Chitosan / sodium hyaluronate hydrogel based on amino acid / chitosan composite regulation and preparation method thereof
Through the method of complex regulation of amino acids/chitosan, the mechanical properties of chitosan/sodium hyaluronate hydrogel are improved, which solves the problem of insufficient strength of existing hydrogels. It is suitable for a variety of medical applications and has low Cost and environmentally friendly preparation features.
Patent Information
- Application Number
- CN202410951305.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-15
AI Technical Summary
The existing chitosan/sodium hyaluronate hydrogel has weak mechanical properties, low toughness and strength, and cannot meet the practical application requirements of withstanding certain mechanical loads.
Using a preparation method based on amino acid/chitosan complex regulation, the precipitate and supernatant are separated by standing to remove excess small molecules to form a regular structure, and the topology of the hydrogel is controlled by dropping a mixed solution containing amino acids and chitosan. structure, combined with the drying process to improve the mechanical properties of the hydrogel.
Significantly improves the tensile properties and strength of chitosan/sodium hyaluronate hydrogel, enhances its practical application potential, is suitable for wound dressings, scar suppression, beauty films and other fields, and has adjustable structural properties and mildness preparation conditions.
Smart Images

Figure CN118772443A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogels, and in particular relates to a chitosan / sodium hyaluronate hydrogel based on amino acid / chitosan composite regulation and a preparation method thereof. Background Art
[0002] Natural biomacromolecule hydrogels have good biocompatibility and degradability and are widely used in biomedicine and drug carriers. Chitosan (CS) is a biodegradable and biocompatible cationic polymer, and sodium hyaluronate (HA) is a non-immunogenic and biodegradable natural anionic polymer. The carboxyl groups in sodium hyaluronate and the protonated amino groups in chitosan easily form a high-density ion cross-linked network under the action of ionic bonds, and the network also contains a large number of hydrogen bonds and chain entanglements. As reactive and functional biopolymers, the chitosan / sodium hyaluronate hydrogel formed has good biocompatibility and medical potential.
[0003] However, the chitosan / sodium hyaluronate hydrogels reported so far have weak mechanical properties, low toughness and strength, and cannot meet the needs of many practical applications that require bearing a certain mechanical load. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a chitosan / sodium hyaluronate hydrogel based on amino acid / chitosan composite regulation and a preparation method thereof. The hydrogel has good mechanical properties, high toughness and strength.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A method for preparing chitosan / sodium hyaluronate hydrogel based on amino acid / chitosan composite regulation, the preparation method comprising the following steps:
[0007] (1) heating and stirring sodium hyaluronate powder in water until completely dissolved, then adding chitosan powder and stirring to make it evenly dispersed;
[0008] (2) adding glacial acetic acid solution to step (1) until the chitosan is completely dissolved, and continuing to stir until the mixture is uniformly mixed;
[0009] (3) allowing the reaction solution obtained in step (2) to stand at room temperature, separating the precipitate and the supernatant, washing the precipitate with deionized water, and then allowing the precipitate to stand again to collect the precipitate;
[0010] (4) adding a mixed solution containing amino acids and chitosan to the precipitate obtained in step (3), stirring and dispersing the mixture evenly, allowing the mixture to stand, and removing the supernatant to obtain a hydrogel precursor solution;
[0011] (5) spreading the hydrogel precursor liquid evenly in a container and placing it in an oven at 40 to 60° C. to dry;
[0012] (6) Soaking the dried hydrogel in deionized water until it is completely swollen to obtain chitosan / sodium hyaluronate hydrogel.
[0013] In step (1), the mass ratio of sodium hyaluronate to chitosan is 1-100:9.
[0014] In step (2), the mass concentration of the glacial acetic acid solution is 0.5-5.0%.
[0015] In step (3), the standing time is 2 to 24 hours.
[0016] In step (4), the preparation method of the mixed solution containing amino acids and chitosan is: dissolving chitosan in an aqueous solution of glacial acetic acid, then adding an aqueous solution of amino acids thereto, and mixing and stirring the mixture evenly.
[0017] Furthermore, in the mixed solution containing amino acids and chitosan, the mass ratio of chitosan to amino acids is 1:5-10.
[0018] The mass concentration of glacial acetic acid in the glacial acetic acid aqueous solution is 1-10%; the mass concentration of chitosan in the glacial acetic acid aqueous solution is 0.5-3.0%.
[0019] The amino acid mass concentration in the aqueous solution is 0.5 to 3.0%.
