Multi-core metal organic cage material as well as preparation method and application thereof
By introducing multinuclear metal-organic cage materials into the nanozyme system, the synergistic effect of metal clusters is used to enhance enzyme activity, solving the problems of unclear nanozyme structure and single activity, and achieving the improvement of multiple enzyme activities and biocompatibility. , promoting the application of nanozymes in inflammation treatment.
Patent Information
- Application Number
- CN202410761101.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-13
AI Technical Summary
Existing nanozyme systems face problems such as unclear structure, single catalytic activity, and unclear biological safety, which limits their application in inflammation treatment.
Multi-core metal-organic cage materials are used to form multi-core nanozymes by introducing multiple metals. The synergistic effect of different metals in metal clusters is used to enhance enzyme activity. The catalytic activity is adjusted by metal type and feed amount to construct MOC with multiple enzyme activities. Nanozymes.
It has realized a nanozyme system with clear structure, multiple enzyme activities and good biocompatibility, which can reduce ROS levels in inflammatory sites, promote the research on the structure-activity relationship of nanozymes, and promote the clinical transformation of nanozymes.
Smart Images

Figure CN118772425A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of anti-inflammation, and specifically relates to a multi-core metal organic cage material and a preparation method and application thereof. Background Art
[0002] Inflammation is the body's defense mechanism that can detect and remove harmful exogenous substances. Inflammation is associated with many diseases, including autoimmune diseases, infectious diseases, chronic degenerative diseases, etc., which are one of the main causes of human death. Reactive oxygen species (ROS) are weapons used by immune cells to remove exogenous substances during inflammation. They are also upstream signal molecules of inflammation and are closely related to the occurrence, development and regression of inflammation. However, while removing exogenous substances, excessive ROS can also damage their own cells and tissues and cause excessive inflammation. Therefore, removing excessive ROS is crucial to human health and is also the main way to relieve inflammation. The body mainly uses antioxidant enzymes to remove ROS, including superoxide dismutase (SOD) and catalase (CAT). These natural enzymes have the characteristics of high activity, good specificity, and clear structure. However, the unstable structure of natural enzymes makes them difficult to prepare, easy to inactivate, high cost, difficult to mass produce and store for a long time, and clinical promotion is relatively difficult. Therefore, the medical field urgently needs to develop an antioxidant system that has both natural enzyme activity and structural stability.
[0003] Nanozymes came into being, combining the physical, chemical and biological properties of nanomaterials with the catalytic activity of natural enzymes, and have the advantages of stable structure, multifunctionality, low cost, recyclability, easy large-scale production and storage, etc. After nearly a decade of development, various nanozymes with different structures have been developed and used in the research of various disease treatments, and have also shown excellent therapeutic potential.
[0004] However, existing nanozyme systems face many development bottlenecks:
[0005] 1) The structure of nanozymes is unclear and quality control is difficult, making it difficult to elucidate the structure-activity relationship, which also poses challenges to mass production and clinical transformation;
[0006] 2) There is a lack of standardized procedures for evaluating the catalytic activity of nanozymes, making it difficult to compare the catalytic activities of different nanozymes;
[0007] 3) The activity of nanozymes is often relatively single, and the therapeutic effect is limited;
[0008] 4) The biosafety of nanozymes is still unclear, which brings uncertainty and danger to clinical use. Therefore, the development of nanozymes with clear structures, multiple enzyme activities, and good biocompatibility is an inevitable development goal in this field. Summary of the invention
[0009] In view of the unclear structure and single enzyme activity of nanozymes, the present invention provides a multi-core metal organic cage material and a preparation method and application thereof, providing an optional material for the treatment of inflammation.
[0010] The present invention selects a nanosystem with a clear structure and introduces multiple metals to form a multi-core nanozyme to achieve multiple enzyme activities; and enhances the corresponding enzyme activity through the synergistic effect between different metals in the same metal cluster to achieve multiple antioxidant activities; and adjusts the metal type and content in the multi-core nanozyme by the metal type and feed amount, thereby optimizing the catalytic activity. Through research and evaluation, metal organic cages are an ideal system that meets the above requirements.
