Preparation method and application of polydicyclopentadiene material

By introducing norbornene or phenol or amine compounds with a norbornane structure into polydicyclopentadiene materials, a fully interpenetrating network polymer is formed, which solves the problem of insufficient material strength and anti-aging properties and achieves high strength and toughness. and improvement of excellent dielectric properties.

CN118772379AActive Publication Date: 2024-10-15WANHUA CHEM GRP CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410833411.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-15
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

Existing polydicyclopentadiene materials cannot meet the requirements of high strength, toughness and good aging resistance in some application fields.

Method used

Phenol or amine compounds containing norbornene or norbornane structures are introduced, and cross-linked with dicyclopentadiene in the dicyclopentadiene ring-opening metathesis polymerization system to form a fully interpenetrating network polymer to enhance the material's Strength, toughness and anti-aging properties.

Benefits of technology

The high strength, toughness and excellent anti-aging properties and dielectric properties of the modified polydicyclopentadiene material are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004912459110000021
    Figure BDA0004912459110000021
  • Figure BDA0004912459110000081
    Figure BDA0004912459110000081
  • Figure BDA0004912459110000091
    Figure BDA0004912459110000091
Patent Text Reader

Abstract

The invention discloses a polydicyclopentadiene material which is prepared by taking a dicyclopentadiene monomer and a phenol or amine compound containing a norbornene or norbornane structure as raw materials under the catalysis of a main catalyst and a cocatalyst. The phenol or amine compound containing the norbornene or norbornane structure not only has oxidation resistance, but also can be subjected to cross-linking reaction with dicyclopentadiene under the action of a dicyclopentadiene ring-opening metathesis polymerization system and a catalyst to form a fully interpenetrating network polymer with dicyclopentadiene, so that the aims of enhancing, toughening and resisting aging are fulfilled at the same time; the obtained polydicyclopentadiene material has the advantages of high strength, high toughness, high aging resistance, and good dielectric properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polydicyclopentadiene materials, and in particular relates to a polydicyclopentadiene material modified by a phenolic or amine compound. Background Art

[0002] PDCPD, or polydicyclopentadiene, has been included in Article 130 of the National "Guidelines for the Demonstration of the First Application of Key New Materials (2021 Edition)" due to its lightweight, high physical and mechanical properties, high and low temperature resistance, corrosion resistance, and environmental friendliness. The main properties of PDCPD include low density, corrosion resistance, suitability for large and complex structural products, excellent coating properties, good wave transmission, environmental protection, impact resistance, and short molding cycle. Therefore, as an excellent thermosetting material, it is widely used in engineering machinery, heavy trucks, military industry, chemical industry, medical, and outdoor fields.

[0003] Some application fields require polydicyclopentadiene to have not only high strength and toughness, but also good aging resistance, etc. However, the existing polydicyclopentadiene materials cannot meet the requirements and further improvement of the materials is needed. Summary of the invention

[0004] In view of the above problems existing in the prior art, the present invention aims to provide a polydicyclopentadiene material with higher strength, toughness, excellent anti-aging performance and dielectric properties. The present invention introduces a phenol or amine compound containing a norbornene or norbornane structure, which not only has antioxidant ability, but also can undergo a cross-linking reaction with dicyclopentadiene under the action of a dicyclopentadiene ring-opening metathesis polymerization system and a catalyst, and form a fully interpenetrating network polymer with dicyclopentadiene, thereby achieving the purposes of strengthening, toughening and anti-aging at the same time, so that the obtained modified polydicyclopentadiene material has higher strength, toughness, excellent anti-aging performance and dielectric properties.

