hydrochloric acid were added in a ratio of 1:2, the total acid dosage was 1wt%, the acid leaching time was 12h, the acid leaching temperature was 80°C, and then it was washed and filtered with pure water; the leached quartz sand was dried by a dryer, and magnetically separated by a high-gradient electromagnetic separator with a magnetic field strength of 2T, and then introduced into a rotating atmosphere tubular furnace for high-temperature atmosphere treatment. Before the experiment, argon gas was introduced into the tubular furnace to reduce the oxygen pressure, and then HCl gas was introduced to stabilize the gas pressure in the tubular furnace. The experimental reaction temperature was 800°C, the HCl gas was 1% of the mass of the quartz sand, the reaction time was 3h, and finally high-purity quartz sand was obtained.
[0030] Example 2
[0031] A method for preparing high-purity quartz sand by deep purification of natural quartz ore, the specific steps are as follows:
[0032] The natural granite pegmatite with a particle size of 200-300mm and a SiO2 mass content of 24.8% was washed with clean water, and then crushed to -1mm by a jaw crusher and a roller crusher; the crushed material was passed into an ultrasonic scrubber, and the ultrasonic frequency was adjusted to 30KHz, the scrubbing temperature was 40℃, the motor speed was 800r / min, and the operation time was 30min, and then cleaned with clean water for several times; the scrubbed material was dried and passed into a chute type color sorter for color sorting 2 times; then passed into an X-ray transmission sorter for transmission sorting 3 times; the transmission sorted concentrate was passed into a 700℃ calcining furnace for calcination for 1h, and then The quartz in a high temperature state is quickly passed into pure water at about 20°C for quenching treatment; the material after quenching is dried by the residual heat, and then passed into a hammer crusher for sand making, and then a square swing screen is used to screen out qualified products of 40 to 140 meshes, and the qualified products are passed into a drum magnetic separator with a magnetic field strength of 0.6T and a high-gradient electromagnetic magnetic separator with a magnetic field strength of 2T for magnetic separation treatment 2-3 times; the material after magnetic separation is passed into a microwave calcining furnace for microwave calcination treatment for 2h, the microwave treatment temperature is 800°C, and the microwave frequency is 2.45GHz; the material after microwave treatment is kept at a residual temperature of about 60°C, and is directly passed into a high-voltage DC electric separator for loading for 30min, and the electric The field strength is 5WN / C; the electrostatic concentrate is put into a self-priming flotation machine for flotation operation, the mass concentration of the flotation pulp is 50%, the flotation temperature is 60°C, the stirring speed of the flotation machine is 1200r / min, H2SO4 and HF with a mass concentration of 10% are added to adjust the pulp pH to 2, and 1kg / t of sodium petroleum sulfonate and 2kg / t of octadecylamine are added for flotation for 20 minutes, and flotation is performed 1-3 times, followed by washing with pure water for several times and filtering the water; the flotation quartz concentrate is subjected to alkali leaching at a pulp mass concentration of 50%, and NaOH is added at 0.5wt%, the alkali leaching time is 30 minutes, the alkali leaching temperature is 60°C, and then it is washed and filtered with 60°C pure water Treatment: The quartz sand after alkali leaching is subjected to acid leaching at a pulp mass concentration of 40%, and HF and hydrochloric acid are added in a ratio of 1:2, the total acid dosage is 2wt%, the acid leaching time is 16h, the acid leaching temperature is 80°C, and then it is washed and filtered with pure water; the leached quartz sand is dried by a dryer, and magnetically separated by a high-gradient electromagnetic separator with a magnetic field strength of 2T, and then introduced into a rotating atmosphere tubular furnace for high-temperature atmosphere treatment. Before the experiment, argon gas is introduced into the tubular furnace to reduce the oxygen pressure, and then HCl gas is introduced to stabilize the gas pressure in the tubular furnace. The experimental reaction temperature is 800°C, the HCl gas is 1% of the mass of the quartz sand, and the reaction time is 4h.
