A high voltage breakdown resistant polyimide film and preparation method thereof
By using hexagonal sheet alumina, hexagonal boron nitride and layered clay as inorganic fillers, the problem of limited improvement in high-pressure breakdown performance of polyimide films is solved, and an efficient charge and heat barrier is achieved, which significantly improves the film. corona resistance and thermal conductivity.
Patent Information
- Application Number
- CN202411244435.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-06
AI Technical Summary
In the prior art, when using inorganic fillers of different particle sizes to prepare polyimide films, high-pressure breakdown resistance and thermal conductivity improvements are limited, and nanoparticles and polymers with higher viscosity are difficult to achieve ideal nanoscale recombination, which affects the film. Comprehensive performance.
Hexagonal sheet alumina, hexagonal boron nitride and layered clay are used as inorganic fillers, and the two-dimensional structure of layered clay is used to form a shielding effect, hinder charge movement, and adsorb alumina and boron nitride through clay to improve the film's resistance High temperature and high pressure breakdown resistance.
It significantly improves the corona resistance time and thermal conductivity of the polyimide film, and can maintain a corona resistance time of 90 to 210 minutes under a 2kV voltage, and the thermal conductivity coefficient reaches 0.99 to 1.33W/m·K, ensuring that between electromagnetic lines No short circuit phenomenon.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyimide films, and in particular to a high-voltage breakdown resistant polyimide film and a preparation method thereof. Background Art
[0002] Polyimide film is a new type of high-temperature resistant organic polymer film. It has high modulus, low shrinkage, high strength, low water absorption, hydrolysis resistance, radiation resistance, non-toxicity, excellent insulation and thermal oxidation stability. It is called "golden film" because it is one of the most expensive film materials in the world. It is a key insulating material for high-speed motors and a key voltage-resistant material for ultra-high voltage electronic coils.
[0003] Inorganic nanofillers play an important role in the performance of polyimide films. For example, the overall strength of polyimide films can be increased through the interfacial interaction between inorganic nanofillers such as silica and alumina and the polyimide matrix. However, due to the large specific surface area and surface energy of nanoparticles, there are strong interactions between particles, which are prone to agglomeration. It is difficult to achieve an ideal nanoscale composite between nanoparticles and polymers with high viscosity, which affects the comprehensive performance and product quality of the final polyimide film.
[0004] Prior art CN111087633A discloses a method for preparing a corona-resistant polyimide film, which introduces a first inorganic filler and a second inorganic filler of different particle sizes to form a maximum stacking degree of the filler, and then combines the chemical imidization method to establish a uniform thermal conductive network inside the film. This method can improve the dispersibility of the inorganic filler in the system to a certain extent and avoid the occurrence of inorganic filler agglomeration or sedimentation, but the effect of improving the performance of the polyimide film is limited. Summary of the invention
[0005] In view of the technical problem that the high-voltage breakdown resistance and thermal conductivity of a polyimide film prepared by using inorganic fillers of different particle sizes are limitedly improved, the present invention provides a high-voltage breakdown resistant polyimide film and a preparation method thereof, using hexagonal flaky aluminum oxide, hexagonal boron nitride and layered clay as inorganic fillers, utilizing the structural characteristics of silicate minerals in the layered clay, which are a series of [ZO4] tetrahedrons connected by corner vertices to form a two-dimensional infinitely extended layered silicon-oxygen backbone (hexagonal mesh-like single layer), to form a layered shield to hinder the movement of charges; at the same time, utilizing the adsorption effect of clay on hexagonal flaky aluminum oxide and hexagonal boron nitride, aluminum oxide and boron nitride are attached to the surface of the layered clay, thereby further improving the high temperature resistance and high-voltage breakdown resistance of the film surface.