[0011] In order to further realize the synergistic effect of different metals in metal clusters, we selected metal organic cages with M4O cluster structure. Metal organic cages (MOC) have atomically precise structures and are uniform, discrete, ultra-small nano-polyhedrons constructed by coordination bonds between metal ions or clusters and organic ligands. MOC combines the advantages of organic and inorganic, with precise and stable structures, adjustable components and sizes, nano-scale cavities and sizes, easy synthesis and modification, excellent biocompatibility, etc., and are widely used in biomedicine fields, such as imaging, sensing, tumor treatment, etc. For example, palladium-pyridine-based MOC has photooxidase activity and produces ROS to exert antibacterial properties.
[0012] This type of MOC has an octahedral structure, with six vertices occupied by calix[4]arene, eight faces or 12 edges composed of tricarboxylic acid ligands or dicarboxylic acid ligands, and the carboxylic acid site and the phenolic oxygen of calix[4]arene are respectively bound to the cluster M4O. This type of MOC has 24 metal sites, which can be isomorphically replaced to enrich metal types and thus achieve the diversity of enzyme activity. The interaction between different metals in the four-metal cluster will further enhance the enzyme activity.
[0013] Thanks to the structural characteristics of MOC and the catalytic activity of metal sites, we plan to develop MOC nanozymes with multiple enzyme activities and develop nanozyme systems with clear structures and diverse activities. In order to achieve multiple enzyme activities and optimize components and performance, we plan to introduce multiple metals into MOC and construct MOC nanozymes containing multiple metals.
[0014] There are three main strategies for introducing multiple metals into MOC: metallized ligand strategy, heteronuclear cluster strategy, and isomorphic replacement strategy. The multi-metal MOC obtained by re-coordinating the metallized ligand with other metals has a clear structure, but the components and properties are difficult to control, and there is basically no interaction between different metals. The heteronuclear cluster strategy is to use multi-metal clusters and ligands to coordinate to obtain heteronuclear MOC, which has a clear structure and there are interactions between different metals, but the components and properties are difficult to control. Isomorphic replacement means that different metals can occupy the metal position in MOC equivalently, and the clarity of the resulting MOC structure is reduced. Therefore, the present invention introduces a variety of metals with adjustable types and contents into a metal-organic cage with a clear structure, which can not only combine the required enzyme activity as needed, but also synergistically enhance the corresponding enzyme activity.
[0015] The technical solution provided by the present invention is as follows:
[0016] <First aspect>
[0017] A multi-nuclear metal organic cage material, the components of which include metal clusters, calix[4]arene ligands, and carboxylic acid ligands; the metal ions in the metal clusters include two or more types.
[0018] The metal cluster is a M4O metal cluster;
[0019] The carboxylic acid ligand includes a dicarboxylic acid ligand or a tricarboxylic acid ligand.
[0020] The dicarboxylic acid ligand is selected from 1,4-terephthalic acid, 4,4'-biphenyldicarboxylic acid, and 2,2'-bipyridine-5,5'-dicarboxylic acid;
[0021] The tricarboxylic acid ligand is selected from 1,3,5-benzenetricarboxylic acid, 1,3,5-tris(4-carboxyphenyl)benzene, 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, and 4,4'4"-tricarboxylic acid triphenylamine.
[0022] The polynuclear metal organic cage material includes (M4O)6(calix[4]arene)6(dicarboxylic acid ligand) 12 Or (M4O)6(calix[4]arene)6(tricarboxylic acid ligand)8; wherein the 24 metal ions include two or more types.
[0023] The (M4O)6(calix[4]arene)6(dicarboxylic acid ligand) 12 It includes 6 M4O metal clusters, 6 calix[4]arene ligands, and 12 dicarboxylic acid ligands;
[0024] The (M4O)6(calix[4]arene)6(tricarboxylic acid ligand)8 comprises 6 M4O metal clusters, 6 calix[4]arene ligands, and 8 tricarboxylic acid ligands.
[0025] The metal ion is selected from alkaline earth metals or transition metals;
[0026] The alkaline earth metal includes one or more of magnesium, calcium, strontium and barium;
[0027] The transition metal includes one or more of scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper and zinc.
[0028] The calix[4]arene ligand includes 4-tert-butylsulfonylcalix[4]arene and / or 4-sulfonylsulfonylcalix[4]arene.
[0029] As an embodiment of the present invention, the polynuclear metal organic cage material comprises (M4O)6(calix[4]arene)6(dicarboxylic acid ligand) 12 Or (M4O)6(calix[4]arene)6(tricarboxylic acid ligand)8; wherein the 24 metal ions M include two or more types.