[0005] To achieve the above-mentioned object of the invention, the present invention adopts the following scheme:

[0006] In a first aspect, the present invention provides a phenol or amine compound containing a norbornene or norbornene structure, the structure of which is as follows:

[0007]

[0008] For example, 1,2-R-3,6-dihydroxybenzonorbornene, 1,2-R-3,6-dihydroxybenzonorbornene, 1,2-R-3,6-dihydroxycyclohexanedorbornene, 1,2-R-3,6-bis(4-aminophenoxy)benzonorbornene, 1,2-R-3,6-bis(4-aminophenoxy)benzonorbornene, 1,2-R-3,6-bis(4-aminophenoxy)cyclohexanedorbornene, 1,2-R-3,6-bis(4-aminophenoxy)benzonorbornene, 1,2-R-3,6-bis(4-aminophenoxy)benzonorbornene, 1,2-R-3,6-bis(4-amino-5-methylphenoxy)benzonorbornene, 1,2-R-3,6-bis(4-amino-5-methylphenoxy)benzonorbornene, 1,2-R-3,6-bis(4-amino-3,5-methylphenoxy)benzonorbornene, 1,2-R-3,6-bis(4-amino-3,5-methylphenoxy)benzonorbornene, 1,2-R-3,6-bis(4-amino-3,5-methylphenoxy)cyclohexanedorbornene, 1,2-R-3,6-bis(4-amino-2-trifluoromethylphenoxy)benzonorbornene, 1,2-R-3,6-bis(4-amino-2-trifluoromethylphenoxy)benzonorbornene, 1,2-R-3,6-bis(4-amino-2-trifluoromethylphenoxy)cyclohexanedorbornene, wherein R is hydrogen or methyl, preferably hydrogen.

[0009] In a second aspect, the present invention provides a method for preparing a phenol or amine compound containing a norbornene or norbornene structure, the steps comprising:

[0010] Under nitrogen conditions, norbornene monomers containing phenol or ammonia are mixed with anhydrous ethanol and a hydrogenation catalyst, hydrogen is introduced, and the temperature is increased to carry out a hydrogenation reaction to obtain the product.

[0011] In the present invention, the monomers are, for example, 1,2-R-3,6-dihydroxybenzonorbornene, 1,2-R-3,6-bis(4-aminophenoxy)benzonorbornene, 1,2-R-3,6-bis(4-amino-5-methylphenoxy)benzonorbornene, 1,2-R-3,6-bis(4-amino-3,5-methylphenoxy)benzonorbornene, 1,2-R-3,6-bis(4-amino-2-trifluoromethylphenoxy)benzonorbornene, wherein R is hydrogen or methyl, preferably hydrogen, and the most preferred monomers are 3,6-dihydroxybenzonorbornene and 3,6-bis(4-aminophenoxy)benzonorbornene;

[0012] In the present invention, the volume ratio of the mass of the norbornene monomer containing phenol or ammonia to anhydrous ethanol is 50-150 g / L, for example, 50, 70, 90, 110, 130, 150 g / L.

[0013] In the present invention, the hydrogenation catalyst is a conventional choice in the field, such as a homogeneous catalyst containing metals such as nickel and / or palladium, at least one of supported catalysts containing metals such as palladium and / or nickel, preferably at least one of supported catalysts containing palladium and / or nickel, more preferably at least one of supported catalysts such as palladium / carbon, palladium / silicon dioxide, and Raney nickel; preferably, the active metal content in the hydrogenation catalyst is 5-10wt%, such as 5, 6, 7, 8, 9, 10wt%;

[0014] The amount of the hydrogenation catalyst used is 2-15% of the mass of the norbornene monomer containing phenol or ammonia, for example, 2, 3, 4, 5, 6, 8, 10, 12, 14, 15%.

[0015] In the present invention, the pressure of the introduced hydrogen is 4-10 MPa, for example 4, 5, 6, 7, 8, 9, 10 MPa, preferably 5-10 MPa.

[0016] In the present invention, the hydrogenation reaction has a reaction temperature of 60-220°C, such as 60, 80, 100, 150, 170, 190, 210, 220°C, preferably 80-220°C; and a reaction time of 8-12h, such as 4, 5, 6, 7, 8, 9, 10, 11, 12h.

[0017] In the present invention, after the hydrogenation reaction is completed, post-treatment processes such as cooling, filtering, crystallization, washing, and drying are also included, which are conventional operations in the art and have no special requirements in the present invention.

[0018] In a third aspect, the present invention provides use of the above-mentioned phenol or amine compound containing a norbornene or norbornane structure in the preparation of polydicyclopentadiene.

