Preparation method and application of halogen-free flame retardant with high temperature thermal stability and no discoloration

Through the acid-base reaction of orthophosphoric acid and hexanediamine and the dehydration and polycondensation reaction of orthophosphoric acid, the obtained polyphosphoric acid organic amine salt has a stable and does not discolor at high temperature, which solves the problem of existing halogen-free flame retardants at high temperatures. The problem of easy discoloration and poor thermal stability is suitable for the flame retardant requirements of high-temperature processing resins.

CN118772420BActive Publication Date: 2024-12-03CHENGDU FULAILONG TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411270268.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-03
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The existing halogen-free flame retardants are prone to discoloration at high temperatures and have poor thermal stability, which cannot meet the flame retardant requirements of resins such as PA, PET, etc. with processing temperatures above 220°C.

Method used

The acid-base reaction of orthophosphoric acid and hexanediamine, dehydration and polycondensation reaction of orthophosphoric acid and hexanediamine, dehydration and polycondensation reaction, polyphosphate organic amine salt with phosphorus-nitrogen structure is prepared as a halogen-free flame retardant, and a mixed solvent of water and sulfolane or silicone oil is used. , control the reaction temperature and time, and carry out reaction under vacuum conditions.

Benefits of technology

The halogen-free flame retardant produced has good thermal stability and is not easy to discolor at high temperatures of 280-300℃. It is suitable for flame retardant of glass fiber reinforced systems such as PA, PET, PBT, PP, PE, etc., and improves the flame retardant with resin. Compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772420B_ABST
    Figure CN118772420B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of flame retardants, and in particular to a preparation method and application of a halogen-free flame retardant with high temperature thermal stability and no discoloration, wherein a phosphorus-containing inorganic acid and an organic dibasic base are subjected to acid-base reaction, dehydration pyrophosphorylation reaction, and dehydration polycondensation reaction to obtain a polyphosphate organic amine salt containing phosphorus and nitrogen as a halogen-free flame retardant. The present invention adopts the preparation method and application of the above-mentioned halogen-free flame retardant with high temperature thermal stability and no discoloration, and the prepared halogen-free flame retardant has good compatibility with resin, high thermal stability, and is not easy to discolor, which conforms to the development direction of phosphorus environmentally friendly flame retardants and solves the flame retardant demand of high temperature processing resins.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardants, and in particular to a preparation method and application of a halogen-free flame retardant with high-temperature thermal stability and no discoloration. Background Art

[0002] Halogen-free flame retardants refer to flame retardant materials that do not contain halogen elements (such as chlorine and bromine). Compared with halogen-containing flame retardants, they produce less harmful gases when burned and are more in line with environmental protection requirements. The development of halogen-free flame retardants has made great progress in recent years, but there are still few flame retardants with high stability, high compatibility, and high carbonization. In addition, the economical pyrophosphate flame retardants in the prior art still have the disadvantages of easy discoloration at high temperatures and poor thermal stability. For example, pyrophosphate piperazine turns red at 220°C and degrades quickly at 290°C. It cannot be used for resins with processing temperatures above 220°C, such as PA and PET. For this reason, the development of halogen-free flame retardants with high temperature thermal stability and no discoloration has become an urgent need for the development of flame retardants. Summary of the invention

[0003] The purpose of the present invention is to provide a preparation method and application of a halogen-free flame retardant with high-temperature thermal stability and no discoloration. The prepared halogen-free flame retardant has good compatibility with resin, high thermal stability, and is not easy to discolor. It conforms to the development direction of phosphorus environmentally friendly flame retardants and solves the flame retardant needs of high-temperature processing resins.

[0004] To achieve the above object, the present invention provides a method for preparing a halogen-free flame retardant with high temperature thermal stability and no discoloration, wherein an organic polyphosphate amine salt containing phosphorus and nitrogen is prepared as a halogen-free flame retardant by acid-base reaction, dehydration pyrophosphorylation reaction, and dehydration polycondensation reaction of orthophosphoric acid and hexamethylenediamine, and the structural formula of the organic polyphosphate amine salt is as follows:

[0005]

[0006] In the formula, n is an integer greater than 2.

[0007] Preferably, the molar ratio of orthophosphoric acid to hexamethylenediamine in the acid-base reaction is 2 to 1:1.

[0008] Preferably, the solvent used in the acid-base reaction is a mixture of water and sulfolane or silicone oil, and the weight ratio of water to sulfolane or silicone oil is 5:1.

