Preparation method of high-strength ardealite-based road functional aggregate
By combining polyurethane solid-solid phase change materials with high-strength phosphogypsum base road aggregates, the problems of low phosphogypsum utilization and road temperature damage are solved, and the resource utilization of phosphogypsum and road temperature regulation are realized, meeting the needs of Demand for road aggregates.
Patent Information
- Application Number
- CN202410845953.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The comprehensive utilization rate of phosphogypsum is low, resulting in environmental pollution and resource waste. At the same time, road temperature diseases are serious problems in road construction and use. A material that can effectively prevent and reduce these diseases is needed.
Polyurethane solid-solid phase change material (PUSSP) is combined with high-strength phosphogypsum base road aggregate, and the heat storage energy of polyurethane solid-solid phase change material is used to reduce road temperature fluctuations, combined with the resource utilization of phosphogypsum, to prepare Functional aggregate for high-strength phosphogypsum base road.
It realizes the resource utilization of phosphogypsum, reduces the occurrence and expansion of road temperature diseases, meets the demand for road aggregates, and provides a widely applicable temperature regulation effect through phase stability and heat storage characteristics.
Smart Images

Figure BDA0004915701310000131 
Figure BDA0004915701310000132 
Figure BDA0004915701310000133
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a high-strength phosphogypsum-based functional aggregate for roads, belonging to the technical field of engineering materials and preparation. Background Art
[0002] Phosphogypsum is a byproduct of wet phosphoric acid production and one of the largest solid wastes in the chemical industry. For every ton of phosphate fertilizer produced, an average of 3.75 tons of phosphogypsum is produced. At present, the annual emission of phosphogypsum in the world reaches 280 million tons, and my country has exceeded 50 million tons, accounting for more than 70% of industrial by-product gypsum, while the comprehensive utilization rate of phosphogypsum is less than 40%. At present, most phosphogypsum is treated by open-air stacking. Phosphogypsum contains a large amount of harmful substances, which not only occupies a large amount of land resources, but also pollutes our living environment. Using phosphogypsum to prepare building materials, roadbed materials and goaf filling materials in mining areas is one of the main ways to quickly and rapidly consume phosphogypsum on a large scale. However, when phosphogypsum is used in powder form, there are problems such as low utilization rate and difficult transportation.
[0003] Road temperature damage refers to various road damages caused by temperature changes during road construction and use. The causes, types and characteristics of such damages are closely related to temperature changes. The following is a detailed analysis of road temperature damages:
[0004] 1. Causes
[0005] Temperature drop: In cold winter, the temperature drop will cause low-temperature shrinkage and cracking of road materials (especially asphalt concrete). This shrinkage deformation causes the bottom surface of the surface layer to bear tensile force. When the tensile force exceeds the tensile strength of the asphalt surface layer, the bottom of the asphalt surface layer will crack.
[0006] Temperature cyclic changes: Cyclic changes in temperature and humidity and the repeated effects of vehicle loads will accelerate the expansion and formation of cracks.
[0007] 2. Types
[0008] Cracks: Cracks are the most common type of road temperature damage. There are many types of cracks, including block cracks, irregular cracks, longitudinal cracks, transverse cracks, etc. Among them, transverse cracks are mainly caused by low-temperature shrinkage cracking caused by a sudden drop in temperature, while longitudinal cracks may be related to the large temperature difference at the joints of the front and rear paving.
[0009] Potholes: Based on cracks, the intrusion of water and the action of vehicle loads may cause the asphalt aggregate of the road surface to fall off and form potholes.
[0010] Rutting: When the temperature is high, the softness and creep characteristics of the asphalt mixture will cause grooves to form on the road surface under the repeated rolling of vehicles, and gradually take shape over time.
[0011] 3. Features
[0012] Seasonality: Road temperature diseases often have obvious seasonal characteristics, especially in winter and spring. Due to large temperature changes, the probability of occurrence of such diseases will also increase accordingly.
[0013] Recurrence: Once cracks and other defects are formed, if they are not repaired and treated promptly and effectively, the defects will continue to expand and worsen over time, and may even form a vicious cycle.
[0014] In summary, road temperature damage is one of the inevitable problems in the process of road construction and use. How to choose appropriate road materials to effectively prevent and reduce the occurrence and expansion of road temperature damage is an urgent issue to be solved. Summary of the invention
[0015] The technical problem to be solved by the present invention is to provide a method for preparing high-strength phosphogypsum-based functional aggregate for roads, combining the comprehensive resource utilization of solid waste from wet phosphoric acid production with the alleviation of road temperature damage.
[0016] The present invention is realized by the following scheme: a method for preparing high-strength phosphogypsum-based functional aggregate for roads, wherein a polyurethane solid-solid phase change material (PUSSP) is loaded on the high-strength phosphogypsum-based aggregate for roads.