[0030] The (M4O)6(calix[4]arene)6(dicarboxylic acid ligand) 12 It includes 6 M4O metal clusters, 6 calix[4]arene ligands, and 12 dicarboxylic acid ligands;
[0031] The (M4O)6(calix[4]arene)6(tricarboxylic acid ligand)8 comprises 6 M4O metal clusters, 6 calix[4]arene ligands, and 8 tricarboxylic acid ligands.
[0032] The dicarboxylic acid ligand is selected from 1,4-terephthalic acid, 4,4'-biphenyldicarboxylic acid, and 2,2'-bipyridine-5,5'-dicarboxylic acid;
[0033] The tricarboxylic acid ligand is selected from 1,3,5-benzenetricarboxylic acid, 1,3,5-tris(4-carboxyphenyl)benzene, 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, and 4,4'4"-tricarboxylic acid triphenylamine.
[0034] The calix[4]arene ligand includes 4-tert-butylsulfonylcalix[4]arene and / or 4-sulfonylsulfonylcalix[4]arene.
[0035] The metal ion is selected from alkaline earth metals or transition metals;
[0036] The alkaline earth metal includes one or more of magnesium, calcium, strontium and barium;
[0037] The transition metal includes one or more of scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper and zinc.
[0038] <Second Aspect>
[0039] The present invention also provides a method for preparing a multi-core metal organic cage material, comprising the following steps:
[0040] Step 1: Mix a metal salt, a carboxylic acid ligand, and a calix[4]arene ligand, and dissolve them in an organic solvent to form a solution A; the metal salt contains two or more metal ions;
[0041] Step 2, subjecting solution A to thermal reaction and cooling;
[0042] Step three: separating and drying the crystals in the product of step two to obtain a multi-core metal organic cage material.
[0043] In step 1, the metal salt includes a II-valent metal salt or a III-valent metal salt.
[0044] In step 1, the calix[4]arene ligand comprises sulfonylcalix[4]arene.
[0045] The sulfonylcalix[4]arene includes 4-tert-butylsulfonylcalix[4]arene or 4-sulfonic acidsulfonylcalix[4]arene.
[0046] In step 1, the carboxylic acid ligand includes a dicarboxylic acid ligand or a tricarboxylic acid ligand.
[0047] The dicarboxylic acid ligand is selected from 1,4-terephthalic acid, 4,4'-biphenyldicarboxylic acid, and 2,2'-bipyridine-5,5'-dicarboxylic acid;
[0048] The tricarboxylic acid ligand is selected from 1,3,5-benzenetricarboxylic acid, 1,3,5-tris(4-carboxyphenyl)benzene, 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, and 4,4'4"-tricarboxylic acid triphenylamine.
[0049] In step 1, the organic solvent includes one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, tetrahydrofuran, acetonitrile, methanol, ethanol, isopropanol, and n-butanol.
[0050] As an embodiment of the present invention, in step 1, the organic solvent includes N,N-dimethylformamide and methanol; the volume ratio of N,N-dimethylformamide to methanol is 5-30:1.
[0051] In step 1, the metal salt is one of nitrates, chlorides or acetates of alkaline earth metals or transition metals, including hydrates thereof.
[0052] The alkaline earth metal includes one or more of magnesium, calcium, strontium and barium;
[0053] The transition metal includes one or more of scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper and zinc.
[0054] In solution A, the molar ratio of the total amount of metal salt to the calix[4]arene ligand is 2-10:1.
[0055] In solution A, the molar ratio of the total amount of metal salt to the carboxylic acid contained in the polyacid ligand is 0.2-10:1.
[0056] In step 2, solution A is placed in a metal bath for heating reaction at a temperature of 90-140° C. and a reaction time of 2-36 hours.
[0057] In step 3, separation and drying can be performed by directly removing the solvent and naturally air-drying, or by centrifugal washing and vacuum drying.
[0058] <Third Aspect>
[0059] The application of the multi-core metal organic cage material in anti-inflammatory also falls within the protection scope of the present invention.
[0060] The present invention has the following beneficial effects:
[0061] 1. The multi-core metal organic cage provided by the present invention has a clear structure, strong adjustability, good stability, strong antioxidant ability, low cytotoxicity, and good biocompatibility. It can reduce the level of ROS in inflammatory sites and promote the structure-activity relationship research of nanozymes.
[0062] 2. The present invention can obtain multi-core metal organic cages through a simple solvothermal method, which can be prepared in large quantities in a controllable manner and can greatly promote the clinical transformation of nanozymes.
