Magnesium oxychloride cement stirring and connecting method

Through the magnesium oxychloride cement dialing method, by configuring and mixing specific ingredients and then pouring them into the molded component body, the problem of magnesium oxychloride cement failing to meet the three force detection standards in the direct butt joining method is solved, and the optimal material is achieved. Strength and structural safety, suitable for prefabricated buildings.

CN118771844APending Publication Date: 2024-10-15XIAMEN ZHONGXING XINMEI NEW MATERIALS TECHNOLOGY RESEARCH INSTITUTE (LLP)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410762929.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The three-force detection of the structure of magnesium oxychloride cement in the direct butt joint method cannot meet the construction standards, resulting in potential safety hazards in load-bearing applications.

Method used

A magnesium oxychloride cement dialing method is used to prepare the magnesium chloride solution, detect the baume degree, add toughening agent and anti-halogen agent, add magnesium oxide, carbon fiber filling granularity and silicon steel, stir evenly and pour into the molded component After the mold is taken out, it is connected into a room, and the tongue and groove design is used to realize the connection of the building blocks.

Benefits of technology

It improves the dilute flow and anti-halogen problems of magnesium oxychloride cement, controls the cross-linking curing temperature of oxychloride, and improves the strength of the material and the load-bearing capacity of the structure, making it able to meet the three-force testing standards of buildings and is suitable for prefabricated Buildings and small structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771844A_ABST
    Figure CN118771844A_ABST
Patent Text Reader

Abstract

The invention provides a stirring and connecting method for magnesium oxychloride cement. The stirring and connecting method for the magnesium oxychloride cement comprises the following steps: S1, preparing a magnesium chloride solution; s2, detecting whether the baume degree meets the requirement or not; s3, adding a flexibilizer and an anti-halogenating agent into the magnesium chloride solution, and uniformly stirring; s4, magnesium oxide is added for continuous stirring, and magnesium oxychloride cement is prepared; s5, adding the carbon fiber filling granularity and the silicon element into the magnesium oxychloride cement, and uniformly stirring; and S6, pouring the stirred magnesium oxychloride cement into the molded component body, and pulling and connecting the molded component body to form a house after demolding. According to the magnesium oxychloride cement pulling and connecting method provided by the invention, several building blocks are pulled and connected into a house shape through the rabbets, the building blocks are used for fabricated buildings and small-structure buildings, and the problem that three-force detection of magnesium oxychloride cement buildings does not reach the standard is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnesium oxychloride cement, in particular to a magnesium oxychloride cement dialing method. Background Art

[0002] Since magnesium oxychloride cement has stronger adhesion than ordinary silicate rock cement, many manufacturers use direct butt connection method. The application strength of this connection method is equivalent to the life of the material itself. Its structural strength is second only to the integral casting module, but it can fully meet the construction application standards. Although it can temporarily solve structural problems, the real three-force test cannot meet the standards.

[0003] Therefore, it is necessary to provide a new magnesium oxychloride cement dialing method to solve the above-mentioned technical problems. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a magnesium oxychloride cement splicing method.

[0005] The present invention provides a magnesium oxychloride cement dialing method, which comprises:

[0006] S1: prepare magnesium chloride solution;

[0007] S2: Check whether the Baume degree meets the requirements;

[0008] If yes, S3: add toughening agent and anti-halogen agent to magnesium chloride solution and stir evenly;

[0009] S4: adding magnesium oxide and continuing stirring to prepare magnesium oxychloride cement;

[0010] S5: adding carbon fiber filler particles and silicon steel into magnesium oxychloride cement and mixing evenly;

[0011] S6: Pour the mixed magnesium oxychloride cement into the molded component body, and connect it into a room after it is removed from the mold.

[0012] Preferably, the particle size ratio of the magnesium chloride solution, magnesium oxide, anti-halogen agent, toughening agent, silicon steel element, and carbon fiber filling is 110:100:0.006:0.008:0.3:0.2.

[0013] Preferably, the preparation of magnesium chloride solution comprises:

[0014] At room temperature, stir water and magnesium chloride granules in a ratio of 120:100 until the granules are completely dissolved.

[0015] Preferably, the step of detecting whether the Baume degree meets the requirements comprises:

[0016] After the magnesium chloride solution has been set for 24 hours, test the Baume degree at room temperature to see if it is 22-25. If so, proceed to the next step. If not, return to the first step and make adjustments to meet the requirements.