[0017] The polyurethane solid-solid phase change material (PUSSP) is synthesized from methylene diphenyl diisocyanate (MDI, 98% analytically pure) as a hard segment, polyethylene glycol 4000 (PEG4000, 98% analytically pure) as a soft segment, and 1,4-butanediol (BDO, 98% analytically pure) as a chain extender, and the solution used in the synthesis process is N,N-dimethylformamide dimethyl acetal (DMF, 98% analytically pure).
[0018] The preparation process of the polyurethane solid-solid phase change material (PUSSP) is as follows: weighed methylene diphenyl diisocyanate and polyethylene glycol are put into an oven to melt into a liquid state, and then N, N-dimethylformamide dimethyl acetal is mixed into the liquid methylene diphenyl diisocyanate and polyethylene glycol, and then stirred in an 80° C. oil bath for 3 hours, and then 1, 4-butanediol solution is added and stirred for 2 hours, and the obtained reactant is placed in a 90° C. oven for 48 hours to remove N, N-dimethylformamide dimethyl acetal.
[0019] During the synthesis of the polyurethane solid-solid phase change material (PUSSP), nitrogen is introduced as a protective gas.
[0020] A method for preparing a high-strength phosphogypsum-based functional aggregate for a road, wherein the preparation process is carried out according to the following steps:
[0021] Step 1: pretreating phosphogypsum;
[0022] Step 2: grind the prepared polyurethane solid-solid phase change material into powder, the grinding time is 10 minutes, and the particle size is controlled to be less than 1 mm;
[0023] Step 3: Mix the polyurethane solid-solid phase change material with the phosphogypsum powder, fix the dosage to 10%, and fully grind and mix them for 30 minutes to evenly load the polyurethane solid-solid phase change material on the phosphogypsum powder;
[0024] Step 4: Add the phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash and silica fume loaded with polyurethane solid-solid phase change material into a mixer and mix for 60 to 120 seconds, then add the remaining slurry of the pipe pile and mix for 40 to 60 seconds; add water during the mixing process until the materials are evenly mixed;
[0025] Step 5, adding the mixed material of step 2 into a granulator and forming by pressure;
[0026] Step six: carbonizing and curing the prepared aggregate.
[0027] The pretreatment method of phosphogypsum in step 1 is: drying the phosphogypsum, cooling and aging for 24 to 48 hours, the drying temperature of the phosphogypsum drying treatment is 120° C. to 180° C., and the drying time is 4 to 8 hours.
[0028] The amount of water added in step 4 is 25% to 40% of the total amount of dry raw materials.
[0029] The ring die compression ratio of the granulator in step 5 is 2.5 to 6.5;
[0030] The carbonization curing conditions of step six are as follows: curing temperature: 20°C to 55°C, CO2 gas concentration 20% to 90%, CO2 gas pressure 0.1MPa to 0.6MPa, curing time 1 to 7 days, relative humidity of the curing room during the curing period 40% to 80%, after carbonization curing, the aggregate is placed in a stockpile and sprayed with water regularly for natural curing for 21 to 28 days.
[0031] The components of the high-strength phosphogypsum-based road aggregate include phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash, silica ash, and pipe pile slurry. The percentage of each component is: phosphogypsum 50% to 95%, slag powder 3% to 25%, cement clinker 0.5% to 15%, steel slag powder 0.5% to 10%, fly ash 0.5% to 10%, and silica ash 0.5% to 10%. The pipe pile slurry is 25% to 35% of the dry material weight of the mixture of phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash, and silica ash.
[0032] The beneficial effects of the present invention are:
[0033] 1. The polyurethane solid-solid phase change material of the present invention can spontaneously reduce the adverse effects of temperature on roads by storing heat energy. At the same time, the phosphogypsum-based road aggregate can be used as a support to meet the demand for road aggregate, which is conducive to promoting the comprehensive resource utilization of solid waste from wet phosphoric acid production and the reduction of road temperature diseases;
[0034] 2. The polyurethane solid-solid phase change material prepared by the present invention has good phase stability, no leakage occurs during the entire phase change heat storage process, and the phase change behavior is from solid to solid, which is widely applicable to road temperature control in my country. DETAILED DESCRIPTION
[0035] The present invention is further described below, but the protection scope of the present invention is not limited to the described contents.
[0036] For the sake of clarity, not all features of an actual embodiment are described. In the following description, well-known functions and structures are not described in detail because they would obscure the invention with unnecessary detail. It should be recognized that in the development of any actual embodiment, a large number of implementation details must be made to achieve the specific goals of the developer, such as changing from one embodiment to another according to relevant system or relevant business limitations. In addition, it should be recognized that such development work may be complex and time-consuming, but it is merely routine work for those skilled in the art.