[0063] 3. Due to the different coordination conditions and activities of different metals, not all the elements introduced arbitrarily can satisfy the construction of multi-core metal-organic cages, nor can they necessarily achieve the function of eliminating active oxygen. The present invention has successfully introduced a variety of metal elements, such as magnesium, manganese, iron, cobalt, nickel, zinc, etc., into metal-organic cages with clear structures through a large number of experiments; it has high structural stability and component adjustability; especially the cobalt-nickel system has good active oxygen scavenging ability. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0065] Figure 1 Schematic diagram of constructing multi-core MOC using 4-tert-butylsulfonylcalix[4]arene and trimesic acid as examples;
[0066] Figure 2 Optical photos of multi-core metal-organic cage crystals prepared from different metal combinations;
[0067] Figure 3 is the XRD pattern of a representative multi-core metal organic cage crystal;
[0068] Figure 4The mass spectrum of a representative polynuclear metal-organic cage;
[0069] Figure 5 To evaluate the superoxide dismutase-like activity of polynuclear metal-organic cages using the NBT method;
[0070] Figure 6 To evaluate the catalase-like activity of polycore metal-organic cages using the oxygen evolution method. DETAILED DESCRIPTION
[0071] The present invention is described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0072] Figure 1 Schematic diagram of the construction of multinuclear MOC using 4-tert-butylsulfonylcalix[4]arene and trimesic acid as examples.
[0073] Example 1
[0074] A method for preparing a binuclear metal organic cage MOC-BTC-CoNi comprises the following steps:
[0075] Step 1: Weigh cobalt chloride, nickel chloride, 1,3,5-benzenetricarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, cobalt chloride 0.025 mmol, nickel chloride 0.025 mmol, 1,3,5-benzenetricarboxylic acid 0.03 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol.
[0076] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0077] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0078] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain a binuclear metal organic cage MOC-BTC-CoNi. Figure 2 Crystalline optical photographs, Figure 3 XRD in Figure 4 The mass spectrometry results in the table all showed that it was successfully prepared.
[0079] Example 2
[0080] A method for preparing a tri-nuclear metal organic cage MOC-BTC-MgMnZn comprises the following steps:
[0081] Step 1. Weigh magnesium chloride, manganese chloride, zinc chloride, 1,3,5-benzenetricarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, magnesium chloride 0.017 mmol, zinc chloride 0.017 mmol, manganese chloride 0.017 mmol, 1,3,5-benzenetricarboxylic acid 0.03 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol.
[0082] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0083] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0084] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain the tri-nuclear metal organic cage MOC-BTC-MgMnZn. Figure 2 The optical photograph of the crystal shows that it was successfully prepared.
[0085] Example 3
[0086] A method for preparing a tri-nuclear metal organic cage MOC-BTC-MgCoZn comprises the following steps:
[0087] Step 1. Weigh a certain amount of magnesium chloride, cobalt chloride, zinc chloride, 1,3,5-benzenetricarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, magnesium chloride 0.017 mmol, zinc chloride 0.017 mmol, cobalt chloride 0.017 mmol, 1,3,5-benzenetricarboxylic acid 0.03 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol.
[0088] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0089] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0090] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain the trinuclear metal organic cage MOC-BTC-MgCoZn. Figure 2 The optical photograph of the crystal shows that it was successfully prepared.
[0091] Example 4
[0092] A method for preparing a tetranuclear metal organic cage MOC-BTC-MgMnCoZn comprises the following steps:
[0093] Step 1. Weigh a certain amount of magnesium chloride, manganese chloride, zinc chloride, 1,3,5-benzenetricarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, magnesium chloride 0.0125 mmol, zinc chloride 0.0125 mmol, manganese chloride 0.0125 mmol, cobalt chloride 0.0125 mmol, 1,3,5-benzenetricarboxylic acid 0.03 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol.
[0094] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0095] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0096] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain the tetranuclear metal organic cage MOC-BTC-MgMnCoZn. Figure 2 The optical photograph of the crystal shows that it was successfully prepared.
[0097] Example 5
[0098] A method for preparing a pentanuclear metal organic cage MOC-BTC-MgMnCoNiZn-1 comprises the following steps:
[0099] Step 1. Weigh a certain amount of magnesium chloride, zinc chloride, manganese chloride, cobalt chloride, nickel chloride, 1,3,5-benzenetricarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, magnesium chloride 0.01 mmol, zinc chloride 0.01 mmol, manganese chloride 0.01 mmol, cobalt chloride 0.01 mmol, nickel chloride 0.01 mmol, 1,3,5-benzenetricarboxylic acid 0.03 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol.