[0033] Example 3
[0034] A method for preparing high-purity quartz sand by deep purification of natural quartz ore, the specific steps are as follows:
[0035] The natural quartzite with a particle size of 200-300mm and a SiO2 mass content of 98.6% is washed with clean water, and then crushed to -5mm by a jaw crusher and a vertical impact crusher; the crushed material is passed into an ultrasonic scrubber, and the ultrasonic frequency is adjusted to 30KHz, the scrubbing temperature is 50℃, the motor speed is 600r / min, and the operation time is 20min, and then cleaned with clean water for several times; the scrubbed material is dried and passed into a crawler color sorter for color sorting twice; the color-sorted concentrate is passed into a calcining furnace at 800℃ for calcination for 4h, and then the quartz in a high temperature state is quickly passed into pure water at about 20℃ for quenching After quenching, the material is dried by residual heat, and then passed into the X-ray transmission separator for transmission separation for 3 times; after transmission separation, the concentrate is passed into the high-aluminum ceramic ball mill for grinding and sand making for 50 minutes, and then the circular vibrating screen is used to screen out qualified products of 80-220 mesh, and the qualified products are passed into the periodic magnetic separator with a magnetic field strength of 0.4-1.5T and the high-gradient electromagnetic magnetic separator with a magnetic field strength of 2T for magnetic separation for 2-3 times; the material after magnetic separation is passed into the microwave calcining furnace for microwave calcination for 2h, the microwave treatment temperature is 800℃, and the microwave frequency is 2.45GHz; the material after microwave treatment is kept at a residual temperature of about 60℃ and directly passed into the high-voltage DC electric separator The electrostatic ore concentrate was loaded for 30 minutes, and the electric field strength was 5WN / C; the electrostatic ore concentrate was put into the self-priming flotation machine for flotation operation, the mass concentration of the flotation pulp was 50%, the flotation temperature was 50℃, the stirring speed of the flotation machine was 1000r / min, HCL with a mass concentration of 10% was added to adjust the pulp pH to 2, and 1.2kg / t oleic acid and 1.2kg / t octadecylamine were added for flotation for 20 minutes, followed by washing with pure water for several times and filtering the water; the flotation concentrate was alkali leached at a pulp mass concentration of 50%, and NaOH was added at 0.1wt%, the alkali leaching time was 5min, the alkali leaching temperature was 60℃, and then it was washed and filtered with 60℃ pure water; the alkali leaching The treated quartz sand is acid-leached according to a pulp mass concentration of 40%, and HF and hydrochloric acid are added in a ratio of 1:2, the total acid dosage is 1wt%, the acid leaching time is 12h, the acid leaching temperature is 80°C, and then it is washed and filtered with pure water; the leached quartz sand is dried by a dryer, and magnetically separated by a high-gradient electromagnetic separator with a magnetic field strength of 2T, and then introduced into a rotating atmosphere tubular furnace for high-temperature atmosphere treatment. Before the experiment, argon gas is introduced into the tubular furnace to reduce the oxygen pressure, and then HCl gas is introduced to stabilize the gas pressure in the tubular furnace. The experimental reaction temperature is 800°C, the HCl gas is 1% of the mass of the quartz sand, and the reaction time is 3h, and finally high-purity quartz sand is obtained.
[0036] After testing, it was found that the quartz sand produced using this process method can fully reduce the single impurity content and total impurity content in the quartz sand (data see Table 1 below). By adjusting the product particle size and experimental conditions, it can be suitable for quartz crucibles, quartz drawn tubes, quartz ingots and other quartz products, expanding the application of silicon-based raw materials in photovoltaics, semiconductors, electric light sources, optics, electronic communications and other fields.
[0037] Table 1
[0038]
[0039]
[0040] The above specific implementation method part specifically introduces the analytical method involved in the present invention. It should be noted that the above introduction is only to help those skilled in the art better understand the method and ideas of the present invention, rather than limiting the relevant content. Without departing from the principle of the present invention, those skilled in the art may also make appropriate adjustments or modifications to the present invention, and the above adjustments and modifications shall also fall within the scope of protection of the present invention.