[0037] The preparation process of polyurethane solid-solid phase change material (PUSSP) is as follows: weighed methylene diphenyl diisocyanate and polyethylene glycol are placed in an oven to melt into liquid, then N, N-dimethylformamide dimethyl acetal is mixed into the liquid methylene diphenyl diisocyanate and polyethylene glycol and stirred in an 80°C oil bath for 3 hours, then 1,4-butanediol solution is added and stirred for 2 hours, and the obtained reactant is placed in a 90°C oven for 48 hours to remove N, N-dimethylformamide dimethyl acetal.
[0038] A method for preparing a high-strength phosphogypsum-based functional aggregate for a road, wherein the preparation process is carried out according to the following steps:
[0039] Step 1: pretreating phosphogypsum;
[0040] Step 2: Use Galaxy YHPM-450 disc grinder to grind the prepared polyurethane solid-solid phase change material (PUSSP) for 10 minutes. The particle size should be controlled below 1 mm so that it can be smoothly loaded on the phosphogypsum powder.
[0041] Step 3: Mix the polyurethane solid-solid phase change material (PUSSP) with the phosphogypsum powder at a fixed dosage of 10%, and use a Galaxy YHPM-450 disc grinder to fully grind and mix for 30 minutes to uniformly load the polyurethane solid-solid phase change material (PUSSP) on the phosphogypsum powder;
[0042] Step 4: Add the phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash and silica fume loaded with polyurethane solid-solid phase change material (PUSSP) into a mixer and mix for 60 to 120 seconds, then add the residual slurry of the pipe pile and mix for 40 to 60 seconds; add water during the mixing process until the materials are evenly mixed, and the water accounts for 25% to 40% of the total dry raw materials;
[0043] Step 5, adding the mixed material of step 2 into a granulator, and forming by pressure, the compression ratio of the ring die of the granulator being 2.5 to 6.5;
[0044] Step 6: Carbonization-curing the prepared aggregate at a curing temperature of 20°C to 55°C, a CO2 gas concentration of 20% to 90%, a CO2 gas pressure of 0.1MPa to 0.6MPa, a curing time of 1 to 7 days, and a relative humidity of 40% to 80% in the curing room during the curing period. After carbonization-curing, the aggregate is placed in a stockpile and sprayed with water regularly for natural curing for 21 to 28 days.
[0045] Example 1: A high-strength phosphogypsum-based recycled aggregate loaded with polyurethane solid-solid phase change material (PUSSP), the polyurethane solid-solid phase change material (PUSSP) includes: MDI 23%, PEG 70%, BDO 7%, weigh the corresponding mass raw materials, put PEG4000 and MDI into an oven to melt into liquid, then mix the liquid raw materials into DMF and stir, and carry out the reaction in an 80°C oil bath for 3h, then add BDO solution and stir for 2h, and place the reactants in a 90°C oven for 48h to remove DMF. Nitrogen needs to be introduced as a protective gas during the synthesis process, and the mass fraction of the soft segment of the synthesis formula is 70%, and sample P70 is obtained.
[0046] The raw material components of high-strength phosphogypsum-based recycled aggregate include 50% phosphogypsum, 5% slag powder, 15% cement clinker, 10% steel slag powder, 10% fly ash, and 10% silica fume. The pile slurry is 25% of the dry material weight of the mixture of phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash, and silica fume.
[0047] Functional aggregate preparation includes the following steps:
[0048] Step 1: After drying the phosphogypsum, cool and age it for 24 hours. The drying temperature of the phosphogypsum drying treatment is 120° C. and the drying time is 4 hours.
[0049] Step 2: Use Galaxy YHPM-450 disc grinder to grind the prepared polyurethane solid-solid phase change material (PUSSP) into powder. The grinding time is 10 minutes. The particle size should be controlled below 1 mm so that it can be smoothly loaded on the phosphogypsum powder.
[0050] Step 3: Mix the polyurethane solid-solid phase change material (PUSSP) with the phosphogypsum powder at a fixed dosage of 10%, and use a Galaxy YHPM-450 disc grinder to fully grind and mix for 30 minutes to evenly load the polyurethane solid-solid phase change material (PUSSP) on the phosphogypsum powder.