[0100] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0101] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0102] Step 4: remove the supernatant in the sample bottle, and leave the obtained crystals open in a ventilated place to air dry naturally to obtain the pentanuclear metal organic cage MOC-BTC-MgMnCoNiZn-1. Figure 2 Crystalline optical photographs, Figure 3 Powder X-ray diffraction pattern, Figure 4 The mass spectrometry data in show that it was successfully prepared.
[0103] Example 6
[0104] A method for preparing a pentanuclear metal organic cage MOC-BTC-MgMnCoNiZn-2 comprises the following steps:
[0105] Step 1. Weigh a certain amount of magnesium chloride, zinc chloride, manganese chloride, cobalt chloride, nickel chloride, 1,3,5-benzenetricarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, magnesium chloride 0.003 mmol, manganese chloride 0.006 mmol, cobalt chloride 0.01 mmol, nickel chloride 0.013 mmol, zinc chloride 0.017 mmol, 1,3,5-benzenetricarboxylic acid 0.03 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol.
[0106] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0107] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0108] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain the pentanuclear metal organic cage MOC-BTC-MgMnCoNiZn-2. Figure 2 The optical photograph of the crystal shows that it was successfully prepared.
[0109] Example 7
[0110] A method for preparing a binuclear metal organic cage MOC-PTA-MgZn comprises the following steps:
[0111] Step 1: Weigh a certain amount of magnesium chloride, zinc chloride, 1,4-terephthalic acid and 4-tert-butylsulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, magnesium chloride 0.02 mmol, zinc chloride 0.02 mmol, 1,4-terephthalic acid 0.02 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol.
[0112] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0113] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0114] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain the binuclear metal organic cage MOC-PTA-MgZn.
[0115] Example 8
[0116] A method for preparing a tri-nuclear metal organic cage MOC-BDC-MgMnZn comprises the following steps:
[0117] Step 1. Weigh a certain amount of magnesium chloride, manganese chloride, zinc chloride, 4,4'-biphenyldicarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, magnesium chloride 0.013 mmol, manganese chloride 0.013 mmol, zinc chloride 0.013 mmol, 4,4'-biphenyldicarboxylic acid 0.02 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol.
[0118] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0119] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0120] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain the tri-nuclear metal organic cage MOC-BDC-MgMnZn.
[0121] Example 9
[0122] A method for preparing a tetranuclear metal organic cage MOC-BPDC-MgMnCoZn comprises the following steps:
[0123] Step 1, weigh a certain amount of magnesium chloride, manganese chloride, cobalt chloride, zinc chloride, 2,2'-bipyridine-5,5'-dicarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively, and place them in a 2 ml sample bottle; wherein, magnesium chloride 0.01 mmol, manganese chloride 0.01 mmol, cobalt chloride 0.01 mmol, zinc chloride 0.01 mmol, 2,2'-bipyridine-5,5'-dicarboxylic acid 0.02 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol;
[0124] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0125] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0126] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain the tetranuclear metal organic cage MOC-BPDC-MgMnCoZn.
[0127] Example 10
[0128] A method for preparing a pentanuclear metal organic cage MOC-BTB-MgMnCoNiZn comprises the following steps:
[0129] Step 1, weigh a certain amount of magnesium chloride, manganese chloride, cobalt chloride, nickel chloride, zinc chloride, 1,3,5-tris(4-carboxyphenyl)benzene and 4-tert-butylsulfonylcalix[4]arene respectively, and place them in a 2 ml sample bottle; wherein, magnesium chloride 0.01 mmol, manganese chloride 0.01 mmol, cobalt chloride 0.01 mmol, nickel chloride 0.01 mmol, zinc chloride 0.01 mmol, 1,3,5-tris(4-carboxyphenyl)benzene 0.03 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol;
[0130] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0131] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0132] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain the pentanuclear metal organic cage MOC-BTB-MgMnCoNiZn.
[0133] Embodiment 11
[0134] A method for preparing a binuclear metal organic cage MOC-BTC-FeZn comprises the following steps:
[0135] Step 1: Weigh a certain amount of ferric chloride, zinc chloride, 1,3,5-benzenetricarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, ferric chloride 0.025 mmol, zinc chloride 0.025 mmol, 1,3,5-benzenetricarboxylic acid 0.03 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol.
