Granular compound fertilizer prepared by using potassium sulfate co-production intermediate and preparation method thereof
Through the method of combining membrane technology with evaporation and crystallization, the problem of high energy consumption of evaporation and concentration of ammonium chloride mother liquor in metathesis method is solved, and high-efficiency and low-cost ammonium chloride compound fertilizer production is achieved.
Patent Information
- Application Number
- CN202411237231.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-05
AI Technical Summary
In the existing metathesis process for preparing potassium sulfate, the evaporation and concentration of the by-product potassium ammonium chloride mother liquor requires a large amount of energy, resulting in high production costs and low production efficiency.
Using a method of combining membrane technology with evaporative crystallization, a multi-step treatment is carried out through ceramic membranes and reverse osmosis membranes to remove moisture and solid impurities in the mother liquor, improve the concentration efficiency of potassium ammonium chloride, and reduce energy consumption.
It significantly reduces energy consumption and production costs, and improves the production efficiency of ammonium potassium chloride composite fertilizer.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of compound fertilizers, and in particular to a granular compound fertilizer prepared by utilizing a potassium sulfate co-production intermediate and a preparation method thereof. Background Art
[0002] Potassium sulfate is prepared by double decomposition, for example, potassium sulfate fertilizer is prepared by reacting ammonium sulfate with potassium chloride. When potassium sulfate is crystallized, a large amount of mother liquor is produced as a by-product. The main components of this mother liquor are potassium chloride and ammonium chloride, of which ammonium chloride is a reaction product. Due to the low conversion rate, the potassium chloride content in the mother liquor generally reaches about 15% of the amount of raw materials added, and the sum of the contents of N and K2O in the mother liquor is about 34%. In fertilizer manufacturing companies, this mother liquor containing a large amount of plant nutrients is usually evaporated and concentrated to obtain solid fertilizer. For example, the Chinese invention patent application with publication number CN106315622A discloses a "production equipment system for co-producing potassium sulfate and ammonium chloride", in which the mother liquor after separating potassium sulfate is discharged through the liquid phase outlet of the centrifuge, and solid ammonium chloride potassium fertilizer is obtained by evaporation. Evaporation and concentration of the mother liquor requires a large amount of energy consumption. According to actual calculations, the energy cost consumed is equivalent to the value of the solid fertilizer obtained. In addition, due to the long evaporation and concentration time of the by-product mother liquor, the process for preparing potassium sulfate by double decomposition is difficult to balance, which seriously affects the production efficiency. Summary of the invention
[0003] In order to overcome the above technical problems, the present invention provides a granular compound fertilizer prepared by using potassium sulfate co-production intermediate and a preparation method thereof. The present invention combines membrane technology with evaporation crystallization to prepare potassium ammonium chloride compound fertilizer, which saves energy and reduces emissions and reduces production costs of enterprises compared with traditional evaporation and concentration processes.
[0004] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0005] A method for preparing granular compound fertilizer by using potassium sulfate co-production intermediates, comprising the following steps:
[0006] S1, adding ammonium sulfate into water and stirring to dissolve to obtain an ammonium sulfate solution, introducing the ammonium sulfate solution into a crystallizer, heating it, and then adding potassium chloride into the crystallizer under stirring conditions, keeping the temperature to react, and obtaining potassium sulfate slurry;
[0007] S2, performing solid-liquid separation on the potassium sulfate slurry to obtain potassium sulfate and potassium ammonium chloride mother liquor;
[0008] S3, filtering the potassium ammonium chloride mother liquor through a ceramic membrane to remove solids and obtain a ceramic membrane filtrate;
[0009] S4, subjecting the ceramic membrane filtrate to reverse osmosis membrane concentration treatment to remove most of the water to obtain potassium ammonium chloride concentrate;
[0010] S5, evaporating and crystallizing the potassium ammonium chloride concentrated solution to obtain potassium ammonium chloride granular compound fertilizer.
[0011] In the technical scheme, potassium sulfate is prepared by double decomposition, and a byproduct potassium ammonium chloride mother liquor is produced at the same time. The traditional method is to prepare potassium ammonium chloride mother liquor by evaporation, concentration and crystallization, remove the water content of potassium ammonium chloride mother liquor, and obtain potassium ammonium chloride compound fertilizer. Since the mother liquor contains a large amount of water, evaporation and crystallization need to consume a large amount of energy, and the production cost of potassium ammonium chloride compound fertilizer is high. In order to solve the above problems, the present invention first uses a ceramic membrane to remove small particle solid impurities remaining in the mother liquor, and then uses a reverse osmosis membrane to intercept ammonium chloride and potassium chloride in the mother liquor, allowing water to pass through (water recycling can be achieved), thereby achieving the purpose of concentrating ammonium chloride and potassium chloride, and the concentrated potassium ammonium chloride mother liquor contains a small amount of water, and then uses an evaporation and crystallization process to remove the remaining water to obtain potassium ammonium chloride compound fertilizer. Compared with the traditional direct large-scale evaporation and crystallization process, the energy consumption of the enterprise is significantly reduced, thereby reducing the production cost of the enterprise.