Claims
1. A method for preparing high-purity quartz sand by deep purification of natural quartz ore, characterized in that: The following steps are involved: Crushing, ultrasonic scrubbing, color sorting, calcination, quenching, transmission sorting, sand making, magnetic separation, microwave roasting, electric field interference sorting, flotation, leaching, high temperature atmosphere.
2. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: During the crushing operation, the feed particle size of natural quartz ore is 50-500mm. The natural quartz ore is washed with clean water on the surface and crushed to a particle size of 1-30mm. The crushing operation equipment adopts one or more of jaw crusher, gyratory crusher, cone crusher, impact crusher, impact crusher and double-roll crusher.
3. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: During the ultrasonic scrubbing operation, the ultrasonic frequency is 15-60KHz, the operating temperature is 30-60°C, the drum scrubber rotation speed is 100-1000r / min, and the ultrasonic scrubbing time is 1min-2h.
4. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: The color sorter used in color sorting operations is one or more of the crawler type, chute type and drop type; The applicable particle size of color sorting is 0.1-50mm, and the number of color sorting is 1-3 times; it is equipped with an air compressor or air compressor station for auxiliary air supply.
5. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: The calcining equipment in the calcining operation is one of a rotary tube furnace, a box muffle furnace, a rotary kiln, and a pot calcining furnace; the calcining temperature is 600-1200°C, and the calcining time is 1-5h; the quenching medium is a liquid or gaseous substance, the liquid medium is one or more of water, oil, brine, and alkaline water, the temperature is 0-50°C, and the gaseous medium is one or more of liquid nitrogen, liquid helium, liquid neon, and liquid argon.
6. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: Transmission sorting uses one of X-rays, gamma rays, alpha rays, and beta rays; the detection components used are scintillation counters or scintillation detectors; the equipment used is selected from one or more of X-ray sorting machines, TDS intelligent dry sorting machines, radioactive sorting machines, and X-ray intelligent sorting machines; the transmission sorting is suitable for particle sizes of 0.1 to 300 mm, and the number of transmission sorting is 1 to 3 times.
7. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: The particle size of the sand making feed material is 0.5-30mm, and the qualified particle size of the discharge material is 40-140 mesh material; the sand making method is wet sand making or dry sand making; the sand making crushing equipment is one or more of ball mill, rod mill, hammer crusher, impact crusher, roll crusher, Raymond mill; the sand making screening equipment is one or more of square swing screen, linear vibrating screen, high-frequency vibrating screen, elliptical vibrating screen, circular vibrating screen; the sand making dust removal equipment is one or more of bag dust collector, cyclone dust collector, electrostatic precipitator, wet dust collector.
8. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: The magnetic separation methods include dry magnetic separation, wet magnetic separation, and dry-wet combined magnetic separation; the magnetic separation separators include weak magnetic field magnetic separators and strong magnetic field magnetic separators; the weak magnetic field magnetic separators include one or more of permanent magnetic drum magnetic separators, permanent magnetic drum magnetic separators, permanent magnetic roller magnetic separators, and permanent magnetic tape magnetic separators, and the magnetic field strength is 0.4 to 1.5 T; the strong magnetic separators include one or more of electromagnetic dry powder magnetic separators, high gradient electromagnetic magnetic separators, strong magnetic field roller magnetic separators, vertical ring strong magnetic field magnetic separators, and periodic magnetic separators, and the magnetic field strength is 1.5 to 3.6 T.
9. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: In the microwave roasting operation, the microwave frequency is 300MHz~300GHz, the power of the microwave roasting device is 1~15kW; the preheating temperature is 600~850℃, the operating temperature is 600~1700℃, and the operating time is 10min~5h.
10. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: The specific operation of electric field interference sorting is as follows: the quartz sand particles are heated to 30-80°C, and then passed into a high-voltage direct current electric field for loading for 1 min-2 h; the direct current electric field is one or more of an electrostatic field, a corona electric field, and a composite electric field; the intensity of the high-voltage direct current electric field is 2-6 WN / C; the electric separator is one or more of a high-voltage electric separator, a double-roller electric separator, a three-roller high-voltage electric separator, and a Capco high-voltage electric separator.
11. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: The flotation reagents used in the flotation operation include one or more of a pH adjuster, a collector, an inhibitor, an active agent, and a frother; the pH adjuster is one or more of HF, HCl, H2SO4, HNO3, NaOH, KOH, ammonia water, and Na2CO3; the pH of acid flotation is 1 to 6, the pH of alkaline flotation is 9 to 13, and the pH of neutral flotation is 7; the collector is an amine X-NH2, a hydroxyl X-OH, a hydrocarbon oil C n H 2n+2-m , ester RCOOX, sulfhydryl, amino acid RNHR-X or more; the inhibitor is one of phosphate, lignin, starch; the activator is an associated mineral activator or a quartz activator; the foaming agent is one of ethers, alcohols, ether alcohols, esters, ketone alcohols or more; the flotation machine is an air-filled flotation machine or a self-aspirated flotation machine; the flotation reaction temperature is 40-80°C, the flotation reaction time is 10min-2h; the number of flotations is one or more, the pulp mass concentration is 40-60%; the flotation machine stirring speed is 500-1500rpm / min.
12. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: The leaching method is one or more of alkali leaching, acid leaching and salt leaching; the chemical reagent used for alkali leaching is one or more of sodium hydroxide, potassium hydroxide and ammonia water, the amount of alkali is 0.1-1wt%, the alkali leaching temperature is 20-40℃, and the alkali leaching time is 0-10min; the chemical reagent used for acid leaching is one or more of hydrofluoric acid, hydrochloric acid, nitric acid, sulfuric acid, oxalic acid, glacial acetic acid, phosphoric acid and citric acid, the amount of acid is 1-5wt% of quartz sand, the acid leaching temperature is 40-80℃, and the acid leaching time is 4-24h; the chemical reagent used for salt leaching is one or more of sodium carbonate, sodium bicarbonate, sodium dihydrogen phosphate and sodium bisulfate, the amount of salt is 0.1-1wt% of quartz sand, the salt leaching temperature is 40-80℃, and the salt leaching time is 0-4h; the alkali leaching, acid leaching and salt leaching steps are not in order, and pure water is used to clean after each leaching; the mass concentration of the leached slurry is 40-60%.
13. The method for preparing high-purity quartz sand by deep purification of natural quartz ore according to claim 1, characterized in that: The high-temperature atmosphere generating device is one of a rotary atmosphere tubular furnace and a fluidized bed high-temperature atmosphere tubular furnace, and the reaction chamber is selected from one of a platinum tube, a quartz glass tube, a ceramic tube, and a tantalum-tungsten alloy tube; the reaction temperature is 500-1000°C, and the calcination time is 1-5 hours; the tubular furnace purification gas before the reaction is one of helium, neon, argon, krypton, and xenon, and the oxygen pressure is reduced in the tube; the high-temperature atmosphere reactant is one or more of a halogen element and a halide; the reactant content does not exceed 0.1-10% of the mass of the quartz sand, and the tail gas is collected and treated as a waste gas.
Citation Information
Patent Citations
Method for removing gas-liquid inclusion and impurity during high-purity quartz sand production
CN102180584A
Process for preparing ultrahigh pure quartz sand through silica raw material
CN103613102A
Preparation method for high-purity quartz sand
CN104340981A
Method for preparing electronic-grade high-purity quartz sand
CN114378026A
Method for low-carbon efficient extraction of high-purity sio 2 from high-silicon hematite tailings
WO2024036664A1
Cited By
Preparation process of high-quality quartz tube
CN119143407A
High-purity quartz sand purification method based on microwave synergistic gradient high-voltage electric field
CN120964822A