[0136] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0137] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0138] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain a binuclear metal organic cage MOC-BTC-FeZn.
[0139] Example 12
[0140] A method for preparing a binuclear metal organic cage MOC-BTC-MgZn-SO3 comprises the following steps:
[0141] Step 1: Weigh a certain amount of magnesium chloride, zinc chloride, 1,3,5-benzenetricarboxylic acid and 4-sulfonatesulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, magnesium chloride 0.025 mmol, zinc chloride 0.025 mmol, 1,3,5-benzenetricarboxylic acid 0.03 mmol and 4-sulfonatesulfonylcalix[4]arene 0.01 mmol.
[0142] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0143] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0144] Step 4: remove the supernatant in the sample bottle, and leave the obtained crystals open in a ventilated place to dry naturally, thereby obtaining a binuclear metal organic cage MOC-BTC-MgZn-SO3.
[0145] Example 13
[0146] A method for preparing a hexanuclear metal organic cage MOC-BTC-MgMnFeCoNiZn comprises the following steps:
[0147] Step 1, weigh a certain amount of magnesium chloride, manganese chloride, cobalt chloride, nickel chloride, zinc chloride, 1,3,5-benzenetricarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively, and place them in a 2 ml sample bottle; wherein, magnesium chloride 0.01 mmol, manganese chloride 0.01 mmol, iron chloride 0.01 mmol, cobalt chloride 0.01 mmol, nickel chloride 0.01 mmol, zinc chloride 0.01 mmol, 1,3,5-benzenetricarboxylic acid 0.03 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol;
[0148] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0149] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0150] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain the hexanuclear metal organic cage MOC-BTC-MgMnFeCoNiZn.
[0151] Embodiment 14
[0152] The difference between this embodiment and embodiment 1 is that in step 1, the dosage is as follows:
[0153] 0.04mmol of cobalt chloride, 0.01mmol of nickel chloride, 0.03mmol of 1,3,5-benzenetricarboxylic acid and 0.01mmol of 4-tert-butylsulfonylcalix[4]arene were used to obtain the binuclear metal organic cage MOC-BTC-CoNi-2. Figure 4 The mass spectrometry data in show that it was successfully prepared.
[0154] Comparative Example 1
[0155] A method for preparing a mononuclear metal organic cage MOC-BTC-Co comprises the following steps:
[0156] Step 1: Weigh cobalt chloride, 1,3,5-benzenetricarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, cobalt chloride 0.05 mmol, 1,3,5-benzenetricarboxylic acid 0.03 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol.
[0157] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0158] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0159] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain the mononuclear metal organic cage MOC-BTC-Co. Figure 2 Crystalline optical photographs, Figure 3 Powder X-ray diffraction pattern, Figure 4 The mass spectrometry data in show that it was successfully prepared.
[0160] Comparative Example 2
[0161] A method for preparing a mononuclear metal organic cage MOC-BTC-Ni comprises the following steps:
[0162] Step 1: Weigh nickel chloride, 1,3,5-benzenetricarboxylic acid and 4-tert-butylsulfonylcalix[4]arene respectively and place them in a 2 ml sample bottle; wherein, nickel chloride 0.05 mmol, 1,3,5-benzenetricarboxylic acid 0.03 mmol and 4-tert-butylsulfonylcalix[4]arene 0.01 mmol.
[0163] Step 2: Add DMF and methanol in a volume ratio of V:V=20:1 to the sample bottle containing the mixed drug in step 1, and dissolve by ultrasonic to obtain a mixed solution; wherein the added DMF and methanol are 1 ml and 50 μL respectively;
[0164] Step 3: Place the sample bottle containing the mixed solution in step 2 in a constant temperature metal bath with a heating module, react at 100° C. for 24 hours, and take out the sample bottle after the system cools to room temperature;
[0165] Step 4: remove the supernatant in the sample bottle, and expose the obtained crystals to air dry naturally in a ventilated place to obtain the mononuclear metal organic cage MOC-BTC-Ni. Figure 2 Crystalline optical photographs, Figure 4 The mass spectrometry data in show that it was successfully prepared.
[0166] Performance test case
[0167] The performance of the multi-core metal organic cages prepared in Example 1 and Comparative Examples 1-2 was tested.
[0168] 1. Superoxide dismutase (SOD)-like activity.