[0012] Preferably, in step S1, the heating temperature is 45-50°C.
[0013] Preferably, in step S1, the mass ratio of ammonium sulfate to potassium chloride is 1:1.1-1.5.
[0014] Preferably, in step S3, the pore size of the ceramic membrane is 500-800 nm.
[0015] Preferably, in step S4, the method for preparing the reverse osmosis membrane comprises the following steps:
[0016] S41, adding m-phenylenediamine, sodium dodecyl sulfate and triethylamine into deionized water and stirring to dissolve, then adding the modified hollow mesoporous silica and stirring to disperse uniformly to obtain an aqueous suspension;
[0017] S42, adding trimesoyl chloride to n-hexane solvent, heating and stirring to dissolve, to obtain a trimesoyl chloride organic phase solution;
[0018] S43, immersing the polysulfone-based membrane in an organic phase solution of trimesoyl chloride, taking it out and placing it in an aqueous phase suspension to react at room temperature, taking it out and placing it in an oven for curing and cross-linking to obtain a reverse osmosis membrane intermediate;
[0019] S44, adding polyethyleneimine, sodium lauryl sulfate and triethylamine into deionized water and stirring to dissolve to obtain a polyethyleneimine aqueous solution;
[0020] S45, immersing the reverse osmosis membrane intermediate in an organic phase solution of trimesoyl chloride, taking it out and placing it in an aqueous phase solution of polyethyleneimine to react at room temperature, taking it out and placing it in an oven for curing and cross-linking to obtain a reverse osmosis membrane.
[0021] In the technical solution of the present invention, as described above, a reverse osmosis membrane is used to intercept ammonium chloride and potassium chloride in the mother liquor to achieve concentrated recovery of ammonium chloride potassium, but the defect of using a reverse osmosis membrane is that the pore size of the reverse osmosis membrane is relatively small, and the membrane water flux is relatively low, which affects the concentration efficiency of the membrane to ammonium chloride and potassium chloride. The present invention is to solve the above problems, improve the reverse osmosis membrane, use m-phenylenediamine and trimesoyl chloride as reaction monomers, interfacial polymerization occurs on the surface of a polysulfone-based membrane, and a dense separation functional layer with intercepted ammonium chloride potassium is generated. The present invention is to improve the flux of the reverse osmosis membrane, by mixing hollow mesoporous silica into a m-phenylenediamine solution, the hollow mesoporous silica is doped into the dense separation functional layer, and the pore structure of the hollow mesoporous silica is used to form a water molecule channel in the dense separation layer, thereby improving the water flux of the reverse osmosis membrane and improving the concentration efficiency of the membrane to ammonium chloride and potassium chloride. However, a further problem is that the surface of the dense separation functional layer is also dispersed with hollow mesoporous silica particles, and ammonium chloride and potassium chloride are easily transmitted through the pores of the hollow mesoporous silica particles, thereby affecting the interception of ammonium chloride and potassium chloride by the reverse osmosis membrane. In order to solve this problem, the present invention continues to cover the surface of the dense separation functional layer with a polyamide layer, that is, polyethyleneimine and trimesoyl chloride are used to undergo an interfacial polymerization reaction on the surface of the dense separation functional layer, and the generated polyamide layer can cover the hollow mesoporous silica on the surface of the dense separation functional layer, thereby preventing ammonium chloride and potassium chloride from easily passing through the pores of the hollow mesoporous silica particles, maintaining the interception of ammonium chloride and potassium chloride by the reverse osmosis membrane, and realizing the separation of ammonium chloride and potassium from water by the reverse osmosis membrane.
[0022] Preferably, in step S41, the mass ratio of m-phenylenediamine to modified hollow mesoporous silica is 1:0.1-0.3.
[0023] Preferably, in step S45, the reaction time at room temperature is 10-20 minutes.
[0024] Preferably, the preparation method of the modified hollow mesoporous silica comprises the following steps:
[0025] S411, adding hollow mesoporous silica to the hydrolyzate of epoxy silane coupling agent, stirring for reaction, centrifuging, washing and drying to obtain coupling agent modified hollow mesoporous silica;
[0026] S412, adding the coupling agent modified hollow mesoporous silica into the polyethyleneimine solution, heating to 80° C., stirring for reaction, and performing centrifugal separation, washing, and drying to obtain modified hollow mesoporous silica.
