Ultra-high performance concrete and preparation method thereof

By using a combination of high-alumina cement, high-temperature-resistant aggregates and fiber materials in concrete, the problem of structural failure of conventional refractory concrete in high-temperature environments above 1500°C is solved, and the effects of high fire resistance and high residual compressive strength are achieved.

CN118771827APending Publication Date: 2024-10-15CHINA WEST CONSTR ACAD OF BUILDING MATERIALS CO LTD +1

Patent Information

Application Number
CN202410798098.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing technology, the cement and aggregate components of conventional refractory concrete cannot adapt to high temperature environments above 1500°C, resulting in heat loss impact and failure of the concrete structure.

Method used

A combination of high-alumina cement, high-temperature-resistant aggregates and fiber materials, including corundum, emery, silicon nitride ceramics and other materials, is used to avoid thermal decomposition and expansion deformation by improving the cement stone-aggregate interface and the high-temperature resistance of the cement stone structure. , forming stable C3A6H3 and AlOH3 phases to improve the thermal stability and compressive strength of concrete.

Benefits of technology

It achieves the high fire resistance and residual compressive strength of concrete in high-temperature environments above 1500°C, ensuring that the structure can still maintain more than 60% of the compressive strength under extremely high temperatures, significantly improving the fire-resistant performance of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004902415350000101
    Figure BDA0004902415350000101
  • Figure BDA0004902415350000111
    Figure BDA0004902415350000111
Patent Text Reader

Abstract

The invention provides ultra-high performance concrete and a preparation method thereof, and relates to the technical field of concrete, the ultra-high performance concrete comprises the following components by weight: 600-800 parts of high alumina cement, 200-400 parts of a mineral admixture, 800-1100 parts of a high temperature resistant aggregate, 100-400 parts of a fiber material, 5-10 parts of a water reducer and 150-250 parts of water; the high-temperature-resistant aggregate comprises at least one of corundum, carborundum or silicon nitride ceramic; the fiber material comprises steel fibers and organic synthetic fibers; the mineral admixture is at least one of fly ash, slag powder, phosphorus slag powder, silica fume or metakaolin. By adopting a full-high-alumina cement system, stable C3A6H3 and Al (OH) 3 phases are formed, so that cement stone structure collapse is avoided. The technical problem that in the prior art, cement and aggregate components in conventional refractory concrete cannot adapt to heat loss impact caused by the high-temperature environment of 1500 DEG C or above is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of concrete, and in particular to an ultra-high performance concrete and a preparation method thereof. Background Art

[0002] Ultra-high performance concrete (UHPC) is a new type of cement-based composite material that has better mechanical properties and durability than ordinary and high-performance concrete. It has been widely used in key engineering projects such as super high-rise buildings, urban transportation, and industrial infrastructure.

[0003] However, in the field of high temperature protection above 1500℃, such as metal smelting and rocket launch, ultra-high performance concrete still needs to make breakthroughs. According to the fire protection requirements of building design, the maximum temperature resistance limit of concrete components is usually 1050℃. In the prior art, the invention patent with publication number CN115784682A discloses a fire-resistant and explosion-resistant ultra-high performance concrete, which has a maximum residual compressive strength of 70MPa after 2 hours at 1050℃, and the strength remains 45%.

[0004] In a high temperature environment above 1500℃, the cement and aggregate components in conventional refractory concrete cannot adapt to the heat loss impact brought by the higher temperature, and will inevitably form defects in any aspect of cement paste, aggregate, and cement paste-aggregate interface, thus causing the concrete structure to fail.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The object of the present invention is to provide an ultra-high performance concrete and a preparation method thereof, so as to at least solve the technical problem in the prior art that the cement and aggregate components in conventional refractory concrete cannot adapt to the heat loss shock caused by a high temperature environment above 1500°C.

[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0008] In a first aspect, the present invention provides an ultra-high performance concrete, comprising the following components in parts by weight: 600-800 parts of high-alumina cement, 200-400 parts of mineral admixture, 800-1100 parts of high-temperature resistant aggregate, 100-400 parts of fiber material, 5-10 parts of water reducer and 150-250 parts of water;

[0009] The high temperature resistant aggregate comprises at least one of corundum, corundum or silicon nitride ceramics;

[0010] The fiber material includes steel fiber and organic synthetic fiber;

[0011] The mineral admixture is at least one of fly ash, slag powder, phosphorus slag powder, microsilica powder or metakaolin.

