Solvent-resistant and heat-resistant nylon and preparation method thereof

Through the high-compression condensation reaction of biphenyl diamine and aromatic dibasic acid, solvent-resistant and heat-resistant nylon was prepared, which solved the problem of insufficient resistance to organic solvents by traditional nylon materials, and improved their solvent-resistant, heat-resistant and Mechanical properties and simplify the preparation process, suitable for industrial applications.

CN118772398BActive Publication Date: 2024-11-19CHUANHUA GRP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411260235.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-19
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

Traditional nylon materials have weak resistance to organic solvents, resulting in limited application in certain industrial fields, and are cumbersome in preparation methods and poor mechanical and thermal resistance.

Method used

Biphenyl diamine and aromatic dibasic acid are used as raw materials to react through specific high-compression condensation and gradient heating conditions to prepare solvent-resistant and heat-resistant nylon to improve its solvent-resistant and heat-resistant properties.

Benefits of technology

The obtained nylon material has excellent solvent resistance, heat resistance and mechanical properties, low water absorption rate, and simple and easy to prepare, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772398B_ABST
    Figure CN118772398B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polymer materials and relates to a solvent-resistant and heat-resistant nylon and a preparation method thereof. The preparation raw materials include biphenyl diamine and aromatic dibasic acid; the biphenyl diamine is selected from at least one of 9,9-bis(4-aminophenyl)fluorene, 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl, 4,4'-diaminobiphenyl, 1,1'-biphenyl-3,3'-dimethyldimethylamine, 1,1'-biphenyl-3,3'-diamine, 2,2'-dimethyl-1,1'-biphenyl-3,3'-diamine, 4,4'-diaminoterphenyl, and 4,4'-diamino-3,3'-dimethylbiphenyl; the aromatic dibasic acid is selected from at least one of 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 9-threonone-2,7-dicarboxylic acid, and 4,4'-biphenyldicarboxylic acid. The nylon of the invention has excellent solvent resistance, heat resistance and mechanical properties, and has lower water absorption rate and higher yield and molecular weight.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to a solvent-resistant and heat-resistant nylon and a preparation method thereof. Background Art

[0002] Nylon (PA) is a type of polymer containing -CO-NH- in the repeating unit. As one of the five general-purpose engineering plastics, it has excellent mechanical properties, good biocompatibility, outstanding wear resistance and low water absorption. It is widely used in engineering, medical and health, electronic appliances, automotive parts and other fields.

[0003] However, due to the presence of a large number of polar amide groups in the molecular chain of traditional nylon materials, solvent molecules are prone to interact with nylon materials, resulting in the penetration and absorption of solvents. Therefore, its resistance to organic solvents is relatively weak, which will cause nylon materials to swell, soften, or even dissolve in some organic solvent environments, reducing the stability and durability of the materials and limiting their application in certain industrial fields. In addition, the preparation methods of existing nylon materials are cumbersome, and the obtained nylons often have problems with poor mechanical properties and heat resistance. Therefore, the preparation of solvent-resistant and high-heat-resistant nylon has become a hot topic in the field of polymer material technology in recent years. Summary of the invention

[0004] In order to solve the defects in the prior art, the present invention provides a solvent-resistant and heat-resistant nylon and a preparation method thereof. The nylon prepared thereby has excellent solvent resistance, heat resistance, mechanical properties, lower water absorption, higher yield and molecular weight.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a solvent-resistant and heat-resistant nylon, wherein the raw materials for preparing the nylon include biphenyl-type diamine and aromatic dibasic acid;

[0007] The biphenyl type diamine is selected from at least one of 9,9-bis(4-aminophenyl)fluorene, 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl, 4,4'-diaminobiphenyl, 1,1'-biphenyl-3,3'-dimethyldimethylamine, 1,1'-biphenyl-3,3'-diamine, 2,2'-dimethyl-1,1'-biphenyl-3,3'-diamine, 4,4'-diaminoterphenyl, and 4,4'-diamino-3,3'-dimethylbiphenyl;

[0008] The aromatic dibasic acid is at least one selected from 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 9-threonone-2,7-dicarboxylic acid, and 4,4'-biphenyldicarboxylic acid.