[0027] In the technical solution of the present invention, as described above, a polyamide layer is covered on the surface of the dense separation functional layer. During the experimental test, the polyamide layer is easily detached from the surface of the dense separation functional layer under high water pressure conditions, thereby causing the interception rate of the reverse osmosis membrane to ammonium chloride and potassium chloride to decrease. In order to solve this problem, the present invention modifies the hollow mesoporous silica, grafts polyethyleneimine on the surface of the hollow mesoporous silica, and loads amino groups on the surface of the hollow mesoporous silica. The amino groups dispersed on the surface of the dense separation functional layer can participate in the interfacial polymerization reaction between the polyethyleneimine of the polyamide layer and trimesoyl chloride, thereby bonding the dense separation functional layer to the polyamide layer through the force of chemical bonds, and preventing the polyamide layer from falling off the surface of the dense separation functional layer.
[0028] Preferably, in step S412, the stirring reaction time is 120-135 min.
[0029] In order to ensure that a sufficient amount of polyethyleneimine is grafted on the surface of the hollow mesoporous silica, the dense separation functional layer is bonded to the polyamide layer, and the reaction time of the coupling agent-modified hollow mesoporous silica and polyethyleneimine is controlled to be greater than 120 minutes. However, it was unexpectedly found during the experiment that when the reaction time of the coupling agent-modified hollow mesoporous silica and polyethyleneimine is greater than 135 minutes, the water flux of the reverse osmosis membrane is greatly reduced. This may be because polyethyleneimine is a hyperbranched structure. When an excessive amount of polyethyleneimine is grafted on the surface of the hollow mesoporous silica, polyethyleneimine will react with trimesoyl chloride, and the generated polymer will be coated on the surface of the hollow mesoporous silica, blocking the pore structure on the surface of the hollow mesoporous silica, thereby reducing the water flux of the reverse osmosis membrane. Therefore, the present invention simultaneously controls the reaction time of the coupling agent-modified hollow mesoporous silica and polyethyleneimine to be less than 135 minutes.
[0030] A granular compound fertilizer prepared by utilizing potassium sulfate co-production intermediate is prepared by the above method.
[0031] The present invention has the following beneficial effects:
[0032] 1) Use ceramic membrane to remove small solid impurities remaining in the mother liquor, and then use reverse osmosis membrane to intercept ammonium chloride and potassium chloride in the mother liquor, allowing water to pass through, so as to achieve the purpose of concentrating ammonium chloride and potassium chloride. The concentrated ammonium chloride potassium mother liquor contains a small amount of water, and then use evaporation and crystallization process to remove the remaining water to obtain ammonium chloride potassium compound fertilizer. Compared with the traditional direct large-scale evaporation and crystallization process, it significantly reduces the energy consumption of the enterprise, thereby reducing the production cost of the enterprise;
[0033] 2) The reverse osmosis membrane is improved, and the prepared reverse osmosis can intercept and concentrate potassium ammonium chloride while having a higher water flux and a higher concentration efficiency for potassium ammonium chloride. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0035] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art. Example 1
[0036] A method for preparing granular compound fertilizer by using potassium sulfate co-production intermediates, comprising the following steps:
[0037] S1, adding 60 kg of ammonium sulfate into 90 kg of water and stirring to dissolve to obtain an ammonium sulfate solution, introducing the ammonium sulfate solution into a crystallizer, heating to 50° C., and then adding potassium chloride to the crystallizer under stirring, the mass ratio of ammonium sulfate to potassium chloride being 1:1.4, and keeping the temperature for reaction for 45 minutes to obtain potassium sulfate slurry;
[0038] S2, performing solid-liquid separation on the potassium sulfate slurry to obtain potassium sulfate and potassium ammonium chloride mother liquor;
[0039] S3, filtering the potassium ammonium chloride mother liquor through a ceramic membrane with a pore size of 600 nm to remove solids and obtain a ceramic membrane filtrate;
[0040] S4, subjecting the ceramic membrane filtrate to reverse osmosis membrane concentration treatment to remove most of the water to obtain potassium ammonium chloride concentrate, the reverse osmosis membrane operating pressure is 40 bar, and the temperature is 45°C;
[0041] S5, evaporating and crystallizing the potassium ammonium chloride concentrated solution to obtain potassium ammonium chloride granular compound fertilizer.