[0020] The amino acid is any one or more of arginine, lysine, and γ-aminobutyric acid.
[0021] In step (4), the ratio of the mass of the precipitate to the sum of the mass of the amino acid and the chitosan is 1.4 to 4.4:1.
[0022] In step (5), the mixture is placed in an oven at 40 to 60° C. for drying.
[0023] The present invention also provides a chitosan / sodium hyaluronate hydrogel prepared according to the preparation method of the present invention, wherein the strain range is 79-370%, the stress range is 0.08-0.20Mpa, and the swelling rate is 176-356%.
[0024] The preparation method of chitosan / sodium hyaluronate hydrogel based on amino acid / chitosan composite regulation provided by the present invention comprises the following steps: firstly, a mixed solution of sodium hyaluronate and chitosan is placed in a static state to separate a precipitate; the static state is separated and stratified to achieve the separation and rearrangement of the macro-aggregates of chitosan / sodium hyaluronate precipitate in the lower layer and the small molecular aggregates in the upper suspension, thereby eliminating the interference of the redundant small molecules on the subsequent crystallization process of the precipitated macro-aggregates and providing more cross-linking sites for the subsequent assembly of the hydrogel; and then, the residual small molecules in the structure of the precipitated macro-molecular aggregates are removed by water washing and the hydrophilic groups are rearranged to make the structure The structure is more regular and easy to penetrate and cross-link with amino acid / chitosan small molecule aggregates; then, a mixed solution containing amino acids and chitosan is added to the washed precipitate to obtain a hydrogel precursor liquid. The dropping process is essentially a process in which the topological structure of the precipitated macromolecular aggregates is regulated. In this process, relatively uniformly distributed amorphous topological entanglements are formed, which significantly improves the mechanical properties of the hydrogel; then, the hydrogel precursor liquid is spread flat in a container and placed in an oven at 40-60°C for drying. Drying further rearranges the macromolecular aggregates and crystallizes into a compact layered structure, further improving the mechanical properties of the hydrogel.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The present invention prepares chitosan / sodium hyaluronate hydrogel with high strength and toughness based on the composite regulation of amino acid / chitosan, and the method is original.
[0027] (2) The preparation method provided by the present invention greatly improves the tensile properties and strength of chitosan / sodium hyaluronate hydrogel, and improves its practical application potential, and can be applied to wound dressings, scar inhibition and cosmetic films, etc.
[0028] (3) The chitosan / sodium hyaluronate hydrogel provided by the present invention has adjustable structural properties, and chitosan / sodium hyaluronate hydrogels with different toughness can be prepared according to actual mechanical performance requirements by adjusting various factors, such as the mass ratio of chitosan / sodium hyaluronate precipitate to the mixed solution of amino acids and chitosan, the type of amino acids in the mixed solution of amino acids and chitosan, and the ratio of amino acids to chitosan, to prepare chitosan / sodium hyaluronate hydrogels with different toughness.
[0029] (4) The preparation conditions of the hydrogel in the present invention are mild, the cost is low, the equipment requirements are not high, and it is green and pollution-free, and has great development potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 are the mechanical properties of the hydrogels in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3;
[0031] Figure 2The mechanical properties and swelling properties of the hydrogels in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3;
[0032] Figure 3 is the cyclic compression performance of the hydrogels in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3;
[0033] Figure 4 are the contact angles and contact angle change rates of the hydrogels in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3;
[0034] Figure 5 are scanning electron microscope images of the hydrogels in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3;
[0035] Figure 6 The XRD diffraction patterns of the hydrogels in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3;
[0036] Figure 7 The SAXS scattering spectra of the hydrogels in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3;
[0037] Figure 8 IR spectra of the hydrogels in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3;
[0038] Fig. 9 2 are thermogravimetric diagrams of the hydrogels in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3. DETAILED DESCRIPTION
[0039] The present invention is described in detail below with reference to the embodiments.
[0040] Example 1
[0041] A method for preparing chitosan / sodium hyaluronate hydrogel based on amino acid / chitosan composite regulation comprises the following steps:
[0042] (1) Accurately weigh 1.12 g of sodium hyaluronate powder with a molecular weight of 370,000 Da and place it in an enzyme catalytic parallel reactor filled with 105 mL of deionized water. Set the temperature to 45° C. and the speed to 500 rpm for dissolution. After complete dissolution, add 1.68 g of chitosan powder with a molecular weight of 700,000 Da and stir for 5 min to evenly disperse the chitosan.