[0012] Furthermore, the particle size of the high temperature resistant aggregate is fine sand of 20 to 120 meshes.

[0013] Furthermore, the high temperature resistant aggregate also includes fine stone with a particle size of 5 to 10 mm, and the mass ratio of the fine stone to fine sand is less than 0.4.

[0014] Furthermore, the mass ratio of the steel fiber to the organic synthetic fiber is 1.0:(0.1-0.5).

[0015] Furthermore, the refractoriness of the high-alumina cement and the refractoriness of the high-temperature resistant aggregate are both ≥1500°C;

[0016] Preferably, the high alumina cement is selected from CA50 cement or CA60 cement;

[0017] Preferably, the Mohs hardness of the high temperature resistant aggregate is ≥7.0.

[0018] Furthermore, the corundum is at least one of white corundum, brown corundum, and plate-like corundum;

[0019] Preferably, the corundum comprises the following chemical components in mass percentage: Al2O3: >95%, Fe3O2: ≤1.0%;

[0020] Preferably, the corundum comprises the following chemical components in mass percentage: SiC: >95%, Fe3O2: ≤1.0%;

[0021] Preferably, the silicon nitride ceramic comprises the following chemical components in mass percentage: Si3N4: >95%, Fe3O2: ≤1.0%.

[0022] Furthermore, the fiber material has a fiber length of 8 to 30 mm and a fiber diameter of 100 to 600 μm;

[0023] Preferably, the organic synthetic fiber includes at least one of polyacrylonitrile fiber, polyoxymethylene fiber, and polyvinyl alcohol fiber;

[0024] Preferably, the base material tensile strength of the steel fiber is greater than 1000 MPa, and the elastic modulus is greater than 180 GPa;

[0025] Preferably, the melting point of the organic synthetic fiber is ≤200°C and the carbon content is <60%;

[0026] Preferably, the 28-day strength activity index of the mineral admixture is not less than 80%.

[0027] Furthermore, the water reducing agent includes a defoaming component and a retarding component, wherein the defoaming component includes at least one of alcohols, silicones or phosphates, and the retarding component includes at least one of borax, sodium fluorosilicate, citric acid or sugars.

[0028] Preferably, the amount of the defoaming component added is (2-8) / 1000 of the total mass of the water reducer; the amount of the retarding component added is (2-8) / 1000 of the total mass of the water reducer;

[0029] Preferably, the water reducing agent has a water reducing rate of not less than 30%.

[0030] Furthermore, the refractoriness of the ultra-high performance concrete is ≥1500°C, and the residual compressive strength ratio after being subjected to a high temperature of 1500°C for 2 hours is ≥60%.

[0031] In a second aspect, the present invention provides a method for preparing the above-mentioned ultra-high performance concrete, comprising the following steps:

[0032] A. Weigh high alumina cement, mineral admixture, and high temperature resistant aggregate, mix and stir to obtain a dry mix;

[0033] B. Weigh the water reducer and water and add them to the dry mix, and continue stirring until a fluid material is formed;

[0034] C. Weigh the fiber material, add it evenly and slowly into the fluid material and stir it thoroughly to make the fiber evenly dispersed to obtain ultra-high performance concrete.

[0035] The present invention provides an ultra-high performance concrete and a preparation method thereof. By adopting a full high-alumina cement system, it is different from silicate cement. Its hydration products are mainly hydrated calcium aluminate and aluminum gel phase, without CaOH2. In the medium temperature section, the crystal transformation of hydrated calcium aluminate replaces the thermal decomposition of CaOH2 in silicate cement, and forms stable C3A6H3 and AlOH3 phases, so that the cement stone structure will not collapse. It solves the problem in the prior art that when concrete is in the medium temperature section (600-1000°C), the hydration products will decompose in large quantities (Ca(OH)2-CaO, CSH-silicon dehydrated phase), causing the cement stone and the cement stone aggregate interface to crack, resulting in structural failure, and therefore unable to resist thermal damage at higher temperatures. By further limiting the technical parameters of organic fiber in improving the high temperature resistance of concrete, it is avoided that high ignition loss organic fiber is difficult to form a complete microporous channel in concrete, thereby failing to achieve the ideal vapor pressure release effect.