[0042] The method for preparing a reverse osmosis membrane comprises the following steps:
[0043] S41, adding 4 g of m-phenylenediamine, 0.05 g of sodium dodecyl sulfate and 0.15 g of triethylamine to 500 mL of deionized water, stirring and dissolving, then adding modified hollow mesoporous silica, the mass ratio of m-phenylenediamine to modified hollow mesoporous silica being 1:0.25, stirring and dispersing uniformly to obtain an aqueous suspension;
[0044] S42, adding 2 g of trimesoyl chloride into 500 mL of n-hexane solvent, heating and stirring to dissolve, to obtain an organic phase solution of trimesoyl chloride;
[0045] S43, immersing the polysulfone-based membrane in an organic phase solution of trimesoyl chloride for 10 minutes, taking it out and placing it in an aqueous phase suspension, reacting it at room temperature for 30 minutes, taking it out and placing it in an oven at 70° C. for curing and cross-linking for 1 hour to obtain a reverse osmosis membrane intermediate;
[0046] S44, adding 2 g of polyethyleneimine, 0.02 g of sodium dodecyl sulfate and 0.1 g of triethylamine to 500 mL of deionized water and stirring to dissolve to obtain a polyethyleneimine aqueous solution;
[0047] S45, immersing the reverse osmosis membrane intermediate in an organic phase solution of trimesoyl chloride for 10 minutes, taking it out and placing it in an aqueous phase solution of polyethyleneimine, reacting it at room temperature for 18 minutes, taking it out and placing it in an oven at 60° C. for curing and cross-linking for 50 minutes to obtain a reverse osmosis membrane.
[0048] The preparation method of modified hollow mesoporous silica comprises the following steps:
[0049] S411, adding 0.2 g of epoxy silane coupling agent KH-560 to 300 mL of deionized water and stirring to dissolve to obtain an epoxy silane coupling agent hydrolyzate, adding 2 g of hollow mesoporous silica to the epoxy silane coupling agent hydrolyzate, heating to 50° C., stirring to react for 50 min, and centrifugally separating, washing, and drying to obtain coupling agent-modified hollow mesoporous silica;
[0050] S412, adding 1 g of coupling agent-modified hollow mesoporous silica into 200 mL of 1.5% polyethyleneimine solution, heating to 80° C., stirring the reaction for 130 min, and obtaining modified hollow mesoporous silica after centrifugal separation, washing, and drying. Example 2
[0051] A method for preparing granular compound fertilizer by using potassium sulfate co-production intermediates, comprising the following steps:
[0052] S1, adding 60 kg of ammonium sulfate into 90 kg of water and stirring to dissolve to obtain an ammonium sulfate solution, introducing the ammonium sulfate solution into a crystallizer, heating to 45°C, and then adding potassium chloride to the crystallizer under stirring, the mass ratio of ammonium sulfate to potassium chloride being 1:1.2, and keeping the temperature for reaction for 45 minutes to obtain potassium sulfate slurry;
[0053] S2, performing solid-liquid separation on the potassium sulfate slurry to obtain potassium sulfate and potassium ammonium chloride mother liquor;
[0054] S3, filtering the potassium ammonium chloride mother liquor through a ceramic membrane with a pore size of 600 nm to remove solids and obtain a ceramic membrane filtrate;
[0055] S4, subjecting the ceramic membrane filtrate to reverse osmosis membrane concentration treatment to remove most of the water to obtain potassium ammonium chloride concentrate, the reverse osmosis membrane operating pressure is 40 bar, and the temperature is 45°C;
[0056] S5, evaporating and crystallizing the potassium ammonium chloride concentrated solution to obtain potassium ammonium chloride granular compound fertilizer.
[0057] The method for preparing a reverse osmosis membrane comprises the following steps:
[0058] S41, adding 4 g of m-phenylenediamine, 0.05 g of sodium dodecyl sulfate and 0.15 g of triethylamine to 500 mL of deionized water, stirring and dissolving, then adding modified hollow mesoporous silica, the mass ratio of m-phenylenediamine to modified hollow mesoporous silica being 1:0.15, stirring and dispersing uniformly to obtain an aqueous suspension;
[0059] S42, adding 2 g of trimesoyl chloride into 500 mL of n-hexane solvent, heating and stirring to dissolve, to obtain an organic phase solution of trimesoyl chloride;
[0060] S43, immersing the polysulfone-based membrane in an organic phase solution of trimesoyl chloride for 10 minutes, taking it out and placing it in an aqueous phase suspension, reacting it at room temperature for 30 minutes, taking it out and placing it in an oven at 70° C. for curing and cross-linking for 1 hour to obtain a reverse osmosis membrane intermediate;
[0061] S44, adding 2 g of polyethyleneimine, 0.02 g of sodium dodecyl sulfate and 0.1 g of triethylamine to 500 mL of deionized water and stirring to dissolve to obtain a polyethyleneimine aqueous solution;
[0062] S45, immersing the reverse osmosis membrane intermediate in an organic phase solution of trimesoyl chloride for 10 minutes, taking it out and placing it in an aqueous solution of polyethyleneimine, reacting it at room temperature for 12 minutes, taking it out and placing it in an oven for curing and cross-linking at 60° C. for 50 minutes, to obtain a reverse osmosis membrane.