[0009] Preferably, the molar ratio of the biphenyl diamine to the aromatic dibasic acid is 1:(0.6-1). More preferably, the molar ratio of the biphenyl diamine to the aromatic dibasic acid is 1:1.

[0010] Preferably, the biphenyl diamine is 9,9-bis(4-aminophenyl)fluorene.

[0011] Preferably, the aromatic dibasic acid is 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid.

[0012] Preferably, the structural formula of the solvent-resistant and heat-resistant nylon is as shown in Formula I below:

[0013]

[0014] Formula I.

[0015] More preferably, the number average molecular weight of the solvent-resistant and heat-resistant nylon is 59,000-69,000.

[0016] In a second aspect, the present invention provides a method for preparing solvent-resistant and heat-resistant nylon, comprising the following steps:

[0017] S1. Mixing a biphenyl diamine, an aromatic dibasic acid and a solvent in a protective atmosphere to obtain a mixture; the biphenyl diamine is selected from at least one of 9,9-bis(4-aminophenyl)fluorene, 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl, 4,4'-diaminobiphenyl, 1,1'-biphenyl-3,3'-dimethyldimethylamine, 1,1'-biphenyl-3,3'-diamine, 2,2'-dimethyl-1,1'-biphenyl-3,3'-diamine, 4,4'-diaminoterphenyl and 4,4'-diamino-3,3'-dimethylbiphenyl; the aromatic dibasic acid is selected from at least one of 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 9-threonone-2,7-dicarboxylic acid and 4,4'-biphenyldicarboxylic acid;

[0018] S2, the mixture is stirred at elevated temperature, and after reaching the target temperature, pressurized for condensation reaction to obtain reactant 1;

[0019] S3, reacting the reactant 1 under conditions of gradient temperature increase and pressure increase to obtain reactant 2;

[0020] S4, after depressurizing and heating, react in a vacuum environment to obtain solvent-resistant and heat-resistant nylon.

[0021] Preferably, the molar ratio of the biphenyl diamine to the aromatic dibasic acid is 1:(0.6-1). More preferably, the molar ratio of the biphenyl diamine to the aromatic dibasic acid is 1:1.

[0022] Preferably, the mass of the solvent accounts for 30-50% of the sum of the mass of the biphenyl diamine and the aromatic dibasic acid.

[0023] Preferably, the protective atmosphere in S1 is selected from any one of nitrogen, argon, helium and neon.

[0024] Preferably, a catalyst is also added to S1.

[0025] Preferably, the catalyst is selected from at least one of sodium hypophosphite, sodium hypophosphite, dibutyltin oxide, potassium hypophosphite, zinc oxide, potassium hypophosphite, tin oxide, magnesium hypophosphite, calcium hypophosphite, stannous chloride and zinc acetate.

[0026] Preferably, the mass of the catalyst accounts for 0.1-0.25% of the sum of the mass of the biphenyl diamine and the aromatic dibasic acid.

[0027] Preferably, the stirring speed in S2 is 200-300 r / min, and the target temperature is 90-120 °C.

[0028] Preferably, the pressurized pressure in S2 is 0.4-0.9 Mpa.

[0029] Preferably, the reaction time of the S2 condensation reaction is 1 to 3 h.

[0030] Preferably, the gradient temperature increase condition in S3 is: increasing the temperature to 240-280° C. at a heating rate of 20-30° C. / min.

[0031] Preferably, the pressure of the pressurized environment in S3 is 3-5 Mpa.

[0032] Preferably, the reaction time after the heating in S3 is completed is 1 to 3 h.

[0033] Preferably, the pressure after decompression in S4 is 0.3-0.6 Mpa.

[0034] Preferably, the temperature in S4 is raised to 320-360 °C.

[0035] Preferably, the reaction time of S4 is 2 to 4 h.