[0036] High-alumina cement is used as a cementitious material, and fly ash, slag powder, phosphorus slag powder, microsilica powder, kaolin and other high-activity mineral admixtures with volcanic ash activity are used to replace part of the cement to compensate for the strength loss and volume shrinkage caused by the crystal transformation in the medium temperature range of 600-1000 degrees, and improve the thermal stability of cement stone. Secondly, steel fiber and organic fiber are used to compositely strengthen the cement stone-aggregate interface, and the ability of the cement stone-aggregate interface to resist high-temperature thermal damage is improved through fiber selection and multi-fiber mixing ratio optimization. Finally, refractory aggregates such as corundum, corundum, and silicon nitride ceramics are used to replace conventional aggregates. With the advantages of high melting point, high hardness, and stable composition at high temperature, the structural damage caused by thermal decomposition and expansion deformation of conventional aggregates in the medium and high temperature range is avoided. Through the mutual constraints, complementary advantages, and synergistic efficiency of the above three aspects, an ideal gain effect is achieved. It further solves the technical problem that the cement and aggregate components in conventional refractory concrete cannot adapt to the heat loss impact caused by the high temperature environment above 1500℃. DETAILED DESCRIPTION

[0037] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0038] The methods and techniques of the present invention are generally performed according to conventional methods well known in the art and as described in various general and more specific references that are cited and discussed throughout the present specification unless otherwise indicated.

[0039] In order for concrete to be able to withstand high temperatures of 1000 degrees or even above 1500 degrees, it is necessary to work on the three aspects of concrete: cement stone, aggregate, and cement stone-aggregate interface. None of them can be missing. If any one of them is insufficient, it will lead to structural defects in the concrete and bring the risk of high-temperature bursting.

[0040] The present invention provides an ultra-high performance concrete, comprising the following components in parts by weight: 600-800 parts of high-alumina cement, 200-400 parts of mineral admixtures, 800-1100 parts of high-temperature resistant aggregates, 100-400 parts of fiber materials, 5-10 parts of water reducing agents, and 150-250 parts of water;

[0041] The high temperature resistant aggregate comprises at least one of corundum, corundum or silicon nitride ceramics;

[0042] The fiber material includes steel fiber and organic synthetic fiber;

[0043] The mineral admixture is at least one of fly ash, slag powder, phosphorus slag powder, microsilica powder or metakaolin.

[0044] By adopting a full high-alumina cement system, which is different from silicate cement, its hydration products are mainly hydrated calcium aluminate and aluminum gel phase, without CaOH2. In the medium temperature range, the crystal transformation of hydrated calcium aluminate replaces the thermal decomposition of CaOH2 in silicate cement, and forms stable C3A6H3 and AlOH3 phases, so the cement stone structure will not collapse. This solves the problem in the prior art that when concrete is in the medium temperature range (600-1000℃), the hydration products will decompose in large quantities (Ca(OH)2-CaO, CSH-silicon oxide dehydrated phase), causing the cement stone and the cement stone aggregate interface to crack, resulting in structural failure, and therefore unable to resist thermal damage at higher temperatures.

[0045] On this basis, when the temperature is above 1000 degrees, the high-alumina cement product undergoes a sintering reaction to produce ceramic bonding, showing higher strength and refractoriness.

[0046] By further limiting the technical parameters of organic fibers in improving the high temperature resistance of concrete, it is avoided that high ignition loss organic fibers are difficult to form complete microporous channels in concrete, thereby failing to achieve the ideal vapor pressure release effect.