[0019] A method for preparing polydicyclopentadiene, comprising the steps of:

[0020] Under nitrogen protection, dicyclopentadiene monomer, phenol or amine compound containing norbornene or norbornene structure, and main catalyst are added into the reaction kettle, and co-catalyst is added under mechanical stirring, and the mixture is rapidly mixed and reacted.

[0021] In the present invention, the molar ratio of the main catalyst, the co-catalyst and the dicyclopentadiene monomer is 1:10:2500 to 1:80:5000;

[0022] The amount of the phenol or amine compound containing norbornene or norbornene structure added is 5-25% of the mass of the dicyclopentadiene monomer.

[0023] The selected main catalyst is a tungsten catalyst and / or a molybdenum catalyst, preferably a tungsten catalyst with phenols, such as the one described in CN116063662A The R substituent may be H or an alkyl group below C10, preferably methyl, ethyl, propyl or butyl; the tungsten-based catalyst is preferably WOCl2(OC6H2-2,6-Cl2-4-CH3)2.

[0024] The co-catalyst is an organic tin compound and / or an alkyl aluminum compound, preferably an alkyl aluminum compound R n AlH 4-n , R can be methyl, ethyl, propyl, butyl, octyl, and the alkyl aluminum compound is preferably triethylaluminum or triisobutylaluminum;

[0025] The reaction temperature is 70-180° C. and the reaction time is 1-4 hours.

[0026] The beneficial effects of the present invention are:

[0027] The modified polydicyclopentadiene material of the invention has higher strength, toughness, excellent anti-aging performance and dielectric property. DETAILED DESCRIPTION

[0028] In order to better understand the technical solution of the present invention, the content of the present invention is further described below in conjunction with the following specific embodiments, but the content of the present invention is not limited to the following embodiments.

[0029] The sources of the main raw materials in the examples and comparative examples of the present invention are as follows. Other sources are obtained from common commercial channels unless otherwise specified:

[0030] Palladium on carbon (5%): Beijing Inokai Technology Co., Ltd.;

[0031] 3,6-Bis(4-aminophenoxy)benzonorbornene: synthesized according to patent CN113511980B;

[0032] Tungsten catalyst with phenols: synthesized according to CN116063662A;

[0033] Dicyclopentadiene: Beijing Inokai Technology Co., Ltd.;

[0034] Triisobutyl aluminum: Beijing Inokai Technology Co., Ltd.;

[0035] Triethylaluminum: Beijing Inokai Technology Co., Ltd.;

[0036] 3,6-Dihydroxy-benzonorbornene: Beijing Inokai Technology Co., Ltd.

[0037] Example 1

[0038] Preparation of cyclohexane-norbornane compounds containing phenolic groups:

[0039] Add 16.5g of palladium carbon (5%) catalyst to the reactor, and under nitrogen conditions, add 110g of 3,6-dihydroxy-benzonorbornene and 1L of anhydrous ethanol to a 2L reactor, replace with nitrogen three times, replace with hydrogen three times, maintain a hydrogen environment, then heat the system to 200°C, set the hydrogen pressure to 5MPa, and react for 8h. After the reaction is completed, filter to remove the palladium carbon catalyst, pour the filtrate into a large amount of water, crystallize at low temperature, collect the precipitate, filter, wash, and vacuum dry to obtain 106g of white powder, i.e. 3,6-dihydroxy-cyclohexane and norbornene.

[0040] The structure is:

[0041] Characterization: H 1 NMR(CDCl3)δ1.00-3.00(14,m),3.50-5.00(2,m),3.50-5.00(2,s).

[0042] Example 2

[0043] Preparation of aminobenzonorbornane containing compounds:

[0044] Add 2.25g of palladium carbon (5%) catalyst to the reactor, and under nitrogen conditions, add 112.5g of 3,6-bis(4-aminophenoxy)benzonorbornene and 1L of anhydrous ethanol to a 2L reactor, replace with nitrogen three times, replace with hydrogen three times, maintain a hydrogen environment, then heat the system to 60°C, set the hydrogen pressure to 5MPa, and react for 12h. After the reaction is completed, filter to remove the palladium carbon catalyst, pour the filtrate into a large amount of water, crystallize at low temperature, collect the precipitate, filter, wash, and vacuum dry to obtain 108.4g of white powder, i.e. 3,6-bis(4-aminophenoxy)benzonorbornene.