[0063] The preparation method of modified hollow mesoporous silica comprises the following steps:
[0064] S411, adding 0.2 g of epoxy silane coupling agent KH-560 to 300 mL of deionized water and stirring to dissolve to obtain an epoxy silane coupling agent hydrolyzate, adding 2 g of hollow mesoporous silica to the epoxy silane coupling agent hydrolyzate, heating to 50° C., stirring to react for 50 min, and centrifugally separating, washing, and drying to obtain coupling agent-modified hollow mesoporous silica;
[0065] S412, add 1 g of coupling agent-modified hollow mesoporous silica into 200 mL of 1.5% polyethyleneimine solution, heat to 80°C, stir and react for 125 min, and obtain modified hollow mesoporous silica after centrifugal separation, washing and drying. Example 3
[0066] A method for preparing granular compound fertilizer by using potassium sulfate co-production intermediates, comprising the following steps:
[0067] S1, adding 60 kg of ammonium sulfate into 90 kg of water and stirring to dissolve to obtain an ammonium sulfate solution, introducing the ammonium sulfate solution into a crystallizer, heating to 48° C., and then adding potassium chloride to the crystallizer under stirring, the mass ratio of ammonium sulfate to potassium chloride being 1:1.3, and keeping the temperature for reaction for 45 minutes to obtain potassium sulfate slurry;
[0068] S2, performing solid-liquid separation on the potassium sulfate slurry to obtain potassium sulfate and potassium ammonium chloride mother liquor;
[0069] S3, filtering the potassium ammonium chloride mother liquor through a ceramic membrane with a pore size of 600 nm to remove solids and obtain a ceramic membrane filtrate;
[0070] S4, subjecting the ceramic membrane filtrate to reverse osmosis membrane concentration treatment to remove most of the water to obtain potassium ammonium chloride concentrate, the reverse osmosis membrane operating pressure is 40 bar, and the temperature is 45°C;
[0071] S5, evaporating and crystallizing the potassium ammonium chloride concentrated solution to obtain potassium ammonium chloride granular compound fertilizer.
[0072] The method for preparing a reverse osmosis membrane comprises the following steps:
[0073] S41, adding 4 g of m-phenylenediamine, 0.05 g of sodium dodecyl sulfate and 0.15 g of triethylamine to 500 mL of deionized water, stirring and dissolving, then adding modified hollow mesoporous silica, the mass ratio of m-phenylenediamine to modified hollow mesoporous silica being 1:0.2, stirring and dispersing uniformly to obtain an aqueous suspension;
[0074] S42, adding 2 g of trimesoyl chloride into 500 mL of n-hexane solvent, heating and stirring to dissolve, to obtain an organic phase solution of trimesoyl chloride;
[0075] S43, immersing the polysulfone-based membrane in an organic phase solution of trimesoyl chloride for 10 minutes, taking it out and placing it in an aqueous phase suspension, reacting it at room temperature for 30 minutes, taking it out and placing it in an oven at 70° C. for curing and cross-linking for 1 hour to obtain a reverse osmosis membrane intermediate;
[0076] S44, adding 2 g of polyethyleneimine, 0.02 g of sodium dodecyl sulfate and 0.1 g of triethylamine to 500 mL of deionized water and stirring to dissolve to obtain a polyethyleneimine aqueous solution;
[0077] S45, immersing the reverse osmosis membrane intermediate in an organic phase solution of trimesoyl chloride for 10 minutes, taking it out and placing it in an aqueous solution of polyethyleneimine, reacting it at room temperature for 15 minutes, taking it out and placing it in an oven for curing and cross-linking at 60° C. for 50 minutes, to obtain a reverse osmosis membrane.