[0051] Step 4: Add phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash and silica fume loaded with phase change materials into a mixer and mix for 60 seconds, then add the remaining slurry of the pipe pile and mix for 40 seconds; add water during the mixing process until the materials are evenly mixed, and the water accounts for 25% of the total dry raw materials;
[0052] Step 5, adding the mixed material in step 4 into the granulator, adopting pressure molding, the compression ratio of the ring die of the granulator is 2.5, the mixed material is added into the material cavity of the granulator, the mixed material falls on the inner surface of the ring die, and moves under the drive of the ring die until the pressure roller contacts, is grabbed and gradually compacted, and finally enters the die hole of the ring die, is extruded in the die hole to form molded particles, and then enters the molding material cutting cavity, is cut by a blade, and the cutting length of the molded particles can be adjusted;
[0053] Step 6: Carbonization-curing the prepared aggregate, curing temperature: 20°C, CO2 gas concentration 20%, CO2 gas pressure 0.1MPa, curing time 1 day, relative humidity of the curing room during the curing period 40%, after carbonization curing, place the aggregate in the stockpile, spray water regularly for natural curing for 21 days.
[0054] The test results of recycled aggregates show that the crushing index is 18.7%, the water absorption rate is 10.5%, and the apparent density is 1685kg / m3, which meets the requirements of Class II crushed stone in GBT14685-2011 Standard for Construction Crushed Stone and Pebbles and JTG TF50-2011 Technical Specifications for Highway Bridge and Culvert Construction. After the curing of recycled aggregates is completed, the leaching solution is prepared according to the Horizontal Oscillation Method for Toxicity Leaching of Solid Waste (HJ557-2010). The total phosphorus content in the leachate is tested according to the "Determination of Total Phosphorus in Solid Waste by Ammonium Molybdate Spectrophotometry" (HJ 712-2014), and the fluoride ion content is tested according to the "Determination of Fluoride in Solid Waste by Ion Selective Electrode Method" (GB / T 15555.11-1995). The fluoride ion concentration of the leachate is 0.03 mg / L, and the total phosphorus is 0.14 mg / L, which meets the Class III water body standard requirements of the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0055] Example 2: A high-strength phosphogypsum-based recycled aggregate loaded with polyurethane solid-solid phase change material (PUSSP), the polyurethane solid-solid phase change material (PUSSP) includes: MDI 19%, PEG 75%, BDO 6%, weigh the corresponding mass raw materials, put PEG4000 and MDI into an oven to melt into liquid, then mix the liquid raw materials into DMF and stir, and carry out the reaction in an 80°C oil bath for 3h, then add BDO solution and stir for 2h, and place the reactants in a 90°C oven for 48h to remove DMF. Nitrogen needs to be introduced as a protective gas during the synthesis process, and the mass fraction of the soft segment of the synthesis formula is 75%, and sample P75 is obtained.
[0056] The raw material components of high-strength phosphogypsum-based recycled aggregate include 65% phosphogypsum, 25% slag powder, 5% cement clinker, 5% steel slag powder, 5% fly ash, and 5% silica fume. The pipe pile slurry is 35% of the dry material weight of the mixture of phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash, and silica fume.
[0057] Functional aggregate preparation includes the following steps:
[0058] Step 1: After drying the phosphogypsum, cool and age it for 48 hours. The drying temperature of the phosphogypsum drying treatment is 180°C and the drying time is 8 hours.
[0059] Step 2: Use Galaxy YHPM-450 disc grinder to grind the prepared polyurethane solid-solid phase change material (PUSSP) into powder. The grinding time is 10 minutes. The particle size should be controlled below 1 mm so that it can be smoothly loaded on the phosphogypsum powder.
[0060] Step 3: Mix the polyurethane solid-solid phase change material (PUSSP) with the phosphogypsum powder at a fixed dosage of 10%, and use a Galaxy YHPM-450 disc grinder to fully grind and mix for 30 minutes to evenly load the polyurethane solid-solid phase change material (PUSSP) on the phosphogypsum powder.
[0061] Step 4: Add phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash and silica fume loaded with phase change materials into a mixer and mix for 120 seconds, then add the remaining slurry of the pipe pile and mix for 60 seconds; add water during the mixing process until the materials are evenly mixed, and the water accounts for 40% of the total dry raw materials;
[0062] Step 5, adding the mixed material of step 4 into the granulator, adopting pressure molding, the compression ratio of the ring die of the granulator is 6.5, the mixed material is added into the material cavity of the granulator, the mixed material falls on the inner surface of the ring die, and moves under the drive of the ring die until the pressure roller contacts, is grabbed and gradually compacted, and finally enters the die hole of the ring die, extruded in the die hole to form molded particles, and then enters the molding material cutting cavity, and is cut by a blade, and the cutting length of the molded particles can be adjusted;
[0063] Step 6: Carbonization-curing the prepared aggregate, curing temperature: 55°C, CO2 gas concentration 90%, CO2 gas pressure 0.6MPa, curing time 7 days, relative humidity of the curing room during the curing period 80%, after carbonization curing, place the aggregate in the yard, spray water regularly for natural curing for 28 days.