[0043] (2) adding 35 mL of 4% glacial acetic acid solution to the final solution of step (1), stirring for 10 min, and the resulting solution is defined as the precursor solution of chitosan / sodium hyaluronate hydrogel;
[0044] (3) transferring the chitosan / sodium hyaluronate hydrogel precursor solution obtained in step (2) into a small beaker and leaving it at room temperature for 24 hours;
[0045] (4) Separate the precipitate and supernatant in step (3), remove the supernatant with a syringe, retain the precipitate, add 1500 ml of deionized water to the precipitate, stir evenly with a glass rod, let stand for 24 hours, and remove the supernatant to obtain the washed precipitate;
[0046] (5) Preparation of a mixed solution containing amino acids and chitosan: Dissolve chitosan in a 4% glacial acetic acid aqueous solution to obtain a chitosan concentration of 2%. Then, under the conditions of 45°C and 500 rpm in a water bath, use an acid burette to slowly add 15 mL of the chitosan solution to 105 mL of a 2% arginine aqueous solution at a rate of 2 drops / second to obtain a mixed solution containing amino acids and chitosan.
[0047] (6) The washed precipitate obtained in step (4) was transferred to an enzyme catalytic parallel reactor, the temperature was set to 45°C, the rotation speed was set to 500 rpm, and the mixed solution containing amino acids and chitosan was added dropwise at a rate of 40 mL / h. After the addition was completed, the stirring reaction was continued for 108 min. The obtained solution was transferred to a beaker and allowed to stand for 2 h. The supernatant was removed with a syringe to obtain the hydrogel precursor solution;
[0048] (7) Divide the hydrogel precursor solution in step (6) into three equal portions, slowly pour them into three plastic culture dishes with a diameter of 9 cm, and spread them to a thickness of 0.84 cm. Dry them at 45°C overnight to form hydrogels.
[0049] (8) Soak the hydrogel dried in step (7) in 40 ml of deionized water until it is completely swollen to obtain chitosan / sodium hyaluronate hydrogel.
[0050] Example 2
[0051] The rest is the same as Example 1, except that step (5) is changed to: dissolving chitosan in a glacial acetic acid aqueous solution with a mass concentration of 4% to make the mass concentration of chitosan 2%, and then slowly adding 6 mL of the chitosan solution to 18 mL of a 2% arginine aqueous solution at a rate of 2 drops / second using an acid burette under water bath conditions at 45°C and 500 rpm to obtain a mixed solution containing amino acids and chitosan.
[0052] The strain of the hydrogel prepared in this embodiment is 361%, the stress is 0.08 Mpa, and the swelling rate is 354%.
[0053] Example 3
[0054] The rest is the same as Example 1, except that step (5) is changed to: dissolving chitosan in a glacial acetic acid aqueous solution with a mass concentration of 4% to make the mass concentration of chitosan 2%, and then slowly adding 6 mL of the chitosan solution to 18 mL of a 2% γ-aminobutyric acid aqueous solution at a rate of 2 drops / second using an acid burette under water bath conditions at 45°C and 500 rpm to obtain a mixed solution containing amino acids and chitosan.
[0055] The strain of the hydrogel prepared in this embodiment is 340%, the stress is 0.09 Mpa, and the swelling rate is 317%.
[0056] Example 4
[0057] The other steps are the same as those in Example 1, except that step (5) is changed to: dissolving chitosan in a glacial acetic acid aqueous solution with a mass concentration of 4% to make the mass concentration of chitosan 1%, and then slowly adding 6 mL of the chitosan solution to 18 mL of a lysine aqueous solution with a mass concentration of 1% at a rate of 2 drops / second using an acid burette under a water bath condition of 45°C and 500 rpm to obtain a mixed solution containing amino acids and chitosan. The hydrogel prepared in this example has a strain of 79%, a stress of 0.095 MPa, and a swelling ratio of 356%.
[0058] Comparative Example 1
[0059] A chitosan / sodium hyaluronate hydrogel and a preparation method thereof, comprising the following steps:
[0060] Steps (1) to (3) are the same as in Example 1;
[0061] (4) separating the precipitate and supernatant in step (3), removing the supernatant with a syringe, and retaining the precipitate;
[0062] (5) The precipitate obtained in step (4) was transferred to a magnetic stirrer, the temperature was set to 45°C, the speed was set to 500 rpm, and stirred for 5 min;
[0063] (6) Divide the hydrogel precursor solution in step (5) into three equal portions, slowly pour them into three 9 cm plastic culture dishes, spread them to a thickness of 0.47 cm, and dry them at 45°C overnight to form hydrogels;
[0064] (7) Soak the hydrogel dried in step (6) in 40 ml of deionized water until it is completely swollen to obtain chitosan / sodium hyaluronate hydrogel.