[0078] The preparation method of modified hollow mesoporous silica comprises the following steps:
[0079] S411, adding 0.2 g of epoxy silane coupling agent KH-560 to 300 mL of deionized water and stirring to dissolve to obtain an epoxy silane coupling agent hydrolyzate, adding 2 g of hollow mesoporous silica to the epoxy silane coupling agent hydrolyzate, heating to 50° C., stirring to react for 50 min, and centrifugally separating, washing, and drying to obtain coupling agent-modified hollow mesoporous silica;
[0080] S412, add 1 g of coupling agent-modified hollow mesoporous silica into 200 mL of 1.5% polyethyleneimine solution, heat to 80°C, stir and react for 125 min, and obtain modified hollow mesoporous silica after centrifugal separation, washing and drying. Example 4
[0081] A method for preparing granular compound fertilizer by using potassium sulfate co-production intermediates, comprising the following steps:
[0082] S1, adding 60 kg of ammonium sulfate into 90 kg of water and stirring to dissolve to obtain an ammonium sulfate solution, introducing the ammonium sulfate solution into a crystallizer, heating to 50° C., and then adding potassium chloride to the crystallizer under stirring, the mass ratio of ammonium sulfate to potassium chloride being 1:1.5, and keeping the temperature for reaction for 45 minutes to obtain potassium sulfate slurry;
[0083] S2, performing solid-liquid separation on the potassium sulfate slurry to obtain potassium sulfate and potassium ammonium chloride mother liquor;
[0084] S3, filtering the potassium ammonium chloride mother liquor through a ceramic membrane with a pore size of 800 nm to remove solids and obtain a ceramic membrane filtrate;
[0085] S4, subjecting the ceramic membrane filtrate to reverse osmosis membrane concentration treatment to remove most of the water to obtain potassium ammonium chloride concentrate, the reverse osmosis membrane operating pressure is 40 bar, and the temperature is 45°C;
[0086] S5, evaporating and crystallizing the potassium ammonium chloride concentrated solution to obtain potassium ammonium chloride granular compound fertilizer.
[0087] The method for preparing a reverse osmosis membrane comprises the following steps:
[0088] S41, adding 4 g of m-phenylenediamine, 0.05 g of sodium dodecyl sulfate and 0.15 g of triethylamine to 500 mL of deionized water, stirring and dissolving, then adding modified hollow mesoporous silica, the mass ratio of m-phenylenediamine to modified hollow mesoporous silica being 1:0.3, stirring and dispersing uniformly to obtain an aqueous suspension;
[0089] S42, adding 2 g of trimesoyl chloride into 500 mL of n-hexane solvent, heating and stirring to dissolve, to obtain an organic phase solution of trimesoyl chloride;
[0090] S43, immersing the polysulfone-based membrane in an organic phase solution of trimesoyl chloride for 10 minutes, taking it out and placing it in an aqueous phase suspension, reacting it at room temperature for 30 minutes, taking it out and placing it in an oven at 70° C. for curing and cross-linking for 1 hour to obtain a reverse osmosis membrane intermediate;
[0091] S44, adding 2 g of polyethyleneimine, 0.02 g of sodium dodecyl sulfate and 0.1 g of triethylamine to 500 mL of deionized water and stirring to dissolve to obtain a polyethyleneimine aqueous solution;
[0092] S45, immersing the reverse osmosis membrane intermediate in an organic phase solution of trimesoyl chloride for 10 minutes, taking it out and placing it in an aqueous solution of polyethyleneimine, reacting it at room temperature for 20 minutes, taking it out and placing it in an oven at 60° C. for curing and cross-linking for 50 minutes to obtain a reverse osmosis membrane.
[0093] The preparation method of modified hollow mesoporous silica comprises the following steps:
[0094] S411, adding 0.2 g of epoxy silane coupling agent KH-560 to 300 mL of deionized water and stirring to dissolve to obtain an epoxy silane coupling agent hydrolyzate, adding 2 g of hollow mesoporous silica to the epoxy silane coupling agent hydrolyzate, heating to 50° C., stirring to react for 50 min, and centrifugally separating, washing, and drying to obtain coupling agent-modified hollow mesoporous silica;
[0095] S412, adding 1 g of coupling agent-modified hollow mesoporous silica to 200 mL of 1.5% polyethyleneimine solution, heating to 80°C, stirring the reaction for 135 min, and obtaining modified hollow mesoporous silica after centrifugal separation, washing, and drying. Example 5
[0096] A method for preparing granular compound fertilizer by using potassium sulfate co-production intermediates, comprising the following steps:
[0097] S1, adding 60 kg of ammonium sulfate into 90 kg of water and stirring to dissolve to obtain an ammonium sulfate solution, introducing the ammonium sulfate solution into a crystallizer, heating to 45°C, and then adding potassium chloride to the crystallizer under stirring, the mass ratio of ammonium sulfate to potassium chloride being 1:1.1, and keeping the temperature for reaction for 45 minutes to obtain potassium sulfate slurry;
[0098] S2, performing solid-liquid separation on the potassium sulfate slurry to obtain potassium sulfate and potassium ammonium chloride mother liquor;
[0099] S3, filtering the potassium ammonium chloride mother liquor through a ceramic membrane with a pore size of 500 nm to remove solids and obtain a ceramic membrane filtrate;
[0100] S4, subjecting the ceramic membrane filtrate to reverse osmosis membrane concentration treatment to remove most of the water to obtain potassium ammonium chloride concentrate, the reverse osmosis membrane operating pressure is 40 bar, and the temperature is 45°C;
[0101] S5, evaporating and crystallizing the potassium ammonium chloride concentrated solution to obtain potassium ammonium chloride granular compound fertilizer.