[0064] The test results of recycled aggregates show that the crushing index is 22.6%, the water absorption rate is 12.6%, and the apparent density is 1567kg / m3, which meets the requirements of Class III crushed stone in GBT14685-2011 Standard for Construction Crushed Stone and Pebbles and JTG TF50-2011 Technical Specifications for Highway Bridge and Culvert Construction. After the curing of recycled aggregates is completed, the leaching solution is prepared according to the Horizontal Oscillation Method for Toxicity Leaching of Solid Waste (HJ557-2010). The total phosphorus content in the leachate is tested according to the "Determination of Total Phosphorus in Solid Waste by Ammonium Molybdate Spectrophotometry" (HJ 712-2014), and the fluoride ion content is tested according to the "Determination of Fluoride in Solid Waste by Ion Selective Electrode Method" (GB / T 15555.11-1995). The fluoride ion concentration of the leachate is 0.04 mg / L, and the total phosphorus is 0.25 mg / L, which meets the Class IV water body standard requirements of the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0065] Example 3: A high-strength phosphogypsum-based recycled aggregate loaded with polyurethane solid-solid phase change material (PUSSP), the polyurethane solid-solid phase change material (PUSSP) includes: MDI 15%, PEG 80%, BDO 5%, weigh the corresponding mass raw materials, put PEG4000 and MDI into an oven to melt into liquid, then mix the liquid raw materials into DMF and stir, and carry out the reaction in an 80°C oil bath for 3h, then add BDO solution and stir for 2h, and place the reactants in a 90°C oven to dry for 48h to remove DMF. Nitrogen needs to be introduced as a protective gas during the synthesis process, and the mass fraction of the soft segment of the synthesis formula is 80%, and sample P80 is obtained.
[0066] The raw material components of high-strength phosphogypsum-based recycled aggregate include 75% phosphogypsum, 10% slag powder, 10% cement clinker, 3% steel slag powder, 1% fly ash, and 1% silica fume. The pipe pile slurry is 30% of the dry material weight of the mixture of phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash, and silica fume.
[0067] Functional aggregate preparation includes the following steps:
[0068] Step 1: After drying the phosphogypsum, cool and age it for 30 hours. The drying temperature of the phosphogypsum drying treatment is 160° C. and the drying time is 6 hours.
[0069] Step 2: Use Galaxy YHPM-450 disc grinder to grind the prepared polyurethane solid-solid phase change material (PUSSP) into powder. The grinding time is 10 minutes. The particle size should be controlled below 1 mm so that it can be smoothly loaded on the phosphogypsum powder.
[0070] Step 3: Mix the polyurethane solid-solid phase change material (PUSSP) with the phosphogypsum powder at a fixed dosage of 10%, and use a Galaxy YHPM-450 disc grinder to fully grind and mix for 30 minutes to evenly load the polyurethane solid-solid phase change material (PUSSP) on the phosphogypsum powder.
[0071] Step 4: Add phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash and silica fume loaded with phase change materials into a mixer and mix for 80 seconds, then add the remaining slurry of the pipe piles and mix for 55 seconds; add water during the mixing process until the materials are evenly mixed, and the water accounts for 32% of the total dry raw materials;
[0072] Step 5, adding the mixed material in step 4 into the granulator, adopting pressure molding, the compression ratio of the ring die of the granulator is 3.5, the mixed material is added into the material cavity of the granulator, the mixed material falls on the inner surface of the ring die, and moves under the drive of the ring die until the pressure roller contacts, is grabbed and gradually compacted, and finally enters the die hole of the ring die, is extruded in the die hole to form molded particles, and then enters the molding material cutting cavity, is cut by a blade, and the cutting length of the molded particles can be adjusted;
[0073] Step 6: Carbonization-curing the prepared aggregate, curing temperature: 30°C, CO2 gas concentration 50%, CO2 gas pressure 0.3MPa, curing time 5 days, relative humidity of the curing room during the curing period 50%, after carbonization curing, place the aggregate in the yard, spray water regularly for natural curing for 26 days.