[0065] Comparative Example 2
[0066] A chitosan / sodium hyaluronate hydrogel and a preparation method thereof, comprising the following steps:
[0067] Steps (1) to (4) are the same as in Example 1;
[0068] (5) The washed precipitate obtained in step (4) was transferred to a magnetic stirrer, the temperature was set to 45°C, the speed was set to 500 rpm, and stirred for 5 min;
[0069] (6) Divide the hydrogel precursor solution in step (5) into three equal portions, slowly pour them into three 9 cm plastic culture dishes, spread them to a thickness of 0.47 cm, and dry them at 45°C overnight to form hydrogels;
[0070] (7) Soak the hydrogel dried in step (6) in 40 ml of deionized water until it is completely swollen to obtain chitosan / sodium hyaluronate hydrogel.
[0071] Comparative Example 3
[0072] The rest is the same as Example 1, except that step (4) is different. In step (4), the precipitate is not washed with water. Step (4) specifically comprises: separating the precipitate and the supernatant in step (3), removing the supernatant with a syringe, and retaining the precipitate.
[0073] Test Case
[0074] The various properties of the hydrogels obtained in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested, and the results are shown below.
[0075] 1. Mechanical properties testing
[0076] A texture analyzer was used to perform uniaxial tensile tests on the hydrogel films obtained in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3. The hydrogel film samples were cut into strips with a length of 50 mm and a width of 5 mm, and their thickness was measured using a spiral micrometer. The trigger point load was 1 g, and the tensile rate was 2 mm / s.
[0077] Toughness and Young's modulus are calculated from stress-strain curves, and stress-strain mechanical properties are measured using a universal tensile machine. Toughness (T) and Young's modulus are calculated using formulas (2-1) and (2-2).
[0078] T=σdε(2-1)
[0079] σ and ε are the stress and strain of the hydrogel, respectively.
[0080]
[0081] S m and Eb m The values corresponding to the first 50% stretching are taken, and W and T refer to the width (mm) and thickness (mm) of the hydrogel, respectively.
[0082] The results are as follows Figure 1 and2 As shown. As can be seen from the figure, the stress and strain of the hydrogel prepared in Example 1 are the largest, and the toughness is the highest. It can be seen from Comparative Examples 1 and 2 that the stress of the hydrogel is improved by washing the chitosan / sodium hyaluronate precipitate with deionized water; it can be seen from Comparative Examples 1 and 3 that the regulation of the mixed solution containing amino acids and chitosan improves the tensile capacity of the hydrogel. First, static stratification realizes the separation and rearrangement of the lower chitosan / sodium hyaluronate precipitate macroaggregates and the small molecule aggregates in the upper suspension, eliminates the interference of excess small molecules on the subsequent crystallization process of the precipitate macroaggregates, and provides more cross-linking sites for the subsequent assembly of the hydrogel. The water washing operation can remove the small molecules remaining in the structure of the precipitated macromolecular aggregates, and rearrange their hydrophilic groups, making the structure more regular, easy to penetrate and cross-link with arginine / chitosan small molecule aggregates, forming a relatively uniformly distributed amorphous topological entanglement, and significantly improving the mechanical properties of the hydrogel. The addition process of the mixed solution containing amino acids and chitosan is essentially the process in which the topological structure of the precipitated macromolecular aggregates is regulated.
[0083] 2. Swelling performance test
[0084] The specific experimental steps for swelling performance testing are as follows: First, place the prepared sample in a constant temperature drying oven, completely dry it at 45°C and weigh it. Next, place the sample in distilled water, and after it is fully swollen, use filter paper to absorb the surface moisture and weigh it again. Each group of samples is tested in parallel 4 times. The swelling rate (SR) of the hydrogel can be calculated according to the following formula:
[0085]
[0086] Among them, M 0 is the weight of the dried gel after drying; M 1 is the weight of the gel when swelling equilibrium is reached.
[0087] The results are as follows Figure 2 As shown in the figure, it can be seen that water washing reduces the swelling rate of the hydrogel, and the introduction of the mixed solution of arginine and chitosan after water washing increases the swelling rate of the hydrogel. This is because the water washing operation can remove the small molecules with stronger hydrophilicity remaining in the structure of the precipitated macromolecular aggregates, thereby reducing the swelling rate. Since arginine contains a guanidine group with strong hydrophilicity, the introduction of the mixed solution of arginine and chitosan increases the swelling rate of the hydrogel.