[0006] In a first aspect, the present invention provides a method for preparing a high voltage breakdown resistant polyimide film, comprising the following steps:
[0007] (1) 1200-1400 parts by weight of dimethylformamide, 50-70 parts by weight of 4,4-diaminodiphenyl ether and 15-20 parts by weight of p-phenylenediamine are stirred and mixed;
[0008] (2) adding 75 to 100 parts by weight of pyromellitic anhydride to the material obtained in step (1), stirring and mixing, and continuously introducing nitrogen during the stirring process to obtain a mixture 1;
[0009] (3) mixing an inorganic auxiliary agent with 50 to 100 parts by weight of dimethylformamide and stirring them uniformly to obtain a second mixture, wherein the inorganic auxiliary agent comprises 0.5 to 1.5 parts by weight of hexagonal boron nitride, 3 to 6 parts by weight of hexagonal flaky aluminum oxide and 3 to 5 parts by weight of layered clay;
[0010] (4) adding mixture 2 into mixture 1 and stirring to form a polyamic acid solution;
[0011] (5) The polyamic acid solution is mixed with 750-1000 parts by weight of acetic anhydride and then mixed with 20-25 parts by weight of pyridine, and the mixture is spread and dried to form a film;
[0012] (6) The film obtained in step (5) is introduced into an imidization furnace, and after high-temperature imidization, it is rolled up to obtain the film.
[0013] Furthermore, the preparation method comprises the following steps:
[0014] (1) 1280 parts by weight of dimethylformamide, 65 parts by weight of 4,4-diaminodiphenyl ether and 17 parts by weight of p-phenylenediamine were stirred and mixed;
[0015] (2) adding 80 parts by weight of pyromellitic dianhydride to the material obtained in step (1), stirring and mixing, and continuously introducing nitrogen during the stirring process to obtain a mixture 1;
[0016] (3) mixing an inorganic auxiliary agent with 80 parts by weight of dimethylformamide and stirring them uniformly to obtain a second mixture, wherein the inorganic auxiliary agent includes 1.1 parts by weight of hexagonal boron nitride, 5 parts by weight of hexagonal flaky aluminum oxide and 3.7 parts by weight of layered clay;
[0017] (4) adding mixture 2 into mixture 1 and stirring to form a polyamic acid solution;
[0018] (5) The polyamic acid solution is mixed with 800 parts by weight of acetic anhydride and then mixed with 23 parts by weight of pyridine, and the mixture is spread and dried to form a film;
[0019] (6) The film obtained in step (5) is introduced into an imidization furnace, and after high-temperature imidization, it is rolled up to obtain the film.
[0020] Furthermore, in step (1), dimethylformamide is first added into the reactor and stirred for 5-10 min at a temperature of 8-10° C. and a stirring speed of 100-200 r / min; then 4,4-diaminodiphenyl ether and p-phenylenediamine are added and stirred together for 20-40 min at a temperature of 8-15° C. and a stirring speed of 200-500 r / min.
[0021] Furthermore, in step (2), the addition time of pyromellitic anhydride is 30-60 min, the temperature is 8-15° C., and the stirring speed is 300-400 r / min.
[0022] Furthermore, in step (3), the average particle size of hexagonal boron nitride is 0.5-1 μm, and the average particle size of hexagonal flaky aluminum oxide is 200-500 nm.
[0023] Furthermore, in step (4), the stirring time is 60-130 min, the temperature is 8-15° C., and the stirring speed is 400-500 r / min.
[0024] Furthermore, step (4) further comprises defoaming the polyamic acid solution obtained by stirring.
[0025] Furthermore, step (5) is specifically as follows: conveying the defoamed polyamic acid solution to a storage tank of a casting nozzle, mixing the polyamic acid solution and acetic anhydride at low temperature in the storage tank, controlling the system temperature to be maintained at 0-5°C, and then conveying the mixed solution in the storage tank to a pin-bar mixer of a die head, mixing with pyridine at -5-0°C, and then taking it away through a scraper in front of the casting nozzle, taking a film using a film laying machine, and drying the film so that the temperature of the film gradually rises during drying, the solvent gradually evaporates, and imidization is performed to form a film.