[0074] The test results of recycled aggregates show that the crushing index is 23.7%, the water absorption rate is 17.7%, and the apparent density is 1505kg / m3, which meets the requirements of Class III crushed stone in GBT14685-2011 Standard for Construction Crushed Stone and Pebbles and JTG TF50-2011 Technical Specifications for Highway Bridge and Culvert Construction. After the curing of recycled aggregates is completed, the leaching solution is prepared according to the Horizontal Oscillation Method for Toxicity Leaching of Solid Waste (HJ557-2010). The total phosphorus content in the leachate is tested according to the "Determination of Total Phosphorus in Solid Waste by Ammonium Molybdate Spectrophotometry" (HJ 712-2014), and the fluoride ion content is tested according to the "Determination of Fluoride in Solid Waste by Ion Selective Electrode Method" (GB / T 15555.11-1995). The fluoride ion concentration of the leachate is 0.07 mg / L, and the total phosphorus is 0.27 mg / L, which meets the Class IV water body standard requirements of the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0075] Example 4: A high-strength phosphogypsum-based recycled aggregate loaded with polyurethane solid-solid phase change material (PUSSP), the polyurethane solid-solid phase change material (PUSSP) includes: MDI 12%, PEG 85%, BDO 3%, weigh the corresponding mass raw materials, put PEG4000 and MDI into an oven to melt into liquid, then mix the liquid raw materials into DMF and stir, and carry out the reaction in an 80°C oil bath for 3h, then add BDO solution and stir for 2h, and place the reactants in a 90°C oven for 48h to remove DMF. Nitrogen needs to be introduced as a protective gas during the synthesis process, and the mass fraction of the soft segment of the synthesis formula is 85%, and sample P85 is obtained.
[0076] The raw material components of high-strength phosphogypsum-based recycled aggregate include 87% phosphogypsum, 2% slag powder, 5% cement clinker, 1% steel slag powder, 2% fly ash, and 3% silica fume. The pipe pile slurry is 28% of the dry material weight of the mixture of phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash, and silica fume.
[0077] Functional aggregate preparation includes the following steps:
[0078] Step 1: After drying the phosphogypsum, cool and age it for 36 hours. The drying temperature of the phosphogypsum drying treatment is 140° C. and the drying time is 7 hours.
[0079] Step 2: Use Galaxy YHPM-450 disc grinder to grind the prepared polyurethane solid-solid phase change material (PUSSP) into powder. The grinding time is 10 minutes. The particle size should be controlled below 1 mm so that it can be smoothly loaded on the phosphogypsum powder.
[0080] Step 3: Mix the polyurethane solid-solid phase change material (PUSSP) with the phosphogypsum powder at a fixed dosage of 10%, and use a Galaxy YHPM-450 disc grinder to fully grind and mix for 30 minutes to evenly load the polyurethane solid-solid phase change material (PUSSP) on the phosphogypsum powder.
[0081] Step 4: Add phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash and silica fume loaded with phase change materials into a mixer and mix for 100 seconds, then add the remaining slurry of the pipe pile and mix for 50 seconds; add water during the mixing process until the materials are evenly mixed, and the water accounts for 34% of the total dry raw materials;
[0082] Step 5, adding the mixed material in step 4 into the granulator, adopting pressure molding, the compression ratio of the ring die of the granulator is 4.5, the mixed material is added into the material cavity of the granulator, the mixed material falls on the inner surface of the ring die, and moves under the drive of the ring die until the pressure roller contacts, is grabbed and gradually compacted, and finally enters the die hole of the ring die, is extruded in the die hole to form molded particles, and then enters the molding material cutting cavity, is cut by a blade, and the cutting length of the molded particles can be adjusted;
[0083] Step 6: Carbonization-curing the prepared aggregate, curing temperature: 40°C, CO2 gas concentration 60%, CO2 gas pressure 0.4MPa, curing time 5 days, relative humidity of the curing room during the curing period 40-80%, after carbonization curing, place the aggregate in the yard, spray water regularly for natural curing for 24 days.
[0084] The test results of recycled aggregates show that the crushing index is 32.5%, the water absorption rate is 20.3%, and the apparent density is 1345kg / m3, which meets the requirements of Class III crushed stone in GBT14685-2011 Standard for Construction Crushed Stone and Pebbles and JTG TF50-2011 Technical Specifications for Highway Bridge and Culvert Construction. After the curing of recycled aggregates is completed, the leaching solution is prepared according to the Horizontal Oscillation Method for Leaching Toxicity of Solid Waste (HJ557-2010). The total phosphorus content in the leachate is tested according to the "Determination of Total Phosphorus in Solid Waste by Ammonium Molybdate Spectrophotometry" (HJ 712-2014), and the fluoride ion content is tested according to the "Determination of Fluoride in Solid Waste by Ion Selective Electrode Method" (GB / T 15555.11-1995). The fluoride ion concentration of the leachate is 0.12 mg / L, and the total phosphorus is 0.32 mg / L, which meets the Class V water body standard requirements of the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0085] Example 5: A high-strength phosphogypsum-based recycled aggregate loaded with polyurethane solid-solid phase change material (PUSSP), the polyurethane solid-solid phase change material (PUSSP) includes: MDI 8%, PEG 90%, BDO 2%, weigh the corresponding mass raw materials, put PEG4000 and MDI into an oven to melt into liquid, then mix the liquid raw materials into DMF and stir, and carry out the reaction in an 80°C oil bath for 3h, then add BDO solution and stir for 2h, and place the reactants in a 90°C oven to dry for 48h to remove DMF. Nitrogen needs to be introduced as a protective gas during the synthesis process, and the mass fraction of the soft segment of the synthesis formula is 90%, and sample P90 is obtained.