[0047] The present invention utilizes high-alumina cement as a cementitious material, and cooperates with fly ash, slag powder, phosphorus slag powder, microsilica powder, metakaolin and other high-activity mineral admixtures with volcanic ash activity to replace part of the cement, so as to compensate for the strength loss and volume shrinkage caused by the crystal transformation in the medium temperature section of 600 to 1000 degrees, and improve the thermal stability of cement stone. Secondly, steel fiber and organic fiber are compositely strengthened to strengthen the cement stone-aggregate interface, and the ability of the cement stone-aggregate interface to resist high-temperature thermal damage is improved by optimizing the fiber selection and multi-fiber mixing ratio. Finally, refractory aggregates such as corundum, corundum, silicon nitride ceramics are used to replace conventional aggregates. With the advantages of high melting point, high hardness, and stable composition at high temperature, the structural damage caused by thermal decomposition and expansion deformation of conventional aggregates in the medium and high temperature sections is avoided. Through the mutual constraints, complementary advantages, and synergistic synergy of the above three aspects, an ideal gain effect is achieved.

[0048] This further solves the technical problem that the cement and aggregate components in conventional refractory concrete cannot adapt to the heat loss impact caused by a high temperature environment above 1500°C.

[0049] In some specific implementations, the particle size of the high temperature resistant aggregate is fine sand of 20 to 120 meshes.

[0050] In some specific implementations, the high temperature resistant aggregate further comprises fine stones with a particle size of 5 to 10 mm, and the mass ratio of the fine stones to fine sand is less than 0.4.

[0051] In some specific embodiments, the mass ratio of the steel fiber to the organic synthetic fiber is 1.0:(0.1-0.5).

[0052] In some specific embodiments, the refractoriness of the high alumina cement and the refractoriness of the high temperature resistant aggregate are both ≥1500°C;

[0053] Preferably, the high alumina cement is selected from CA50 cement or CA60 cement;

[0054] Preferably, the Mohs hardness of the high temperature resistant aggregate is ≥7.0.

[0055] In some specific embodiments, the corundum is at least one of white corundum, brown corundum, and plate-like corundum;

[0056] Preferably, the corundum comprises the following chemical components in mass percentage: Al2O3: >95%, Fe3O2: ≤1.0%;

[0057] Preferably, the corundum comprises the following chemical components in mass percentage: SiC: >95%, Fe3O2: ≤1.0%;

[0058] Preferably, the silicon nitride ceramic comprises the following chemical components in mass percentage: Si3N4: >95%, Fe3O2: ≤1.0%.

[0059] From the perspective of improving aggregates, quartz sand aggregates expand in volume due to phase change in the medium temperature range of 600-1000 degrees, causing damage to the cement stone-aggregate interface. The Fe3O2 content in brown corundum and silicon carbide materials affects the melting point of the materials themselves. By selecting corundum, corundum and silicon nitride ceramics with Fe3O2: ≤1.0% as high-temperature resistant aggregates, the decline in refractory performance due to high Fe3O2 content can be avoided.

[0060] In some specific embodiments, the fiber material has a fiber length of 8 to 30 mm and a fiber diameter of 100 to 600 μm;

[0061] Preferably, the organic synthetic fiber includes at least one of polyacrylonitrile fiber, polyoxymethylene fiber, and polyvinyl alcohol fiber;

[0062] Preferably, the base material tensile strength of the steel fiber is greater than 1000 MPa, and the elastic modulus is greater than 180 GPa;

[0063] Preferably, the melting point of the organic synthetic fiber is ≤200°C and the carbon content is <60%;

[0064] Preferably, the 28-day strength activity index of the mineral admixture is not less than 80%.

[0065] In some specific embodiments, the water reducer includes a defoaming component and a retarding component, the defoaming component includes at least one of alcohols, silicones or phosphates, and the retarding component includes at least one of borax, sodium fluorosilicate, citric acid or sugars.

[0066] Preferably, the amount of the defoaming component added is (2-8) / 1000 of the total mass of the water reducer; the amount of the retarding component added is (2-8) / 1000 of the total mass of the water reducer;

[0067] Preferably, the water reducing agent has a water reducing rate of not less than 30%.

[0068] In some specific implementations, the refractoriness of the ultra-high performance concrete is ≥1500°C, and the residual compressive strength ratio after being subjected to a high temperature of 1500°C for 2 hours is ≥60%.