[0088] 3. Compression performance test
[0089] The compression performance determination method is: a compression test is performed using a texture analyzer. Test type: compression, target: 80% of the sample height, trigger point load: 1g, test speed: 0.1mm / s, return speed: 0.1mm / s, number of cycles: 10 times, recoverable time: 5s, shape: block (the sample is shaped into a regular rectangular block and filled in its size).
[0090] The results are as follows Figure 3 As shown in the figure, the compression and recovery properties of the hydrogel were significantly enhanced by washing the chitosan / sodium hyaluronate precipitate with deionized water and adding a mixed solution containing amino acids and chitosan.
[0091] 4. Contact angle measurement
[0092] An optical contact angle meter was used to measure the contact angle of the hydrogel films obtained in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3. The hydrogel was molded into a 1 cm × 1 cm sheet, immersed in deionized water to fully swell, taken out to remove the free water on the surface, and fixed on a glass slide for measurement.
[0093] like Figure 4 As shown, it can be seen that the hydrogels are ultimately hydrophilic, because the high molecular polymer in the hydrogel has a large pore structure or porosity, which can accommodate water molecules and interact with them. This high water absorption allows the hydrogel to quickly absorb surrounding water and maintain its hydrophilicity. The hydrophilicity of the hydrogel in Example 1 is the best, which may be due to the presence of a microscopic multi-level structure on its surface, which has a low surface energy, allowing water molecules to penetrate more easily, showing a high hydrophilicity.
[0094] 3. Scanning electron microscope detection
[0095] The scanning electron microscope was used to observe Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3. Figure 5 As shown. By observing Comparative Example 1 and Comparative Example 2, it can be seen that the drying effect causes the macromolecular aggregates to rearrange and crystallize into a compact layered structure. Comparative Example 1 contains unwashed small molecule aggregates, which are cross-linked and adsorbed on the macromolecular aggregates, so the surface is smoother than that of Comparative Example 2. The mixed solution containing amino acids and chitosan can adjust the network structure and form new thorn-like crystals. This structure can improve the tensile properties of the hydrogel. Compared with Example 1, the number of thorn-like crystals in Comparative Example 3 is less and the shape is sharper. The possible reason is that the cross-linking occurs between the arginine / chitosan small molecule aggregates and the unwashed small molecule aggregates.
[0096] 4. XRD detection
[0097] The hydrogels of Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were completely dried to remove moisture, cut into squares with a length and width of about 1.5 cm, and the X-ray diffraction spectra were measured using an X-ray diffractometer. The results are shown in FIG. Figure 6 As shown. Except for the hydrogel in Example 1, the other samples all have a sharp peak at about 26°. The sharper the peak, the higher the peak intensity, and the higher the crystallinity of the sample. It can be seen from Comparative Examples 1 and 2 that water washing can improve the crystallinity, which is consistent with the electron microscope image; it can be seen from Comparative Examples 1 and 3 that the introduction of arginine / chitosan small molecule aggregates reduces the crystallinity. In Comparative Example 3, cross-linking occurs between the arginine / chitosan small molecule aggregates and the unwashed small molecule aggregates, so the crystallinity of Example 1 is greater than that of Comparative Example 3.
[0098] 5. SAXS detection
[0099] The X-ray scattering spectra of Example 1, Comparative Example 1 and Comparative Example 2 were measured using a small-angle X-ray scattering instrument. The small-angle X-ray scattering spectra of different samples were shifted, indicating that there were structural and morphological differences between the samples, such as Figure 7 As shown. The hydrogel of Comparative Example 1 shows the broadest peak, indicating that it has the largest average particle size. The hydrogel of Comparative Example 2 shows the narrowest peak, indicating that it has the smallest average particle size. The particle size of the hydrogel of Example 1 is between the two.
[0100] 6. Infrared detection
[0101] The infrared spectra of Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were measured by Fourier transform infrared spectrometer. Figure 8 As shown, at 3250cm -1 Up to 3750cm -1 The broad peak at 1637.5cm is a multiple absorption peak formed by the vibration peak of -NH and the stretching vibration peak of -OH, reflecting the existence of different strengths of intermolecular and intramolecular hydrogen bonds between amino and hydroxyl groups in different samples. -1 The stretching vibration peaks of C=O of carboxylic acids and the bending vibration peaks of NH bonds of amines are located at 900 cm -1 Up to 1171cm -1 The peaks near 1000-400 cm indicate the presence of sugar structures in the composite system. -1 The fingerprint regions of the hydrogels were quite different, indicating that the addition of arginine / chitosan small molecules and the washing operation played an important role in the self-assembly of the hydrogels.