[0086] The raw material composition of high-strength phosphogypsum-based recycled aggregate includes 95% phosphogypsum, 3% slag powder, 0.5% cement clinker, 0.5% steel slag powder, 0.5% fly ash, and 0.5% silica fume. The residual slurry of the pipe pile is 32% of the dry material weight of the mixture of phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash, and silica fume. The preparation of functional aggregate includes the following steps:
[0087] Step 1: After drying the phosphogypsum, cool and age it for 40 hours. The drying temperature of the phosphogypsum drying treatment is 130° C. and the drying time is 5 hours.
[0088] Step 2: Use Galaxy YHPM-450 disc grinder to grind the prepared polyurethane solid-solid phase change material (PUSSP) into powder. The grinding time is 10 minutes. The particle size should be controlled below 1 mm so that it can be smoothly loaded on the phosphogypsum powder.
[0089] Step 3: Mix the polyurethane solid-solid phase change material (PUSSP) with the phosphogypsum powder at a fixed dosage of 10%, and use a Galaxy YHPM-450 disc grinder to fully grind and mix for 30 minutes to evenly load the polyurethane solid-solid phase change material (PUSSP) on the phosphogypsum powder.
[0090] Step 4: Add phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash and silica fume loaded with phase change materials into a mixer and mix for 100 seconds, then add the remaining slurry of the pipe pile and mix for 50 seconds; add water during the mixing process until the materials are evenly mixed, and the water accounts for 30% of the total dry raw materials;
[0091] Step 5, adding the mixed material in step 4 into the granulator, adopting pressure molding, the compression ratio of the ring die of the granulator is 4.5, the mixed material is added into the material cavity of the granulator, the mixed material falls on the inner surface of the ring die, and moves under the drive of the ring die until the pressure roller contacts, is grabbed and gradually compacted, and finally enters the die hole of the ring die, is extruded in the die hole to form molded particles, and then enters the molding material cutting cavity, is cut by a blade, and the cutting length of the molded particles can be adjusted;
[0092] Step 6: Carbonization-curing the prepared aggregate, curing temperature: 26°C, CO2 gas concentration 50%, CO2 gas pressure 0.5MPa, curing time 3 days, relative humidity of the curing room during the curing period 70%, after carbonization curing, place the aggregate in the yard, spray water regularly for natural curing for 25 days.
[0093] The test results of recycled aggregates show that the crushing index is 34.3%, the water absorption rate is 22.5%, and the apparent density is 1015kg / m3, which meets the requirements of Class III crushed stone in GBT14685-2011 Standard for Construction Crushed Stone and Pebbles and JTG TF50-2011 Technical Specifications for Highway Bridge and Culvert Construction. After the curing of recycled aggregates is completed, the leaching solution is prepared according to the Horizontal Oscillation Method for Toxicity Leaching of Solid Waste (HJ557-2010). The total phosphorus content in the leachate is tested according to the "Determination of Total Phosphorus in Solid Waste by Ammonium Molybdate Spectrophotometry" (HJ 712-2014), and the fluoride ion content is tested according to the "Determination of Fluoride in Solid Waste by Ion Selective Electrode Method" (GB / T 15555.11-1995). The fluoride ion concentration of the leachate is 0.15 mg / L, and the total phosphorus is 0.35 mg / L, which meets the Class V water body standard requirements of the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0094] Table 1 Drugs required for PUSSP synthesis and their mass (%)
[0095]
[0096] Table 2 Compression resistance of each embodiment at 7, 14 and 28 days
[0097]
[0098] Table 3 Physical properties of each PUSSP
[0099]
[0100] Table 4 Heat storage characteristic parameters of each PUSSP
[0101]
[0102] Due to the presence of a large number of hard segment micro-regions in PUSSP, the phase transition of the soft segment crystal from the crystalline state to the amorphous state is restricted to a large extent. With the increase of the mass fraction of the PUSSP soft segment, the melting enthalpy and crystallization enthalpy of P90 are higher than those of P70. Therefore, the heat storage characteristics can be improved by increasing the mass fraction of the soft segment during application.
[0103] The adsorption test results show that there is no obvious change in the physical appearance properties of PUSSP before and after heating in the oven, only a slight elastic deformation exists, and there is no adsorption mark on the filter paper under PUSSP, which indicates that PUSSP has good phase stability and no leakage occurs during the entire phase change heat storage process. The phase change behavior is from solid to solid, and it is widely used in road temperature control in my country.