[0009] Preferably, the acid-base reaction is carried out at a temperature of 40 to 100° C. and normal pressure for 0.5 to 3 hours.

[0010] Preferably, the temperature of the dehydration pyrophosphorylation reaction is 220-270° C., and the reaction time is 1-5 h.

[0011] Preferably, the temperature of the dehydration polycondensation reaction is 260-320° C., and the reaction time is 0.5 to 2 h.

[0012] Preferably, the dehydration pyrophosphorylation reaction and the dehydration polycondensation reaction are both carried out under vacuum conditions, with a vacuum degree of -0.06 to -0.099 MPa.

[0013] Preferably, the reaction equation of the acid-base reaction is as follows:

[0014]

[0015] The reaction equation for dehydration pyrophosphorylation is as follows:

[0016]

[0017] The reaction equation of dehydration polycondensation is as follows:

[0018]

[0019] The invention discloses an application of a halogen-free flame retardant with high temperature thermal stability and no discoloration. The halogen-free flame retardant with high temperature thermal stability and no discoloration prepared by the preparation method is used for flame retardancy of PA, PET, PBT, PP and PE glass fiber reinforced systems.

[0020] Beneficial effects of the present invention:

[0021] The present invention adopts the above-mentioned method for preparing a halogen-free flame retardant with high-temperature thermal stability and no discoloration. The prepared halogen-free flame retardant has good thermal stability at a high temperature of 280-300°C, is not easy to discolor, has good compatibility with resin, conforms to the development direction of halogen-free high-phosphorus environmentally friendly flame retardants, and solves the flame retardant needs of high-temperature processing resins.

[0022] The present invention adopts the above-mentioned method for preparing a halogen-free flame retardant with high temperature thermal stability and no discoloration, and the prepared halogen-free flame retardant can be used for flame retardancy of glass fiber reinforced systems such as PA, PET, PBT, PP, and PE.

[0023] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the infrared spectrum of the hexamethylenediamine polyphosphate prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with the accompanying drawings and embodiments. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs. The above-mentioned features or features mentioned in the specific examples mentioned in the present invention can be combined arbitrarily, and these specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0026] Example 1

[0027] The present invention provides a method for preparing a halogen-free flame retardant having high temperature thermal stability and no discoloration, and the steps are as follows:

[0028] S1, acid-base reaction: 1000g of deionized water and 200g of silicone oil were poured into a 5L stainless steel reactor to mix as a solvent, 606.1g of hexamethylenediamine with a content of 99% was weighed, poured into the reactor, the reactor was sealed, the temperature was raised to 40-45°C, 1143.6g of phosphoric acid with a content of 88.5% was weighed, and slowly added dropwise to the reactor, the temperature was maintained below 95°C, and the reaction was carried out for half an hour to obtain hexamethylenediamine diphosphate;

[0029] The stainless steel reactor was heated to distill out free water. When the temperature inside the stainless steel reactor reached 140°C, about 1136.5 g of water was obtained, and the free water was completely discharged.

[0030] S2, dehydration pyrophosphorylation reaction: after the free water is distilled off, the temperature is continuously raised until the temperature in the stainless steel reactor is constant at 270°C, and the temperature is maintained for 1.5 hours, and hexamethylenediamine diphosphate undergoes a dehydration reaction to obtain hexamethylenediamine pyrophosphate, and obtains water removed by intermolecular pyrophosphorylation, and collects about 94g of water;

[0031] S3, dehydration polycondensation reaction: after the completion of step S2, the temperature is continued to be raised to 320°C in the stainless steel reactor, and the hexamethylenediamine pyrophosphate is subjected to polymerization dehydration reaction for 30 minutes. The heating is stopped and the reaction is terminated to obtain hexamethylenediamine polyphosphate containing phosphorus and nitrogen. About 50 g of water is collected and discharged, and then the product is cooled to room temperature and the solvent is filtered out to obtain a waxy and translucent product, which is crushed to obtain a white powdery material, i.e., a halogen-free flame retardant.

[0032] The weight of the white powdery material was 1462.1 g, and the yield was about 99.5%.