[0026] Furthermore, in step (6), the film passes through the first temperature zone, the second temperature zone, the third temperature zone, the fourth temperature zone, the fifth temperature zone and the sixth temperature zone in the imidization furnace in sequence, and the heating temperatures of each temperature zone are 200-220°C, 250-300°C, 300-350°C, 400-450°C, 500-550°C and 450-500°C in sequence, and the heating time of each temperature zone is 10-20s.
[0027] In a second aspect, the present invention provides a polyimide film prepared by the above preparation method.
[0028] The beneficial effects of the present invention are:
[0029] The present invention adds hexagonal flaky aluminum oxide, hexagonal boron nitride and layered clay in the process of synthesizing the polyamic acid solution to improve the corona resistance. The hexagonal flaky aluminum oxide has strong charge conductivity, can effectively alleviate the charge accumulation under local discharge, and make the charge dissipate quickly; the hexagonal boron nitride has strong heat resistance and heat conductivity, can effectively alleviate the heat accumulation under local discharge, and can improve the high-voltage breakdown resistance; the layered clay has a silicate mineral with a layered silicon-oxygen backbone formed by a series of [ZO4] tetrahedrons connected by corner vertices to form a two-dimensional infinitely extended layered silicon-oxygen backbone. The most common silicon-oxygen backbone is that each tetrahedron is connected with three surrounding tetrahedrons by three corner vertices to form a hexagonal mesh-shaped single layer. Clay is used as a carrier to allow aluminum oxide and boron nitride to be adsorbed on the surface of the layered clay, thereby increasing the high-voltage and high-frequency breakdown resistance of the membrane surface, achieving no breakdown in a 2KV voltage test, and ensuring that there is no short circuit between electromagnetic wires.
[0030] The polyimide film prepared by the preparation method of the present invention has good and stable mechanical properties, high voltage breakdown resistance and heat resistance, especially the corona resistance time under 2kV test voltage can reach 90-210min, and the thermal conductivity can reach 0.99-1.33W / m·K. DETAILED DESCRIPTION
[0031] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0032] Example 1
[0033] A high voltage breakdown resistant polyimide film, prepared by the following method:
[0034] (1) Prepare a reactor with nitrogen protection, put 1400 parts by weight of dimethylformamide into the reactor, and open the reactor. Use a stirring device in the reactor to pre-stir the dimethylformamide for 10 minutes, control the temperature at 8-10°C, and stir at a speed of 200 r / min. Then add 70 parts by weight of 4,4-diaminodiphenyl ether and 20 parts by weight of p-phenylenediamine, and continue stirring and mixing for 40 minutes. Control the temperature at 8-15°C and stir at a speed of 500 r / min.
[0035] (2) adding 100 parts by weight of pyromellitic anhydride to the material obtained in step (1) in six portions, stirring and mixing while adding, controlling the addition time of pyromellitic anhydride to be 60 min, maintaining the temperature at 8-15° C., stirring at a speed of 400 r / min, and continuously introducing nitrogen during stirring to obtain a mixture 1;
[0036] (3) mixing an inorganic auxiliary agent with 100 parts by weight of dimethylformamide and stirring them uniformly to obtain a second mixture, wherein the inorganic auxiliary agent comprises 1.5 parts by weight of hexagonal boron nitride (with an average particle size of 1 μm), 6 parts by weight of hexagonal lamellar aluminum oxide (with an average particle size of 200 nm) and 5 parts by weight of layered clay;
[0037] (4) Adding mixture 2 into mixture 1 and stirring for 130 minutes, the temperature is controlled at 8-15°C, the stirring speed is 500 r / min, to form a polyamic acid solution, and the polyamic acid solution is placed in a defoamer for defoaming;
[0038] (5) The defoamed polyamic acid solution is transported to the storage tank of the casting nozzle, and the polyamic acid solution and 1000 parts by weight of acetic anhydride are mixed at low temperature in the storage tank, and the system temperature is controlled to be maintained at 0~5°C. Then, the mixed solution in the storage tank is transported to the pin-bar mixer of the die head, and mixed with 25 parts by weight of pyridine at -5~0°C. The solution is then taken away by the scraper in front of the casting nozzle, and a film is taken by a film laying machine. The film is sent to a drying channel (mirror steel belt in the casting machine, a total of 30m) for drying. The film speed is 18m / min, the drying temperature of the first 15m drying channel is 135°C, and the drying temperature of the last 15m drying channel is 145°C, so that the temperature of the film gradually increases during drying, the solvent gradually evaporates, and imidization film is formed;
[0039] (6) The film obtained in step (5) is introduced into an imidization furnace at a speed of 18 m / min, and sequentially passes through the first temperature zone, the second temperature zone, the third temperature zone, the fourth temperature zone, the fifth temperature zone and the sixth temperature zone, wherein the heating temperatures of each temperature zone are 220°C, 300°C, 350°C, 450°C, 550°C and 500°C, respectively, and the heating time of each temperature zone is 10 s. The film is then rolled up to obtain the film.