[0017] Preferably, the purity grade of the magnesium oxide powder reaches 85 or above.

[0018] Preferably, the step of adding carbon fiber filling particles and silicon steel into magnesium oxychloride cement and stirring evenly comprises:

[0019] Adjust the ingredients according to the stress requirements. If a load-bearing floor is required, add steel bars treated with silicone phospholipid anti-chlorination or high-strength long fibers that meet the building tension standards.

[0020] Preferably, the stirred magnesium oxychloride cement is poured into the molded component body, comprising:

[0021] The molded component body adopts a tongue-and-groove design so that the building blocks configured with magnesium oxychloride cement can be connected with the tongue-and-groove connection.

[0022] Compared with the related art, the magnesium oxychloride cement dialing method provided by the present invention has the following beneficial effects:

[0023] The invention provides a magnesium oxychloride cement dialing method, which improves the dilute fluidity problem and the anti-halogen problem of the magnesium oxychloride cement, can control the temperature when the chlorine oxide produces cross-linking solidification, and enables the magnesium oxychloride cement to reach the best strength. Several building blocks are connected into a house shape through tongue and groove dialing, and are used for prefabricated buildings and small-structure buildings, thereby solving the problem that the three-force detection of the magnesium oxychloride cement building does not meet the standards. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of the process of the magnesium oxychloride cement dialing method provided by the present invention; DETAILED DESCRIPTION

[0025] The present invention will be further described below in conjunction with the accompanying drawings and implementation modes.

[0026] Please refer to Figure 1 in, Figure 1 The present invention provides a schematic diagram of the overall structure of the magnesium oxychloride cement splicing method.

[0027] In the specific implementation process, Figure 1 As shown, a magnesium oxychloride cement dialing method, the magnesium oxychloride cement dialing method comprises:

[0028] S1: prepare magnesium chloride solution;

[0029] S2: Check whether the Baume degree meets the requirements;

[0030] If yes, S3: add toughening agent and anti-halogen agent to magnesium chloride solution and stir evenly;

[0031] S4: adding magnesium oxide and continuing stirring to prepare magnesium oxychloride cement;

[0032] S5: adding carbon fiber filler particles and silicon steel into magnesium oxychloride cement and mixing evenly;

[0033] S6: Pour the mixed magnesium oxychloride cement into the molded component body, and connect it into a room after it is removed from the mold;

[0034] The particle size ratio of the magnesium chloride solution, magnesium oxide, anti-halogen agent, toughening agent, silicon steel element and carbon fiber filling is 110:100:0.006:0.008:0.3:0.2.

[0035] Specifically, S1: the preparation of the magnesium chloride solution comprises:

[0036] At room temperature, stir water and magnesium chloride granules at a ratio of 120:100 until the granules are completely dissolved.

[0037] S2: Whether the Baume degree is tested to meet the requirements, including:

[0038] After the magnesium chloride solution has been standing for 24 hours, immerse the Baume hydrometer in the magnesium chloride solution at room temperature of 20 to 30 degrees to test whether the Baume degree is 22-25. If so, proceed to the next step. If not, return to the first step and make adjustments to meet the requirements. If not, make further adjustments.

[0039] S3: Add toughening agent and anti-halogen agent to magnesium chloride solution and stir evenly;

[0040] Toughening agents are added to increase toughness, improve bearing strength and reduce cracking; anti-halogen agents are added to improve the anti-halogen situation of magnesium oxychloride cement; toughening agents and anti-halogen agents are added to improve the properties of magnesium oxychloride cement itself.

[0041] S4: adding magnesium oxide and continuing stirring to prepare magnesium oxychloride cement;

[0042] The purity grade of the magnesium oxide powder reaches above grade 85, and the magnesium oxide reacts with the magnesium chloride solution to prepare magnesium oxychloride cement, and the next step is quickly carried out after the magnesium oxide powder is added.

[0043] S5: Add carbon fiber filler particles and silicon steel into magnesium oxychloride cement and mix well, including:

[0044] Adjust the ingredients according to the stress requirements. If a load-bearing floor is required, add steel bars treated with silicon phospholipid anti-chlorination or high-strength long fibers that meet the building tension standards. Under normal circumstances, adding 1.5 cm to 2 cm short high-strength carbon fibers can meet the strength requirements of magnesium oxychloride cement.