[0069] Another aspect of the present invention further provides a method for preparing the above-mentioned ultra-high performance concrete, comprising the following steps:

[0070] A. Weigh high alumina cement, mineral admixture, and high temperature resistant aggregate, mix and stir to obtain a dry mix;

[0071] B. Weigh the water reducer and water and add them to the dry mix, and continue stirring until a fluid material is formed;

[0072] C. Weigh the fiber material, add it evenly and slowly into the fluid material and stir it thoroughly to make the fiber evenly dispersed to obtain ultra-high performance concrete.

[0073] Ultra-high performance concrete proposes a preparation method for high-temperature resistant ultra-high performance concrete from four dimensions: cementitious materials, aggregates, fiber materials, and admixtures. ① The technical parameters of cement and mineral admixtures such as refractoriness and activity are refined, and a reasonable cementitious material composition formula is proposed; ② The technical parameters of organic fiber such as loss on ignition and melting point are refined, and the composition ratio of organic fiber and steel fiber is optimized, thereby improving the cement stone-matrix interface characteristics in concrete and exerting an ideal toughening and pressure relief effect; ③ High-hardness and high-melting-point corundum, corundum, and silicon carbide ceramics are selected to replace traditional aggregates, and through reasonable aggregate grading specifications and dosage design, a good compatibility is formed between cement, mineral admixtures, and fiber materials to optimize the pore structure of the concrete matrix; ④ In view of the fact that high-alumina cement sets and hardens too quickly and fiber materials are difficult to disperse during mixing, retarding and defoaming components are selected, the composition of water reducer is optimized, the setting time and microscopic pore structure of concrete are directional controlled, and the construction and mechanical properties of concrete are improved.

[0074] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0075] Example 1

[0076] An ultra-high performance concrete comprises the following components in parts by weight: 600 parts of high-alumina cement, 400 parts of mineral admixture (all fly ash), 1000 parts of high temperature resistant aggregate (all corundum, 5-10 mm fine sand and 20-120 mesh sand powder mass ratio of 0.4:1.0), 300 parts of fiber material (steel fiber + polyacrylonitrile fiber, mass ratio of 10:1). The ultra-high performance concrete is prepared according to the following steps:

[0077] A. Weigh high alumina cement, mineral admixture, and high temperature resistant aggregate according to weight fractions, mix and stir to obtain a dry mix;

[0078] B. Weigh the water reducer and water according to the weight fraction and add them to the dry mix, and continue stirring until a fluid material is formed;

[0079] C. Weigh the fiber material according to the weight fraction, add it evenly and slowly into the fluid material and stir it thoroughly to make the fiber evenly dispersed, thus obtaining ultra-high performance concrete.

[0080] Example 2

[0081] Different from Example 1, the high temperature resistant aggregate is composed of corundum and corundum, the mass ratio of corundum to corundum is 1:1, and the mass ratio of 5-10 mm fine sand to 20-120 mesh sand powder is 0.4:1.0.

[0082] Example 3

[0083] Different from Example 1, the high temperature resistant aggregate is composed of corundum and silicon nitride ceramics, the mass ratio of corundum to silicon nitride ceramics is 1:1, and the mass ratio of 5-10 mm fine sand to 20-120 mesh sand powder is 0.4:1.0.

[0084] Example 4

[0085] The difference from Example 1 is that 300 parts of fiber material (steel fiber+polyacrylonitrile fiber, mass ratio 10:3).

[0086] Example 5

[0087] Different from Example 1, the particle size of the high temperature resistant aggregate is fine sand powder of 20 to 120 meshes.

[0088] Example 6

[0089] The difference from Example 1 is that the polyacrylonitrile fiber is replaced by polyoxymethylene fiber.

[0090] Example 7

[0091] Different from Example 1, the polyacrylonitrile fiber is replaced by polyoxymethylene fiber and polyvinyl alcohol fiber, and the mass ratio of the polyoxymethylene fiber to the polyvinyl alcohol fiber is 1:1.

[0092] Example 8

[0093] An ultra-high performance concrete comprises the following components in parts by weight: 800 parts of high-alumina cement, 200 parts of mineral admixtures (all fly ash), 1000 parts of high-temperature resistant aggregates (corundum + corundum, half corundum and half corundum, and a mass ratio of 5-10 mm fine sand to 20-120 mesh sand powder of 0.4:1.0), and 300 parts of fiber materials (steel fiber + polyacrylonitrile fiber, mass ratio of 10:1).