[0040] Comparative Example 1
[0041] A polyimide film, the preparation method of which is basically the same as that of Example 1, the only difference being the type of inorganic additive in step (3). In Comparative Example 1, only 2.5 parts by weight of hexagonal boron nitride (average particle size of 1 μm) and 10 parts by weight of hexagonal flaky aluminum oxide (average particle size of 200 nm) are used.
[0042] Comparative Example 2
[0043] A polyimide film, the preparation method of which is basically the same as that of Example 1, the only difference being the type of inorganic additive in step (3). In Comparative Example 2, only 7.5 parts by weight of hexagonal boron nitride (average particle size of 1 μm) and 5 parts by weight of layered clay are used.
[0044] Example 2
[0045] A high voltage breakdown resistant polyimide film, prepared by the following method:
[0046] (1) Prepare a reactor with nitrogen protection, put 1280 parts by weight of dimethylformamide into the reactor, and open the reactor. Use a stirring device in the reactor to pre-stir the dimethylformamide for 8 minutes, control the temperature at 8-10°C, and stir at a speed of 200 r / min. Then add 65 parts by weight of 4,4-diaminodiphenyl ether and 17 parts by weight of p-phenylenediamine, and continue stirring and mixing for 30 minutes. Control the temperature at 8-15°C and stir at a speed of 400 r / min.
[0047] (2) adding 80 parts by weight of pyromellitic anhydride to the material obtained in step (1) in six portions, stirring and mixing while adding, controlling the addition time of pyromellitic anhydride to be 45 min, maintaining the temperature at 8-15° C., stirring at a speed of 400 r / min, and continuously introducing nitrogen during stirring to obtain a mixture 1;
[0048] (3) mixing an inorganic auxiliary agent with 80 parts by weight of dimethylformamide and stirring them uniformly to obtain a second mixture, wherein the inorganic auxiliary agent comprises 1.1 parts by weight of hexagonal boron nitride (with an average particle size of 1 μm), 5 parts by weight of hexagonal lamellar aluminum oxide (with an average particle size of 300 nm) and 3.7 parts by weight of layered clay;
[0049] (4) Adding mixture 2 into mixture 1 and stirring for 90 minutes, the temperature is controlled at 8-15°C, the stirring speed is 400 r / min, to form a polyamic acid solution, and the polyamic acid solution is placed in a defoamer for defoaming;
[0050] (5) The defoamed polyamic acid solution is transported to the storage tank of the casting nozzle, and the polyamic acid solution and 800 parts by weight of acetic anhydride are mixed at low temperature in the storage tank, and the system temperature is controlled to be maintained at 0-5°C. Then, the mixed solution in the storage tank is transported to the pin-bar mixer of the die head, and mixed with 23 parts by weight of pyridine at -5-0°C. The solution is then taken away by the scraper in front of the casting nozzle, and a film is taken by a film laying machine. The film is sent to a drying channel (a mirror steel belt in a casting machine, a total of 30 m) for drying. The film speed is 18 m / min, the drying temperature of the first 15 m of the drying channel is 135°C, and the drying temperature of the last 15 m of the drying channel is 145°C, so that the temperature of the film gradually increases during drying, the solvent gradually evaporates, and imidization film is formed;
[0051] (6) The film obtained in step (5) is introduced into an imidization furnace at a speed of 18 m / min, and sequentially passes through the first temperature zone, the second temperature zone, the third temperature zone, the fourth temperature zone, the fifth temperature zone and the sixth temperature zone, wherein the heating temperatures of each temperature zone are 210°C, 275°C, 325°C, 425°C, 525°C and 480°C, respectively, and the heating time of each temperature zone is 15 s. The film is then rolled up to obtain the film.