[0033] Example 2

[0034] The present invention provides a method for preparing a halogen-free flame retardant having high temperature thermal stability and no discoloration, and the steps are as follows:

[0035] S1, acid-base reaction: 1000g of deionized water and 200g of cyclopentane are poured into a 5L stainless steel reactor and mixed as a solvent, 459g of 99% diaminobutane is weighed, poured into the reactor, the reactor is sealed, the temperature is raised to 70-75°C, 1143.6g of 88.5% phosphoric acid is weighed, slowly added dropwise to the reactor, the temperature is maintained below 95°C, and the reaction is carried out for half an hour to obtain diaminobutane diphosphate;

[0036] The stainless steel reactor was heated to distill out free water. When the temperature inside the stainless steel reactor reached 140°C, about 1134.5 g of water was obtained, and the free water was completely discharged.

[0037] S2, dehydration pyrophosphorylation reaction: after the free water is distilled off, the temperature is continuously raised until the temperature in the stainless steel reactor is constant at 270°C, and the temperature is maintained for 3 hours, and hexamethylenediamine diphosphate is dehydrated to obtain diamethylenediamine pyrophosphate, and the water removed by intermolecular pyrophosphorylation is obtained, and about 92.5g of water is collected;

[0038] S3, dehydration polycondensation reaction: after the completion of step S2, the temperature is continued to be raised to 290°C in the stainless steel reactor, and the pyrophosphate dibutylene diamine salt is subjected to polymerization dehydration reaction for 30 minutes, and the heating is stopped to terminate the reaction to obtain polyphosphate dibutylene diamine salt containing phosphorus and nitrogen. About 49.4 g of water is collected and discharged, and then the material is cooled to room temperature and the solvent is filtered out to obtain a waxy and translucent product, which is crushed to obtain a white powdery material, i.e., a halogen-free flame retardant.

[0039] The weight of the white powdery material was 1321.1 g, and the yield was about 99.5%.

[0040] Figure 1 The infrared spectrum of the polyphosphoric acid hexamethylenediamine salt prepared in Example 1 of the present invention is shown in FIG. Figure 1 It can be seen that the infrared spectrum is at 1257.97cm -1 The characteristic absorption peak of -P=O- appeared at 2930.25cm -1 -CH appears 2 -The characteristic absorption peak is at 3647.82cm -1 -NH appears 2 -characteristic absorption peak, it can be known that the product obtained in Example 1 is determined to be polyphosphohexamethylenediamine salt.

[0041] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a halogen-free flame retardant having high temperature thermal stability and no discoloration, characterized in that: The polyphosphoric acid organic amine salt containing phosphorus and nitrogen is prepared as a halogen-free flame retardant by acid-base reaction, dehydration pyrophosphorylation reaction, and dehydration polycondensation reaction of orthophosphoric acid and hexamethylenediamine. The structural formula of the polyphosphoric acid organic amine salt is as follows: In the formula, n is an integer greater than 2.

2. The method for preparing a halogen-free flame retardant having high temperature thermal stability and no discoloration according to claim 1, characterized in that: The molar ratio of orthophosphoric acid to hexamethylenediamine in the acid-base reaction is 2 to 1:

1.

3. The method for preparing a halogen-free flame retardant having high temperature thermal stability and no discoloration according to claim 1, characterized in that: The solvent used in the acid-base reaction is a mixture of water and sulfolane or silicone oil, and the weight ratio of water to sulfolane or silicone oil is 5:

1.

4. The method for preparing a halogen-free flame retardant having high temperature thermal stability and no discoloration according to claim 1, characterized in that: The acid-base reaction is carried out at a temperature of 40 to 100°C and normal pressure for 0.5 to 3 hours.

5. The method for preparing a halogen-free flame retardant having high temperature thermal stability and no discoloration according to claim 1, characterized in that: The temperature of the dehydration pyrophosphorylation reaction is 220-270° C., and the reaction time is 1-5 hours.

6. The method for preparing a halogen-free flame retardant having high temperature thermal stability and no discoloration according to claim 1, characterized in that: The temperature of the dehydration polycondensation reaction is 260-320°C, and the reaction time is 0.5-2h.

7. The method for preparing a halogen-free flame retardant having high temperature thermal stability and no discoloration according to claim 1, characterized in that: The dehydration pyrophosphorylation reaction and the dehydration polycondensation reaction are both carried out under vacuum conditions, with the vacuum degree being -0.06 to -0.099 MPa.

8. An application of a halogen-free flame retardant with high temperature thermal stability and no discoloration, characterized in that: The halogen-free flame retardant with high temperature thermal stability and no discoloration obtained by the preparation method described in any one of claims 1 to 7 is used for flame retardancy of PA, PET, PBT, PP, and PE glass fiber reinforced systems.