[0102] The method for preparing a reverse osmosis membrane comprises the following steps:
[0103] S41, adding 4 g of m-phenylenediamine, 0.05 g of sodium dodecyl sulfate and 0.15 g of triethylamine to 500 mL of deionized water, stirring and dissolving, then adding modified hollow mesoporous silica, the mass ratio of m-phenylenediamine to modified hollow mesoporous silica being 1:0.1, stirring and dispersing uniformly to obtain an aqueous suspension;
[0104] S42, adding 2 g of trimesoyl chloride into 500 mL of n-hexane solvent, heating and stirring to dissolve, to obtain an organic phase solution of trimesoyl chloride;
[0105] S43, immersing the polysulfone-based membrane in an organic phase solution of trimesoyl chloride for 10 minutes, taking it out and placing it in an aqueous phase suspension, reacting it at room temperature for 30 minutes, taking it out and placing it in an oven at 70° C. for curing and cross-linking for 1 hour to obtain a reverse osmosis membrane intermediate;
[0106] S44, adding 2 g of polyethyleneimine, 0.02 g of sodium dodecyl sulfate and 0.1 g of triethylamine to 500 mL of deionized water and stirring to dissolve to obtain a polyethyleneimine aqueous solution;
[0107] S45, immersing the reverse osmosis membrane intermediate in an organic phase solution of trimesoyl chloride for 10 minutes, taking it out and placing it in an aqueous solution of polyethyleneimine, reacting it at room temperature for 10 minutes, taking it out and placing it in an oven for curing and cross-linking at 60° C. for 50 minutes, to obtain a reverse osmosis membrane.
[0108] The preparation method of modified hollow mesoporous silica comprises the following steps:
[0109] S411, adding 0.2 g of epoxy silane coupling agent KH-560 to 300 mL of deionized water and stirring to dissolve to obtain an epoxy silane coupling agent hydrolyzate, adding 2 g of hollow mesoporous silica to the epoxy silane coupling agent hydrolyzate, heating to 50° C., stirring to react for 50 min, and centrifugally separating, washing, and drying to obtain coupling agent-modified hollow mesoporous silica;
[0110] S412, adding 1 g of coupling agent-modified hollow mesoporous silica to 200 mL of 1.5% polyethyleneimine solution, heating to 80° C., stirring the reaction for 120 min, and obtaining modified hollow mesoporous silica after centrifugal separation, washing, and drying. Comparative Example 1
[0111] The difference between Comparative Example 1 and Example 1 is that:
[0112] In the process of preparing the reverse osmosis membrane, steps S44 and S45 are omitted.
[0113] And no modified hollow mesoporous silica is added in step S41.
[0114] The remaining steps are the same as those in Example 1. Comparative Example 2
[0115] The difference between Comparative Example 2 and Example 1 is:
[0116] In the process of preparing the reverse osmosis membrane, steps S44 and S45 are omitted.
[0117] The remaining steps are the same as those in Example 1. Comparative Example 3
[0118] The difference between Comparative Example 3 and Example 1 is that:
[0119] The modified hollow mesoporous silica added in step S41 is replaced with ordinary hollow mesoporous silica,
[0120] The remaining steps are the same as those in Example 1. Comparative Example 4
[0121] The difference between Comparative Example 4 and Example 4 is that:
[0122] During the preparation of modified hollow mesoporous silica,
[0123] Step S412, stirring reaction time is 136 min.
[0124] The remaining steps are the same as those in Example 4.
[0125] Performance Testing
[0126] 1. Rejection rate of ammonium chloride and potassium chloride by reverse osmosis membrane:
[0127] The retention rate refers to the ratio of the amount of a certain solute retained by the membrane to the total amount, according to R = (1-C p / C f )×100%, where R represents the interception rate (%), C f Indicates the solute concentration in the feed solution (mg / L), C p It indicates the concentration of solute in the permeate (mg / L). Before the reverse osmosis membrane retention performance test, the reverse osmosis membrane was first fixed in the membrane performance evaluation device, the osmotic pressure was adjusted to 10 bar, the reverse osmosis membrane was pre-pressed for 30 minutes, and then ammonium chloride and potassium chloride solutions with a concentration of 1g / L were prepared as the test solution. At a pressure of 40 bar and a temperature of 45°C, the retention rate (%) and water flux (LMH) of the reverse osmosis membrane for ammonium chloride and potassium chloride were tested. The test results are shown in Table 1.