[0045] The structure is:

[0046] Symptoms: H 1 NMR(CDCl3)δ1.00-2.00(6H,m),2.00-4.00(2H,m),5.00-6.00(4H,s),6.00-7.00(10H,m).

[0047] Example 3

[0048] Preparation of aminocyclohexane-norbornane-containing compounds:

[0049] Referring to Example 1 of CN117776939A, 3,6-bis(4-aminocyclohexyloxy)cyclohexane and norbornane were prepared.

[0050] The structure is:

[0051] Preparation of polydicyclopentadiene

[0052] Example 4

[0053] Using 3,6-dihydroxy-benzonorbornene

[0054] Under a nitrogen environment, 100 g (0.76 mol) of dicyclopentadiene, 294.5 mg (0.152 mmol) of WOCl2 (OC6H2-2,6-Cl2-4-CH3), and 15 g of 3,6-dihydroxy-benzonorbornene were added to a reactor, and then 12.2 ml (1 mol / L) of triisobutylaluminum / toluene solution was added. The mixture was rapidly stirred for 3 min, and then the pressure was increased. The reaction fluid was pressed into the mold by pressure and reacted at 180 ° C for 4 h.

[0055] The molar ratio of the main catalyst, the co-catalyst and the dicyclopentadiene monomer is 1:80:5000, and the added amount of 3,6-dihydroxy-benzonorbornene is 15% of the mass of the dicyclopentadiene monomer.

[0056] Example 5

[0057] Under nitrogen environment, 100g (0.76mol) of dicyclopentadiene, 2189mg (0.304mmol) of WOCl2 (OC6H2-2,6-Cl2-4-CH3), and 5g of 3,6-dihydroxy-benzonorbornene were added to the reaction kettle, and then 3ml (1mol / L) of triisobutylaluminum / toluene solution was added. The mixture was rapidly stirred for 3min, and then the pressure was increased. The reaction liquid was pressed into the mold by pressure and reacted at 70°C for 1h.

[0058] The molar ratio of the main catalyst, the co-catalyst and the dicyclopentadiene monomer is 1:10:2500, and the added amount of 3,6-dihydroxy-benzonorbornane is 5% of the mass of the dicyclopentadiene monomer.

[0059] Example 6

[0060] Under a nitrogen environment, 100 g (0.76 mol) of dicyclopentadiene, 2158 mg (0.2533 mmol) of WOCl2 (OC6H2-2,6-Cl2-4-CH3), and 10 g of 3,6-dihydroxy-cyclohexane and norbornene were added to a reactor, and then 12.5 ml (1 mol / L) of triethylaluminum toluene solution was added. The mixture was rapidly stirred for 3 minutes, and then the pressure was increased. The reaction liquid was pressed into the mold by pressure and reacted at 90°C for 2 hours.

[0061] The molar ratio of the main catalyst, the co-catalyst and the dicyclopentadiene monomer is 1:50:3000, wherein the added 3,6-dihydroxy-cyclohexane-norbornane accounts for 10% of the mass of the dicyclopentadiene monomer.

[0062] Example 7

[0063] The amounts of main catalyst, co-catalyst and dicyclopentadiene monomer added were the same as those in Example 4. 3,6-dihydroxybenzonorbornene was replaced with 3,6-bis(4-aminophenoxy)benzonorbornene in an amount of 25 g. The reaction temperature was set to 150° C. and the reaction time was 2 h.

[0064] Example 8

[0065] The amounts of the main catalyst, co-catalyst and dicyclopentadiene monomer added are the same as those in Example 5. 3,6-dihydroxybenzonorbornane is replaced with 3,6-bis(4-aminophenoxy)benzonorbornane in an amount of 20 g. The reaction temperature and reaction time are the same as those in Example 5.

[0066] Example 9

[0067] The amounts of the main catalyst, co-catalyst and dicyclopentadiene monomer added are the same as those in Example 6. 3,6-dihydroxy-cyclohexane-norbornane is replaced with 3,6-bis(4-aminocyclohexyloxy)cyclohexane-norbornane in an amount of 16 g. The reaction temperature and reaction time are the same as those in Example 6.