[0094] Example 9

[0095] The difference from Example 8 is that the fiber material is 100 parts.

[0096] Example 10

[0097] The difference from Example 8 is that the fiber material is 400 parts.

[0098] Embodiment 11

[0099] Different from Example 8, the mineral admixture consists of fly ash and microsilica, and the mass ratio of fly ash to microsilica is 3:1.

[0100] Example 12

[0101] Different from Example 8, the mineral admixture consists of fly ash and slag powder, and the mass ratio of fly ash to slag powder is 1:1.

[0102] Embodiment 13

[0103] Different from Example 8, the mineral admixture consists of fly ash, phosphorus slag powder and metakaolin, and the mass ratio of fly ash, phosphorus slag powder and metakaolin is 3:1:1.

[0104] Embodiment 14

[0105] An ultra-high performance concrete comprises the following components in parts by weight: 800 parts of high-alumina cement, 200 parts of mineral admixture (composed of fly ash and microsilica powder, with a mass ratio of 3:1), 800 parts of high-temperature resistant aggregate (corundum + corundum, half corundum and half corundum, and a mass ratio of 5-10 mm fine sand to 20-120 mesh sand powder of 0.4:1.0), and 300 parts of fiber material (steel fiber + polyacrylonitrile fiber, with a mass ratio of 10:2).

[0106] Comparative Example 1

[0107] The difference from Example 1 is that the polyacrylonitrile fiber is removed.

[0108] Comparative Example 2

[0109] The difference from Example 1 is that 300 parts of high alumina cement are replaced by 300 parts of Portland cement.

[0110] Comparative Example 3

[0111] Different from Example 1, the mineral admixture is entirely fly ash, and the activity after 28 days is only 60%.

[0112] Comparative Example 4

[0113] Different from Example 1, the carbon content of the polypropylene fiber exceeds 85%.

[0114] Comparative Example 5

[0115] The difference from Example 1 is that the corundum is replaced by quartz sand.

[0116] Test 1 Concrete performance test

[0117] In this test, the properties of the concrete of Examples 1 to 14 and Comparative Examples 1 to 5 were tested respectively according to the following methods.

[0118] Refractoriness of concrete: After concrete is formed, the refractoriness test is carried out according to the relevant methods in GB / T 7322 "Test methods for refractoriness of refractory materials".

[0119] High temperature test of concrete: According to the embodiment method in CN202211403236 "A fire-resistant and explosion-resistant ultra-high performance concrete and its preparation method", the prepared concrete is placed in a muffle furnace, heated to 1500°C or above, and maintained at a constant temperature for 2 hours. After the furnace cools to room temperature, a residual compressive strength test is carried out. The residual compressive strength ratio is the ratio of the remaining compressive strength after high temperature to the compressive strength before high temperature.

[0120] Concrete wear test: After the concrete is formed, the wear per unit area is tested according to the relevant methods of GB / T 12988 "Test method for wear resistance of inorganic floor materials".

[0121] Table 1 Test results of different concrete properties

[0122]

[0123]

[0124] The specific results are shown in Table 1. It can be seen that the refractoriness of the UHPC prepared in Examples 1 to 14 all reached above 1500°C, and the residual compressive strength after the 1500°C high temperature test was not less than 65%, proving that the UHPC proposed in the present invention has excellent refractoriness in an extremely high temperature environment of 1500°C.

[0125] Due to differences in formulation and raw materials, the performance of each group may vary.

[0126] Comparison of Examples 1 to 3 revealed that the composition differences of high temperature resistant aggregates have a certain influence on the residual compressive strength and refractoriness of UHPC after high temperature. Compared with the single corundum aggregate system, the corundum-carborundum composite aggregate system has more advantages in terms of compressive strength and wear resistance of UHPC after high temperature, and the refractoriness of the corundum-silicon nitride ceramic aggregate system has a relative deviation.