[0169] The superoxide dismutase (SOD)-like activity of polynuclear metal organic cages was determined by nitroblue tetrazolium (NBT) method. The polynuclear metal organic cages (2 mg / mL, 90 μL) were incubated with NBT (750 μmol / L, 0.5 mL), Met (130 mmol / L, 0.5 mL), EDTA-Na2 (100 μmol / L, 0.3 mL), riboflavin (20 μmol / L, 0.5 mL) and phosphate buffer solution (pH = 7.4) under constant intensity ultraviolet irradiation for 60 s, and the SOD-like activity was tested by UV-visible spectrophotometer. The lower the absorbance, the stronger the SOD-like enzyme activity of the corresponding material. The results are shown in Figure 5 And Table 1:
[0170] Table 1 Evaluation of SOD-like enzyme activity of polynuclear metal organic cages by NBT method (absorbance at 120 seconds)
[0171] Metal-organic cage materials Absorbance Example 1 MOC-BTC-CoNi 0.32 Example 2 MOC-BTC-MgMnZn 0.40 Example 3 MOC-BTC-MgCoZn 0.36 Example 4 MOC-BTC-MgMnCoZn 0.37 Example 5 MOC-BTC-MgMnCoNiZn-1 0.35 Example 6 MOC-BTC-MgMnCoNiZn-2 0.36 Example 7 MOC-PTA-MgZn 0.38 Example 8 MOC-BDC-MgMnZn 0.40 Example 9 MOC-BPDC-MgMnCoZn 0.35 Example 10 MOC-BTB-MgMnCoNiZn 0.38 Embodiment 11 MOC-BTC-FeZn 0.40 Example 12 MOC-BTC-MgZn-SO3 0.40 Example 13 MOC-BTC-MgMnFeCoNiZn 0.39 Embodiment 14 MOC-BTC-CoNi-2 0.39 Comparative Example 1 MOC-BTC-Co 0.42 Comparative Example 2 MOC-BTC-Ni 0.45 Comparison No metal organic cage materials added 0.58
[0172] 2. Determination of catalase-like (CAT) activity:
[0173] The catalase (CAT) activity of the polynuclear metal organic cage was measured by a dissolved oxygen meter; specifically, 200 μL of 30% H2O2 solution was added to 14.94 mL of water, and then 100 μL of polynuclear metal molecular cage sample (2 mg / mL) was added, and the increased oxygen release in the solution from 0 to 5 minutes was recorded. The larger the value, the higher the CAT enzyme activity of the corresponding material. The results are shown in Figure 6 and Table 2:
[0174] Table 2 Evaluation of CAT-like enzyme activity of polynuclear metal organic cages by oxygen release method (release amount at 240 seconds)
[0175] Metal-organic cage materials Oxygen release (unit: mg / L) Example 1 MOC-BTC-CoNi 8.5 Example 2 MOC-BTC-MgMnZn 4.5 Example 3 MOC-BTC-MgCoZn 5.6 Example 4 MOC-BTC-MgMnCoZn 4.8 Example 5 MOC-BTC-MgMnCoNiZn-1 4.6 Example 6 MOC-BTC-MgMnCoNiZn-2 4.7 Example 7 MOC-PTA-MgZn 4.2 Example 8 MOC-BDC-MgMnZn 4.5 Example 9 MOC-BPDC-MgMnCoZn 5.0 Example 10 MOC-BTB-MgMnCoNiZn 5.2 Embodiment 11 MOC-BTC-FeZn 4.0 Example 12 MOC-BTC-MgZn-SO3 4.7 Example 13 MOC-BTC-MgMnFeCoNiZn 5.5 Embodiment 14 MOC-BTC-CoNi-2 5.8 Comparative Example 1 MOC-BTC-Co 3.8 Comparative Example 2 MOC-BTC-Ni 4.3 Comparison No metal organic cage materials added 2.5
[0176] The results show that:
[0177] The MOC-BTC-CoNi prepared in Example 1 has advantages over the MOC-BTC-Co of Comparative Example 1 and the MOC-BTC-Ni of Comparative Example 2 in terms of both SOD-like enzyme and CAT-like enzyme activities.
[0178] Compared with Example 14, when the amount of cobalt chloride increased and the amount of nickel chloride decreased, the activities of the SOD-like enzyme and CAT-like enzyme of the prepared multi-core metal organic cage decreased, indicating that the metal content in the multi-core MOC has a certain influence on its activity, and its enzyme activity can be regulated according to different needs.