[0128] Table 1:
[0129]
[0130] 2. Membrane stability performance test: fix the reverse osmosis membrane in the membrane performance evaluation device, adjust the osmotic pressure to 10 bar, pre-press the reverse osmosis membrane for 30 minutes, and then prepare a potassium chloride solution with a concentration of 1 g / L as the test solution. Run it continuously at a pressure of 40 bar for 10 h, 20 h, 30 h, 40 h, 50 h, and 60 h, and then test the retention rate (%) of the reverse osmosis membrane for 1 g / L potassium chloride solution. The test results are shown in Table 2.
[0131] Table 2:
[0132]
[0133] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing granular compound fertilizer using potassium sulfate co-production intermediates, characterized in that: The following steps are involved: S1, adding ammonium sulfate into water and stirring to dissolve to obtain an ammonium sulfate solution, introducing the ammonium sulfate solution into a crystallizer, heating it, and then adding potassium chloride into the crystallizer under stirring conditions, keeping the temperature to react, and obtaining potassium sulfate slurry; S2, performing solid-liquid separation on the potassium sulfate slurry to obtain potassium sulfate and potassium ammonium chloride mother liquor; S3, filtering the potassium ammonium chloride mother liquor through a ceramic membrane to remove solids and obtain a ceramic membrane filtrate; S4, subjecting the ceramic membrane filtrate to reverse osmosis membrane concentration treatment to remove most of the water to obtain potassium ammonium chloride concentrate; S5, evaporating and crystallizing the potassium ammonium chloride concentrated solution to obtain potassium ammonium chloride granular compound fertilizer; In step S4, the method for preparing the reverse osmosis membrane comprises the following steps: S41, adding m-phenylenediamine, sodium dodecyl sulfate and triethylamine into deionized water and stirring to dissolve, then adding the modified hollow mesoporous silica and stirring to disperse uniformly to obtain an aqueous suspension; The preparation method of the modified hollow mesoporous silica comprises the following steps: The hollow mesoporous silica is added into the hydrolyzate of the epoxy silane coupling agent, stirred for reaction, and subjected to centrifugal separation, washing, and drying to obtain the coupling agent-modified hollow mesoporous silica; Add the coupling agent modified hollow mesoporous silica into the polyethyleneimine solution, heat to 80°C, stir and react for 120-135 minutes, centrifuge, wash and dry to obtain modified hollow mesoporous silica; S42, adding trimesoyl chloride into n-hexane solvent, heating and stirring to dissolve, to obtain a trimesoyl chloride organic phase solution; S43, immersing the polysulfone-based membrane in an organic phase solution of trimesoyl chloride, taking it out and placing it in an aqueous phase suspension to react at room temperature, taking it out and placing it in an oven for curing and cross-linking to obtain a reverse osmosis membrane intermediate; S44, adding polyethyleneimine, sodium lauryl sulfate and triethylamine into deionized water and stirring to dissolve to obtain a polyethyleneimine aqueous solution; S45, immersing the reverse osmosis membrane intermediate in an organic phase solution of trimesoyl chloride, taking it out and placing it in an aqueous phase solution of polyethyleneimine to react at room temperature, taking it out and placing it in an oven for curing and cross-linking to obtain a reverse osmosis membrane.
2. The method for preparing granular compound fertilizer by using potassium sulfate co-production intermediate according to claim 1, characterized in that: In the step S1, the heating temperature is 45-50°C.
3. The method for preparing granular compound fertilizer by using potassium sulfate co-production intermediate according to claim 1, characterized in that: In step S1, the mass ratio of ammonium sulfate to potassium chloride is 1:1.1-1.
5.
4. The method for preparing granular compound fertilizer by using potassium sulfate co-production intermediate according to claim 1, characterized in that: In step S3, the pore size of the ceramic membrane is 500-800 nm.
5. The method for preparing granular compound fertilizer by using potassium sulfate co-production intermediate according to claim 1, characterized in that: In the step S41, the mass ratio of m-phenylenediamine to modified hollow mesoporous silica is 1:0.1-0.
3.
6. The method for preparing granular compound fertilizer by using potassium sulfate co-production intermediate according to claim 1, characterized in that: In the step S45, the reaction time at room temperature is 10-20 minutes.