[0036] The beneficial effects of the present invention are:

[0037] The invention introduces a biphenyl structure into the main chain of nylon, which can effectively improve the solvent resistance of nylon and improve the heat resistance of nylon at the same time. The obtained nylon has excellent solvent resistance, heat resistance and mechanical properties, low water absorption, high yield and molecular weight, and excellent comprehensive performance, thereby expanding the application range of nylon materials.

[0038] The preparation method of the invention is simple, easy to implement, green and environmentally friendly, has high economic benefits, and can realize large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a Fourier infrared spectrum characterization diagram of the solvent-resistant and heat-resistant nylon prepared in Example 3. DETAILED DESCRIPTION

[0040] In order to enable those skilled in the art to better understand the technical solution of the invention, the present invention is further described in detail below in conjunction with specific implementation methods.

[0041] Example 1

[0042] This embodiment provides a method for preparing solvent-resistant and heat-resistant nylon, and the steps are as follows:

[0043] S1. Add 348.4 g 9,9-bis(4-aminophenyl)fluorene, 194.6 g 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid (the molar ratio of 9,9-bis(4-aminophenyl)fluorene to 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid is 1:0.6), 0.8 g sodium hypophosphite (0.15% of the sum of the mass of 9,9-bis(4-aminophenyl)fluorene and 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid) and 217.2 g iodine into a magnetically driven high pressure reactor. g deionized water (40% of the sum of the mass of 9,9-bis(4-aminophenyl)fluorene and 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid), and N2 was introduced to replace the air in the reactor;

[0044] S2, start the heating and stirring program of the magnetically driven high-pressure reactor, set the stirring speed to 250 r / min, and after the temperature rises to 100 °C, inflate the reactor and pressurize it to 0.5 MPa, and carry out the condensation reaction for 2 h to obtain reactant 1;

[0045] S3, heating the magnetically driven high-pressure reactor to 250 °C at a heating rate of 20 °C / min, and setting the reactor pressure to 4 MPa. After reaching the temperature, react for 2 h to obtain reactant 2;

[0046] S4, release the pressure to 0.3 MPa, raise the temperature to 340 °C, and conduct a vacuum reaction for 2 h, then pressurize and discharge the material to obtain solvent-resistant and heat-resistant nylon (PA-BT-1).

[0047] The structural formula of the obtained solvent-resistant and heat-resistant nylon is as follows:

[0048]

[0049] Example 2

[0050] This embodiment provides a method for preparing solvent-resistant and heat-resistant nylon, and the steps are as follows:

[0051] S1. Add 348.4 g of 9,9-bis(4-aminophenyl)fluorene, 259.5 g of 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid (the molar ratio of 9,9-bis(4-aminophenyl)fluorene to 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid is 1:0.8), 0.9 g of sodium hypophosphite (0.15% of the sum of the mass of 9,9-bis(4-aminophenyl)fluorene and 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid) and 243.2 g of sodium phosphate to a magnetically driven high-pressure reactor. g deionized water (40% of the sum of the mass of 9,9-bis(4-aminophenyl)fluorene and 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid), and N2 was introduced to replace the air in the reactor;

[0052] The steps of S2 to S4 are the same as those of Example 1 to obtain solvent-resistant and heat-resistant nylon (PA-BT-2).

[0053] The structural formula of the obtained solvent-resistant and heat-resistant nylon is the same as that of Example 1.

[0054] Example 3

[0055] This embodiment provides a method for preparing solvent-resistant and heat-resistant nylon, and the steps are as follows:

[0056] S1. Add 348.4 g of 9,9-bis(4-aminophenyl)fluorene, 324.4 g of 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid (the molar ratio of 9,9-bis(4-aminophenyl)fluorene to 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid is 1:1), 1.0 g of sodium hypophosphite (0.15% of the total mass of 9,9-bis(4-aminophenyl)fluorene and 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid) and 269.1 g of deionized water (40% of the total mass of 9,9-bis(4-aminophenyl)fluorene and 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid) into a magnetically driven high-pressure reactor, and replace the air in the reactor with N2;

[0057] The steps of S2 to S4 are the same as those of Example 1 to obtain solvent-resistant and heat-resistant nylon (PA-BT-3).