[0068] Comparative Example 1

[0069] The amounts of the main catalyst, the co-catalyst and the dicyclopentadiene monomer added are the same as those in Example 4, the amount of 3,6-dihydroxy-benzonorbornene added is 0, and the reaction temperature and reaction time are the same as those in Example 4.

[0070] In each embodiment and comparative example of the present invention, the performance test parameters and corresponding test methods are as follows:

[0071] Tensile strength: GB / T 1040.1-2018;

[0072] Elongation at break: GB / T 1040.1-2018;

[0073] Contact angle: GB / T 30693-2014;

[0074] Aging test: GB / T 3512-2014;

[0075] Impact strength: GB / T 1043.1-2008;

[0076] Dielectric properties: GB / T1409-2006;

[0077] In each embodiment and comparative example of the present invention, the test results of tensile strength, elongation at break and contact angle performance are shown in Table 1:

[0078] Table 1 Performance test results of embodiments and comparative examples

[0079] sample Tensile strength(MPa) Elongation at break / % Contact angle / ° Example 4 58.6 8.1 20.5 Example 5 56.5 7.2 26.4 Example 6 57.4 7.5 20.4 Example 7 59.2 7.2 21.3 Example 8 56.2 7.5 20.5 Example 9 57.4 7.8 23.5 Comparative Example 1 45.2 4.2 83.5

[0080] In each embodiment and comparative example of the present invention, the aging performance test results are shown in Table 2:

[0081] Table 2 Performance test results of embodiments and comparative examples

[0082]

[0083]

[0084] In each embodiment and comparative example of the present invention, the dielectric properties test results are shown in Table 3:

[0085] Table 3 Dielectric properties test results of examples and comparative examples

[0086]

Claims

1. A polydicyclopentadiene, characterized in that: The raw material contains a phenol or amine compound containing a norbornene or norbornene structure, selected from the following structures:

2. The polydicyclopentadiene according to claim 1, characterized in that The amount of the phenol or amine compound containing norbornene or norbornene structure added is 5-25% of the mass of the dicyclopentadiene monomer.

3. A method for preparing polydicyclopentadiene, comprising: Under nitrogen protection, dicyclopentadiene monomer, phenol or amine compound containing norbornene or norbornene structure, main catalyst are added into a reaction kettle, and a co-catalyst is added to react; The phenol or amine compound containing a norbornene or norbornene structure is selected from the following structures:

4. The method according to claim 3, wherein: The amount of the phenol or amine compound containing norbornene or norbornene structure added is 5-25% of the mass of the dicyclopentadiene monomer.

5. The method according to claim 3 or 4, wherein: The molar ratio of the main catalyst, the co-catalyst and the dicyclopentadiene monomer is 1:10:2500 to 1:80:5000.

6. The method according to any one of claims 3 to 5, wherein: The main catalyst is a tungsten catalyst and / or a molybdenum catalyst, preferably a tungsten catalyst with phenols, such as WOCl2(OC6H2-2,6-Cl2-4-CH3)2.

7. The method according to any one of claims 3 to 6, wherein: The co-catalyst is an organic tin compound and / or an alkyl aluminum compound, preferably an alkyl aluminum compound R n AlH 4-n , R is methyl, ethyl, propyl, butyl, or octyl, and the alkyl aluminum compound is preferably triethylaluminum or triisobutylaluminum.

8. The method according to any one of claims 3 to 7, wherein: The reaction temperature is 70-180° C. and the reaction time is 1-4 hours.

Citation Information

Patent Citations

  • Macromolecular polymerized phenol modified polydicyclopentadiene material and preparation method thereof

    CN104292395A

  • Intrinsic flame-retardant polydicyclopentadiene containing double norbornene flame-retardant monomer and preparation method of intrinsic flame-retardant polydicyclopentadiene

    CN117327113A

  • Production of hydrogenated dicyclopentadiene ring-opening polymer

    JP1995252316A

  • A method for controlling hardening rate of polydicyclopentadiene

    KR102041531B1

  • Ring-opened copolymers of dihydrodiclopentadiene, norbornene or alkylnorbornene, and acyclic olefin

    US4136249A