[0179] Compared with Example 3 (MOC-BTC-MgCoZn) and Example 4 (MOC-BTC-MgMnCoZn), the addition of the metal element Mn has almost no effect on the SOD-like enzyme activity, while the CAT-like enzyme activity is reduced. This is because different metals have different catalytic activities, and the addition of metals will affect the content of other metals and thus their activity.
[0180] Comparison between the two penta-nuclear MOCs with different metal contents in Example 5 and Example 6 further demonstrates that the metal content also has an effect on its activity.
[0181] Compared with the two quadruple-core MOCs of Example 4 and Example 9, their activities are very similar, indicating that the type and content of metal have a greater impact on their activity, while the carboxylic acid ligand has a smaller impact.
[0182] Although the technical solutions of the present invention have been described and listed in detail, it should be understood that it is obvious to those skilled in the art to make modifications to the above embodiments or adopt equivalent alternatives. These modifications or improvements made without departing from the spirit of the present invention are within the scope of protection required by the present invention.
Claims
1. A multi-core metal organic cage material, characterized in that: Its components include metal clusters, calix[4]arene ligands, and carboxylic acid ligands; the metal ions in the metal clusters include two or more types.
2. The multi-core metal organic cage material according to claim 1, characterized in that: The metal cluster includes an M4O metal cluster; and the carboxylic acid ligand includes a dicarboxylic acid ligand or a tricarboxylic acid ligand.
3. The multi-core metal organic cage material according to claim 2, characterized in that: The dicarboxylic acid ligand is selected from 1,4-terephthalic acid, 4,4'-biphenyldicarboxylic acid, and 2,2'-bipyridine-5,5'-dicarboxylic acid; The tricarboxylic acid ligand is selected from 1,3,5-benzenetricarboxylic acid, 1,3,5-tris(4-carboxyphenyl)benzene, 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, and 4,4'4"-tricarboxylic acid triphenylamine.
4. The multi-core metal organic cage material according to claim 1, characterized in that: The metal ions are selected from alkaline earth metals or transition metals.
5. The multi-core metal organic cage material according to claim 4, characterized in that: The alkaline earth metal includes one or more of magnesium, calcium, strontium, and barium; the transition metal includes one or more of scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, and zinc.
6. The multi-core metal organic cage material according to claim 1, characterized in that: The calix[4]arene ligand includes 4-tert-butylsulfonylcalix[4]arene and / or 4-sulfonylsulfonylcalix[4]arene.
7. The multi-core metal organic cage material according to claim 1, characterized in that: The polynuclear metal organic cage material includes (M4O)6(calix[4]arene)6(dicarboxylic acid ligand) 12 , or (M4O)6(calix[4]arene)6(tricarboxylic acid ligand)8; wherein the 24 metal ions M include two or more types.
8. A method for preparing a multi-core metal organic cage material, characterized in that: The following steps are involved: Step 1: Mix a metal salt, a carboxylic acid ligand, and a calix[4]arene ligand, and dissolve them in an organic solvent to form a solution A; the metal salt contains two or more metal ions; Step 2, subjecting solution A to thermal reaction and cooling; Step three: separating and drying the crystals in the product of step two to obtain a multi-core metal organic cage material.
9. The preparation method according to claim 8, in step 1, the metal salt is one or more of nitrates, chlorides or acetates of alkaline earth metals or transition metals, including hydrates thereof; In solution A, the molar ratio of the total amount of metal salt to the calix[4]arene ligand is 2-10:1; In solution A, the molar ratio of the total amount of metal salt to the carboxylic acid contained in the polyacid ligand is 0.2-10:1; In step 2, the thermal reaction temperature of solution A is 90-140° C. and the reaction time is 2-36 hours.
10. Use of the multi-core metal organic cage material according to any one of claims 1 to 7, or the multi-core metal organic cage material prepared by the preparation method according to claim 8 or 9 in anti-inflammatory treatment.
Citation Information
Patent Citations
Supramolecular cage complex and preparation method and application thereof
CN106831830A
Supermolecule cage complex as well as preparation method and application thereof
CN107400149A
Discrete coordination molecule container and preparation method and small molecule catalysis application thereof
CN110903326A
Coordination compound as well as preparation method and application thereof
CN112250717A
Modular Assembly of Metal-Organic Super-Containers Incorporating Calixarenes
US20130299423A1