[0058] The structural formula of the obtained solvent-resistant and heat-resistant nylon is the same as that of Example 1.

[0059] Example 4

[0060] The step of S1 is the same as that of Example 1;

[0061] S2, start the heating and stirring program of the magnetically driven high-pressure reactor, set the stirring speed to 200 r / min, and after the temperature rises to 90 °C, inflate the reactor and pressurize it to 0.4 MPa, and carry out the condensation reaction for 1 h to obtain reactant 1;

[0062] S3, heating the magnetically driven high-pressure reactor to 240 °C at a heating rate of 25 °C / min, and setting the reactor pressure to 3 MPa. After reaching the temperature, react for 1 h to obtain reactant 2;

[0063] S4, release the pressure to 0.3 MPa, raise the temperature to 320 °C, and conduct a vacuum reaction for 2 h, then pressurize and discharge the material to obtain solvent-resistant and heat-resistant nylon (PA-BT-4).

[0064] The structural formula of the obtained solvent-resistant and heat-resistant nylon is the same as that of Example 1.

[0065] Example 5

[0066] The step of S1 is the same as that of Example 1;

[0067] S2, start the heating and stirring program of the magnetically driven high-pressure reactor, set the stirring speed to 300 r / min, and after the temperature rises to 120 °C, inflate the reactor and pressurize it to 0.9 MPa, and carry out the condensation reaction for 3 h to obtain reactant 1;

[0068] S3, heating the magnetically driven high-pressure reactor to 280 °C at a heating rate of 30 °C / min, and setting the reactor pressure to 5 MPa. After reaching the temperature, react for 3 h to obtain reactant 2;

[0069] S4, release the pressure to 0.6 MPa, raise the temperature to 360 ° C, and vacuum the reaction for 4 hours, then pressurize and discharge the material to obtain solvent-resistant and heat-resistant nylon (PA-BT-5).

[0070] The structural formula of the obtained solvent-resistant and heat-resistant nylon is the same as that of Example 1.

[0071] Example 6

[0072] Same as Example 1, except that:

[0073] The mass of the deionized water accounts for 30% of the sum of the mass of the biphenyl diamine and the aromatic dibasic acid;

[0074] The mass of the sodium hypophosphite accounts for 0.1% of the sum of the mass of the biphenyl diamine and the aromatic dibasic acid;

[0075] Solvent-resistant and heat-resistant nylon (PA-BT-6) was obtained.

[0076] The structural formula of the obtained solvent-resistant and heat-resistant nylon is the same as that of Example 1.

[0077] Example 7

[0078] Same as Example 1, except that:

[0079] The mass of the deionized water accounts for 50% of the sum of the mass of the biphenyl diamine and the aromatic dibasic acid;

[0080] The mass of the sodium hypophosphite accounts for 0.25% of the sum of the mass of the biphenyl diamine and the aromatic dibasic acid;

[0081] Solvent-resistant and heat-resistant nylon (PA-BT-7) was obtained.

[0082] The structural formula of the obtained solvent-resistant and heat-resistant nylon is the same as that of Example 1.

[0083] Comparative Example 1

[0084] This comparative example provides a method for preparing nylon, and the steps are as follows:

[0085] S1. Add 172.3 g of decanediamine, 324.4 g of 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid (the molar ratio of decanediamine to 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid is 1:1), 0.7 g of sodium hypophosphite (0.15% of the sum of the mass of decanediamine and 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid) and 198.7 g of deionized water (40% of the sum of the mass of decanediamine and 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid) into a magnetically driven high-pressure reactor, and replace the air in the reactor with N2;

[0086] The steps of S2 to S4 are the same as those of Example 1 to obtain nylon (PA-1).