[0127] Comparison between Examples 1 and 4 revealed that the amount of organic fiber added had a significant effect on the refractoriness of UHPC. As the range of organic fiber addition increased, the residual compressive strength and refractoriness of UHPC after high temperature were further improved. At the same time, the unit wear amount increased and the wear resistance decreased slightly.

[0128] The components of Example 5 do not contain 5-10 mm fine stones. Compared with Example 1, the structure becomes more compact and has an advantage in compressive strength, but has not yet had an effect on improving refractoriness.

[0129] In Examples 6 and 7, compared with Example 1, the type of organic fiber is changed. The organic fiber with polyoxymethylene fiber as the main body further enhances the refractoriness of UHPC, and the refractoriness reaches above 1800°C. This is because polyoxymethylene fiber and polyvinyl alcohol fiber have a lower carbon content than polyacrylonitrile, and the proportion of pore transport channels formed after melting in UHPC at high temperature is higher, which greatly reduces the loss of UHPC caused by thermal stress and vapor pressure at high temperature.

[0130] Comparison of Examples 8 to 10 and Example 2 shows that the increase in the amount of high-alumina cement and the amount of fiber material have a significant effect on the compressive strength and refractoriness of UHPC. The residual compressive strength and refractoriness of UHPC after high temperature are further improved with a high amount of fiber material.

[0131] Comparison of Examples 11 to 13 and 2 shows that the change in the type of mineral admixtures affects the mechanical strength, wear resistance and refractoriness of UHPC before and after high temperature. The residual compressive strength after high temperature of the fly ash + phosphorus slag powder + metakaolin composite mineral admixture system is more advantageous, but the unit wear amount increases slightly, the wear resistance deteriorates, and the refractoriness increases slightly.

[0132] Example 14 formed a UHPC with a compressive strength exceeding 200 MPa, and exhibited better performance in terms of 28-day cumulative wear, residual compressive strength after high temperature, and refractoriness.

[0133] Compared with Example 1, the fiber material composition of Comparative Example 1 only includes steel fibers. It is found through experiments that the residual compressive strength ratio after high temperature is only 43%, and the measured refractoriness is 800°C, which illustrates the importance of organic fibers in the preparation of high temperature resistant UHPC. The residual compressive strength of Comparative Example 1 is greatly lost after high temperature, and the refractoriness is obviously lower than that of Example 1. The lack of organic fibers prevents UHPC from forming mesoscopic channels at high temperatures, and the huge thermal stress and hot steam pressure cause damage to the concrete structure.

[0134] Comparative Example 2, compared with Example 1, uses a composite cement system of silicate cement + high alumina cement. In a special high temperature environment of 1500°C, the fire resistance of the concrete is not good.

[0135] In Comparative Example 3, compared with Example 1, the mineral admixture used is fly ash whose activity does not meet the standard (the 28-day activity index is only 60%). The test found that the 28-day compressive strength, residual compressive strength after high temperature and refractoriness of Comparative Example 3 are all lower than those of Example 1, indicating that the difference in admixture quality also has a significant impact on the strength and refractoriness of UHPC.

[0136] The organic fiber used in Comparative Example 4 is polypropylene fiber, which has a carbon content 30% higher than that of the acrylonitrile fiber in Example 1. Therefore, the microscopic pore channel rate formed under the same conditions is lower than that in Example 1, and the measured residual compressive strength and refractoriness are smaller, showing worse fire resistance.

[0137] Comparative Example 5 uses ordinary quartz sand aggregate. Compared with Example 1, the ordinary aggregate is burned and broken and the structure is destroyed in the special high temperature environment of 1500°C. Therefore, the compressive strength after high temperature cannot be measured, and the refractoriness is only 400°C. This shows the importance of high temperature resistant aggregates such as corundum, corundum, silicon nitride ceramics, etc. in the preparation of UHPC to resist the extremely high temperature environment of 1500°C.

[0138] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An ultra-high performance concrete, characterized in that: The invention comprises the following components in parts by weight: 600-800 parts of high-alumina cement, 200-400 parts of mineral admixture, 800-1100 parts of high-temperature resistant aggregate, 100-400 parts of fiber material, 5-10 parts of water reducing agent and 150-250 parts of water; The high temperature resistant aggregate comprises at least one of corundum, corundum or silicon nitride ceramics; The fiber material includes steel fiber and organic synthetic fiber; The mineral admixture is at least one of fly ash, slag powder, phosphorus slag powder, microsilica powder or metakaolin.