[0045] Silicon steel controls the temperature of the cross-linking and curing of chlorine oxides to be between 60 and 80 degrees. Silicon steel solves the high temperature problem caused by the cross-linking and curing of chlorine oxides, and fully and effectively protects the optimal strength in the chlorine oxide chemical reaction.

[0046] S6: Pour the mixed magnesium oxychloride cement into the molded component body, and connect it into a room after it is removed from the mold;

[0047] The molded component body adopts a tongue-and-groove design so that the building blocks configured by magnesium oxychloride cement can be connected by tongue-and-groove, and can be installed and applied after demolding. Specifically, the stirred magnesium oxychloride cement is poured into molded component bodies of different shapes, and after being molded and demolded, the molded component body is connected into a house after being dialed, and the first building wall block, the second building wall block, the third building wall block, the fourth building wall block, the internal two-story structure, the building bottom block and the building roof are demolded, and then assembled into a house. The first building wall block, the second building wall block, the third building wall block, the fourth building wall block and the two-story structure are connected by tongue-and-groove, and magnesium oxychloride cement has good adhesiveness. The gravity, shear force and tension of the building blocks configured by magnesium oxychloride cement all meet the practical standards of construction. For example, a two-way wall with a width of 240 mm, a height of 3500 mm and a length of 3000 mm is connected at 90 degrees. We adopt a new dialing method and its gravity bearing is 50T without abnormal changes. The lateral shear force is estimated to be 300 Newtons without abnormal changes. The vertical tension is 1000 Newtons without abnormal changes.

[0048] The invention provides a magnesium oxychloride cement dialing method, which improves the dilute fluidity problem and the anti-halogen problem of the magnesium oxychloride cement, can control the temperature when the chlorine oxide produces cross-linking solidification, and enables the magnesium oxychloride cement to reach the best strength. Several building blocks are connected into a house shape through tongue and groove dialing, and are used for prefabricated buildings and small-structure buildings, thereby solving the problem that the three-force detection of the magnesium oxychloride cement building does not meet the standards.

[0049] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A magnesium oxychloride cement splicing method, characterized in that: The magnesium oxychloride cement dialing method comprises: S1: prepare magnesium chloride solution; S2: Check whether the Baume degree meets the requirements; If yes, S3: add toughening agent and anti-halogen agent to magnesium chloride solution and stir evenly; S4: adding magnesium oxide and continuing stirring to prepare magnesium oxychloride cement; S5: adding carbon fiber filler particles and silicon steel into magnesium oxychloride cement and mixing evenly; S6: Pour the mixed magnesium oxychloride cement into the molded component body, and connect it into a room after it is removed from the mold.

2. The magnesium oxychloride cement splicing method according to claim 1, characterized in that: The particle size ratio of the magnesium chloride solution, magnesium oxide, anti-halogen agent, toughening agent, silicon steel element and carbon fiber filling is 110:100:0.006:0.008:0.3:0.

2.

3. The magnesium oxychloride cement splicing method according to claim 1, characterized in that: The magnesium chloride solution is prepared, comprising: At room temperature, stir water and magnesium chloride granules in a ratio of 120:100 until the granules are completely dissolved.

4. The magnesium oxychloride cement splicing method according to claim 1, characterized in that: The test of whether the Baume degree meets the requirements includes: After the magnesium chloride solution has been set for 24 hours, test the Baume degree at room temperature to see if it is 22-25. If so, proceed to the next step. If not, return to the first step and make adjustments to meet the requirements.

5. The magnesium oxychloride cement splicing method according to claim 1, characterized in that: The purity grade of the magnesium oxide powder reaches above grade 85.

6. The magnesium oxychloride cement splicing method according to claim 1, characterized in that: The step of adding carbon fiber filling particles and silicon steel into magnesium oxychloride cement and mixing evenly comprises: Adjust the ingredients according to the stress requirements. If a load-bearing floor is required, add steel bars treated with silicone phospholipid anti-chlorination or high-strength long fibers that meet the building tension standards.

7. The magnesium oxychloride cement splicing method according to claim 1, characterized in that: The stirred magnesium oxychloride cement is poured into the molded component body, comprising: The molded component body adopts a tongue-and-groove design so that the building blocks configured with magnesium oxychloride cement can be connected with the tongue-and-groove connection.