[0087] Comparative Example 2

[0088] This comparative example provides a method for preparing nylon, and the steps are as follows:

[0089] S1. Add 348.4 g of 9,9-bis(4-aminophenyl)fluorene, 202.2 g of sebacic acid (the molar ratio of 9,9-bis(4-aminophenyl)fluorene to sebacic acid is 1:1), 0.8 g of sodium hypophosphite (0.15% of the sum of the mass of 9,9-bis(4-aminophenyl)fluorene and sebacic acid) and 220.2 g of deionized water (40% of the sum of the mass of 9,9-bis(4-aminophenyl)fluorene and sebacic acid) into a magnetically driven high-pressure reactor, and replace the air in the reactor with N2;

[0090] The steps of S2 to S4 are the same as those of Example 1 to obtain nylon (PA-2).

[0091] Effect Example 1 Fourier Infrared Spectroscopy Characterization

[0092] The nylon prepared in Example 3 was characterized by infrared spectroscopy. Figure 1 .

[0093] Depend on Figure 1 It can be seen that 3482 cm -1 The characteristic peaks near 2952 cm are attributed to the NH stretching vibration absorption peak on polyamide; -1 The characteristic peaks at 1632 cm-1 are respectively attributed to the antisymmetric and symmetric CH stretching vibration absorption peaks on polyamide (amide band I). -1 The characteristic peaks near 1290 cm-1 are attributed to the -CO-NH- bending vibration (amide band II) of polyamide. -1 The characteristic peaks nearby are attributed to the combined absorption peaks of CN stretching vibration and CH in-plane bending vibration.

[0094] Effect Example 2: Solvent resistance test

[0095] The solvent resistance of the nylon prepared in the examples and comparative examples was tested, and the results are shown in Table 1.

[0096] Test method: GB / T 11547-2008 Determination of resistance of plastics to liquid chemical reagents

[0097] Evaluation indicators: "Excellent" means that the material hardly swells, dissolves or undergoes other obvious changes in the solvent, and has very good solvent resistance; "Good" means that the material has a good ability to resist solvents, and swelling or other changes are relatively small; "Poor" means that the material is more easily affected by the solvent, and there will be obvious swelling, partial dissolution or performance degradation.

[0098] Table 1. Solvent resistance test results

[0099]

[0100] It can be seen from Table 1 that the nylon prepared in the examples of the present invention has good solvent resistance in various organic or inorganic solvents, while the nylon prepared in the comparative example has relatively poor solvent resistance in different solvents.

[0101] Effect Example 3 Thermal Performance Test

[0102] The thermal properties of the nylon prepared in the examples and comparative examples were tested, and the results are shown in Table 2.

[0103] Table 2. Thermal performance test results

[0104]

[0105] It can be seen from Table 2 that the nylon prepared in the embodiment of the present invention has T d5% and T g The values ​​are relatively high, significantly higher than those of the comparative examples, which reflects the excellent thermal properties of the nylon prepared by the present invention, while the comparative examples 1 and 2 which do not use the raw materials of the present invention, T d5% and T g The lower the value, the worse the thermal performance.

[0106] Effect Example 4 Mechanical Properties Test

[0107] The mechanical properties of the nylon prepared in the examples and comparative examples were tested, and the results are shown in Table 3.

[0108] Table 3. Mechanical properties test results

[0109]

[0110] It can be seen from Table 3 that the tensile strength of the nylon prepared in the embodiment of the present invention is significantly higher than that in the comparative example, which reflects the excellent mechanical properties of the nylon of the present invention. However, the comparative examples 1 and 2 that do not use the raw materials of the present invention have lower tensile strength and poorer mechanical properties.

[0111] Effect Example 5 Water Absorption Performance Test

[0112] The water absorption performance of the nylon prepared in the embodiment and the comparative example was tested, and the results are shown in Table 4.

[0113] Table 4. Water absorption test results

[0114]

[0115] It can be seen from Table 4 that the water absorption rate of the nylon prepared in the embodiment of the present invention is relatively low, indicating that the nylon prepared in the present invention is not easy to absorb water, while the water absorption rates of Comparative Examples 1 and Comparative Examples 2 which do not use the raw materials of the present invention are relatively high.