2. The ultra-high performance concrete according to claim 1, characterized in that: The particle size of the high temperature resistant aggregate is fine sand of 20 to 120 meshes.

3. The ultra-high performance concrete according to claim 2, characterized in that: The high temperature resistant aggregate also includes fine stones with a particle size of 5 to 10 mm, and the mass ratio of the fine stones to fine sand is less than 0.

4.

4. The ultra-high performance concrete according to claim 1, characterized in that: The mass ratio of the steel fiber to the organic synthetic fiber is 1.0:(0.1-0.5).

5. The ultra-high performance concrete according to claim 1, characterized in that: The refractoriness of the high alumina cement and the refractoriness of the high temperature resistant aggregate are both ≥1500°C; Preferably, the high alumina cement is selected from CA50 cement or CA60 cement; Preferably, the Mohs hardness of the high temperature resistant aggregate is ≥7.

0.

6. The ultra-high performance concrete according to claim 1, characterized in that: The corundum is at least one of white corundum, brown corundum and plate-like corundum; Preferably, the corundum comprises the following chemical components in mass percentage: Al2O3: >95%, Fe3O2: ≤1.0%; Preferably, the corundum comprises the following chemical components in mass percentage: SiC: >95%, Fe3O2: ≤1.0%; Preferably, the silicon nitride ceramic comprises the following chemical components in mass percentage: Si3N4: >95%, Fe3O2: ≤1.0%.

7. The ultra-high performance concrete according to claim 1, characterized in that: The fiber material has a fiber length of 8 to 30 mm and a fiber diameter of 100 to 600 μm; Preferably, the organic synthetic fiber includes at least one of polyacrylonitrile fiber, polyoxymethylene fiber, and polyvinyl alcohol fiber; Preferably, the base material tensile strength of the steel fiber is greater than 1000 MPa, and the elastic modulus is greater than 180 GPa; Preferably, the melting point of the organic synthetic fiber is ≤200°C and the carbon content is <60%; Preferably, the 28-day strength activity index of the mineral admixture is not less than 80%.

8. The ultra-high performance concrete according to claim 1, characterized in that: The water reducing agent comprises a defoaming component and a retarding component, wherein the defoaming component comprises at least one of alcohols, silicones or phosphates, and the retarding component comprises at least one of borax, sodium fluorosilicate, citric acid or sugars. Preferably, the amount of the defoaming component added is (2-8) / 1000 of the total mass of the water reducer; the amount of the retarding component added is (2-8) / 1000 of the total mass of the water reducer; Preferably, the water reducing agent has a water reducing rate of not less than 30%.

9. The ultra-high performance concrete according to any one of claims 1 to 8, characterized in that: The ultra-high performance concrete has a refractoriness of ≥1500°C, and a residual compressive strength ratio of ≥60% after being subjected to a high temperature of 1500°C for 2 hours.

10. The method for preparing ultra-high performance concrete according to any one of claims 1 to 9, characterized in that: The following steps are involved: A. Weigh high alumina cement, mineral admixture, and high temperature resistant aggregate, mix and stir to obtain a dry mix; B. Weigh the water reducer and water and add them to the dry mix, and continue stirring until a fluid material is formed; C. Weigh the fiber material, add it evenly and slowly into the fluid material and stir it thoroughly to make the fiber evenly dispersed to obtain ultra-high performance concrete.

Citation Information

Patent Citations

  • Fireproof and antiknock ultra-high performance concrete and preparation method thereof

    CN115784682A

  • Wear-resisting castable refractory

    CN102491770A

  • Nano-carbon-containing refractory castable for desulfurization stirrer and preparation method of nano-carbon-containing refractory castable

    CN111689783A

  • Special high-strength corundum castable and preparation method thereof

    CN114149271A

  • Use of a fibre cement composition for manufactured products withstanding thermal shocks

    FR2702209A1

Cited By

  • Mining high-temperature-resistant sealing material