[0102] 7. Thermal stability test
[0103] The hydrogels of Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were dried to completely remove moisture, and about 5 mg of the hydrogel was placed in a ceramic crucible. The thermal stability of the hydrogel was measured at 30-700°C, with a temperature rise of 10°C / min in a nitrogen atmosphere, an oxygen atmosphere in an experimental atmosphere, and a rate of 20 mL / min. The results are shown in FIG. Fig. 9 As shown. The thermal decomposition process is mainly divided into three stages. 100℃-185℃ is the first weight loss stage, which is mainly the volatilization of free water remaining in the hydrogel network structure. 180℃-400℃ is the second weight loss stage, which mainly includes the evaporation of bound water inside the hydrogel and the random breakage of glycosidic bonds. 400-700℃ is the third weight loss stage, which is mainly the depolymerization of sugar rings inside the matrix and the decomposition of polysaccharide structures. It can be seen that the weight loss ratio of different samples in the second stage is quite different, which reflects the different thermal stability of different structures. The differential thermogravimetric curve can better analyze the thermal decomposition process of the material. It can be seen that in the first stage, the thermal stability of Example 1 is the highest, and the thermal stability of Comparative Example 3 is the lowest. In the second and third stages, the thermal stability of Comparative Example 3 is the highest. The possible reason is that Example 1 has the highest hydrophilicity and surface energy, so it is not easy to lose water in the first stage. The swelling rate of the hydrogel in Comparative Example 3 is high, so it is easy to lose water in the first stage. In the second and third stages, due to its most complex cross-linked network structure, the stability is the highest.
[0104] The detailed description of a chitosan / sodium hyaluronate hydrogel based on amino acid / chitosan composite regulation and its preparation method with reference to the above-mentioned examples is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A method for preparing chitosan / sodium hyaluronate hydrogel based on amino acid / chitosan composite regulation, characterized in that: The preparation method comprises the following steps: (1) heating and stirring sodium hyaluronate powder in water until completely dissolved, then adding chitosan powder and stirring to make it evenly dispersed; (2) adding glacial acetic acid solution to step (1) until the chitosan is completely dissolved, and continuing to stir until the mixture is uniformly mixed; (3) allowing the reaction solution obtained in step (2) to stand at room temperature, separating the precipitate and the supernatant, washing the precipitate with deionized water, and then allowing the precipitate to stand again to collect the precipitate; (4) adding a mixed solution containing amino acids and chitosan to the precipitate obtained in step (3), stirring and dispersing the mixture evenly, allowing the mixture to stand, and removing the supernatant to obtain a hydrogel precursor solution; (5) spreading the hydrogel precursor liquid evenly in a container and allowing it to stand to dry; (6) Soaking the dried hydrogel in deionized water until it is completely swollen to obtain chitosan / sodium hyaluronate hydrogel.
2. The preparation method according to claim 1, characterized in that: In step (1), the mass ratio of sodium hyaluronate to chitosan is 1-100:
9.
3. The preparation method according to claim 1, characterized in that: In step (2), the mass concentration of the glacial acetic acid solution is 0.5-5.0%.
4. The preparation method according to claim 1, characterized in that: In step (4), the preparation method of the mixed solution containing amino acids and chitosan is: dissolving chitosan in an aqueous solution of glacial acetic acid, then adding an aqueous solution of amino acids thereto, and mixing and stirring the mixture evenly.
5. The preparation method according to claim 4, characterized in that: In the mixed solution containing amino acid and chitosan, the mass ratio of chitosan to amino acid is 1:5-10.
6. The preparation method according to claim 4, characterized in that: The mass concentration of glacial acetic acid in the glacial acetic acid aqueous solution is 1-10%; the mass concentration of chitosan in the glacial acetic acid aqueous solution is 0.5-3.0%.
7. The preparation method according to claim 4, characterized in that: The amino acid mass concentration in the aqueous solution is 0.5 to 3.0%.
8. The preparation method according to claim 4, characterized in that: The amino acid is any one or more of arginine, lysine, and γ-aminobutyric acid.
9. The preparation method according to claim 1, characterized in that: In step (4), the ratio of the mass of the precipitate to the sum of the mass of the amino acid and the chitosan is 1.4 to 4.4:
1.