[0116] Effect Example 6 Yield and Molecular Weight Test

[0117] The water absorption performance of the nylon prepared in the embodiment and the comparative example was tested, and the results are shown in Table 5.

[0118] Table 5. Yield and molecular weight test results

[0119]

[0120] It can be seen from Table 5 that the yield and molecular weight of the nylon prepared in the embodiment of the present invention are higher than those of the nylon prepared in the comparative example.

[0121] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing solvent-resistant and heat-resistant nylon, It is characterized in that The following steps are involved: S1. Mixing biphenyl diamine, aromatic dibasic acid, catalyst and solvent in a protective atmosphere to obtain a mixture; wherein the biphenyl diamine is selected from 9,9-bis(4-aminophenyl)fluorene, 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl, 4,4'-diaminobiphenyl, 1,1'-biphenyl-3,3'-dimethyldimethylamine, 1,1'-biphenyl-3,3'-diamine, 2,2'-dimethyl-1,1'-biphenyl-3,3'-diamine, 4,4'-diaminoterphenyl, 4,4'-diamino-3,3'-diamine. At least one of methyl biphenyl; the aromatic dibasic acid is selected from at least one of 1,1,3-trimethyl-3-phenylindane-4,5-dicarboxylic acid, 2,2'-biphenyl dicarboxylic acid, 9-threonone-2,7-dicarboxylic acid, and 4,4'-biphenyl dicarboxylic acid; the molar ratio of the biphenyl diamine to the aromatic dibasic acid is 1:(0.6~1); the mass of the catalyst accounts for 0.1~0.25% of the sum of the mass of the biphenyl diamine and the aromatic dibasic acid; the mass of the solvent accounts for 30~50% of the sum of the mass of the biphenyl diamine and the aromatic dibasic acid; S2, the mixture is stirred at elevated temperature, and after reaching the target temperature, pressurized for condensation reaction to obtain reactant 1; S3, reacting the reactant 1 under conditions of gradient temperature increase and pressure increase to obtain reactant 2; S4, after depressurizing and heating, react in a vacuum environment to obtain solvent-resistant and heat-resistant nylon.

2. The preparation method according to claim 1, It is characterized in that The catalyst is selected from at least one of sodium hypophosphite, sodium hypophosphite, dibutyltin oxide, potassium hypophosphite, zinc oxide, potassium hypophosphite, tin oxide, magnesium hypophosphite, calcium hypophosphite, stannous chloride and zinc acetate.

3. The preparation method according to claim 1, It is characterized in that The stirring speed in S2 is 200-300 r / min, and the target temperature is 90-120 °C.

4. The preparation method according to claim 1, It is characterized in that The pressurized pressure in S2 is 0.4~0.9Mpa.

5. The preparation method according to claim 1, It is characterized in that The conditions for the gradient heating in S3 are: heating to 240-280°C at a heating rate of 20-30°C / min.

6. The preparation method according to claim 1, It is characterized in that In the S4, the temperature is raised to 320-360°C.

7. A solvent-resistant and heat-resistant nylon, It is characterized in that The method is prepared according to any one of claims 1 to 6.

8. The solvent-resistant and heat-resistant nylon according to claim 7, It is characterized in that The structural formula of the solvent-resistant and heat-resistant nylon is shown in Formula I below: Formula I.

Citation Information

Patent Citations

  • Aromatic polyamide films for solvent resistant flexible substrates

    CN104884507A

  • Meta-aramid resin for fibrid, fibrid, aramid paper and synthesis method

    CN112812294A

  • High-toughness wear-resistant composite material for rail transit fasteners

    CN114907689A

  • Phosphorus-free halogen-free flame-retardant polyamide as well as preparation method and application thereof

    CN117209752A

  • Biphenyltetracarboxylic acid dianhydride, method for producing the same, polyimide using the same and method for producing the same

    JP2006045198A