[0104] Table 5 Thermal stability indexes of various PUSSP
[0105]
[0106] As the mass fraction of the soft segment decreases, the thermal decomposition temperature of PUSSP increases significantly, which indicates that PUSSP with fewer soft segments has better thermal stability.
[0107] Although the technical solutions of the present invention have been described and listed in detail, it should be understood that it is obvious to those skilled in the art to make modifications to the above embodiments or adopt equivalent alternatives. These modifications or improvements made without departing from the spirit of the present invention are within the scope of protection required by the present invention.
Claims
1. A method for preparing high-strength phosphogypsum-based functional aggregate for roads, characterized in that: The polyurethane solid-solid phase change material is loaded on high-strength phosphogypsum-based road aggregate.
2. The method for preparing a high-strength phosphogypsum-based functional aggregate for roads according to claim 1, characterized in that: The polyurethane solid-solid phase change material is synthesized by using methylene diphenyl diisocyanate as a hard segment, polyethylene glycol 4000 as a soft segment, and 1,4-butanediol as a chain extender. The solution used in the synthesis process is N,N-dimethylformamide dimethyl acetal.
3. The method for preparing a high-strength phosphogypsum-based functional aggregate for roads according to claim 1, characterized in that: The preparation process of the polyurethane solid-solid phase change material is as follows: weighed methylene diphenyl diisocyanate and polyethylene glycol are put into an oven to melt into a liquid state, and then N, N-dimethylformamide dimethyl acetal is mixed into the liquid methylene diphenyl diisocyanate and polyethylene glycol, and then stirred in an 80°C oil bath for 3 hours, and then 1,4-butanediol solution is added and stirred for 2 hours, and the obtained reactant is placed in a 90°C oven for drying for 48 hours to remove N, N-dimethylformamide dimethyl acetal.
4. The method for preparing a high-strength phosphogypsum-based functional aggregate for roads according to claim 3, characterized in that: During the synthesis of the polyurethane solid-solid phase change material, nitrogen is introduced as a protective gas.
5. The method for preparing a high-strength phosphogypsum-based road functional aggregate according to claim 1, characterized in that: The preparation process is carried out according to the following steps: Step 1: pretreating phosphogypsum; Step 2: grind the prepared polyurethane solid-solid phase change material into powder, the grinding time is 10 minutes, and the particle size is controlled to be less than 1 mm; Step 3: Mix the polyurethane solid-solid phase change material with the phosphogypsum powder, fix the dosage to 10%, and fully grind and mix them for 30 minutes to evenly load the polyurethane solid-solid phase change material on the phosphogypsum powder; Step 4: Add the phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash and silica fume loaded with polyurethane solid-solid phase change material into a mixer and mix for 60 to 120 seconds, then add the remaining slurry of the pipe pile and mix for 40 to 60 seconds; add water during the mixing process until the materials are evenly mixed; Step 5, adding the mixed material of step 2 into a granulator and forming by pressure; Step six: carbonizing and curing the prepared aggregate.
6. The method for preparing a high-strength phosphogypsum-based functional aggregate for roads according to claim 5, characterized in that: The pretreatment method of phosphogypsum in step 1 is: drying the phosphogypsum, cooling and aging for 24 to 48 hours, the drying temperature of the phosphogypsum drying treatment is 120° C. to 180° C., and the drying time is 4 to 8 hours.
7. The method for preparing a high-strength phosphogypsum-based functional aggregate for roads according to claim 5, characterized in that: The amount of water added in step 4 is 25% to 40% of the total amount of dry raw materials.
8. The method for preparing a high-strength phosphogypsum-based functional aggregate for roads according to claim 5, characterized in that: The ring die compression ratio of the granulator in step 5 is 2.5 to 6.
5.
9. The method for preparing a high-strength phosphogypsum-based functional aggregate for roads according to claim 5, characterized in that: The carbonization curing conditions of step six are as follows: curing temperature: 20°C to 55°C, CO2 gas concentration 20% to 90%, CO2 gas pressure 0.1MPa to 0.6MPa, curing time 1 to 7 days, relative humidity of the curing room during the curing period 40% to 80%, after carbonization curing, the aggregate is placed in a stockpile and sprayed with water regularly for natural curing for 21 to 28 days.
10. The method for preparing a high-strength phosphogypsum-based functional aggregate for roads according to claim 1, characterized in that: The components of the high-strength phosphogypsum-based road aggregate include phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash, silica ash, and pipe pile slurry. The percentage of each component is: phosphogypsum 50% to 95%, slag powder 3% to 25%, cement clinker 0.5% to 15%, steel slag powder 0.5% to 10%, fly ash 0.5% to 10%, and silica ash 0.5% to 10%. The pipe pile slurry is 25% to 35% of the dry material weight of the mixture of phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash, and silica ash.