[0052] Comparative Example 3
[0053] A polyimide film, the preparation method of which is basically the same as that of Example 2, the only difference being the type of inorganic additive in step (3). In Comparative Example 3, only 1.8 parts by weight of hexagonal boron nitride (average particle size of 1 μm) and 8 parts by weight of hexagonal flaky aluminum oxide (average particle size of 300 nm) are used.
[0054] Comparative Example 4
[0055] A polyimide film, the preparation method of which is basically the same as that of Example 2, the only difference being the type of inorganic additive in step (3). In Comparative Example 4, only 6.1 parts by weight of hexagonal boron nitride (average particle size of 1 μm) and 3.7 parts by weight of layered clay are used.
[0056] Example 3
[0057] A high voltage breakdown resistant polyimide film, prepared by the following method:
[0058] (1) Prepare a reactor with nitrogen protection, put 1200 parts by weight of dimethylformamide into the reactor, and open the reactor. Use a stirring device in the reactor to pre-stir the dimethylformamide for 5 minutes, control the temperature at 8-10°C, and stir at a speed of 100 r / min. Then add 70 parts by weight of 4,4-diaminodiphenyl ether and 15 parts by weight of p-phenylenediamine, continue stirring and mixing for 20 minutes, control the temperature at 8-15°C, and stir at a speed of 200 r / min.
[0059] (2) adding 75 parts by weight of pyromellitic anhydride to the material obtained in step (1) in six portions, stirring and mixing while adding, controlling the addition time of pyromellitic anhydride to be 30 min, maintaining the temperature at 8-15° C., stirring at a speed of 300 r / min, and continuously introducing nitrogen during stirring to obtain a mixture 1;
[0060] (3) mixing an inorganic auxiliary agent with 50 parts by weight of dimethylformamide and stirring them uniformly to obtain a second mixture, wherein the inorganic auxiliary agent comprises 0.5 parts by weight of hexagonal boron nitride (with an average particle size of 0.5 μm), 3 parts by weight of hexagonal lamellar aluminum oxide (with an average particle size of 500 nm) and 3 parts by weight of layered clay;
[0061] (4) Adding mixture 2 into mixture 1 and stirring for 60 minutes, the temperature is controlled at 8-15°C, the stirring speed is 400 r / min, to form a polyamic acid solution, and the polyamic acid solution is placed in a defoamer for defoaming;
[0062] (5) The defoamed polyamic acid solution is transported to the storage tank of the casting nozzle, and the polyamic acid solution and 750 parts by weight of acetic anhydride are mixed at low temperature in the storage tank, and the system temperature is controlled to be maintained at 0~5°C. Then, the mixed solution in the storage tank is transported to the pin-bar mixer of the die head, and mixed with 20 parts by weight of pyridine at -5~0°C. The solution is then taken away by the scraper in front of the casting nozzle, and a film is taken by a film laying machine. The film is sent to a drying channel (a mirror steel belt in a casting machine, a total of 30m) for drying. The film speed is 18m / min, the drying temperature of the first 15m drying channel is 135°C, and the drying temperature of the last 15m drying channel is 145°C, so that the temperature of the film gradually increases during drying, the solvent gradually evaporates, and imidization film is formed;
[0063] (6) The film obtained in step (5) is introduced into an imidization furnace at a speed of 18 m / min, and sequentially passes through the first temperature zone, the second temperature zone, the third temperature zone, the fourth temperature zone, the fifth temperature zone and the sixth temperature zone, wherein the heating temperatures of each temperature zone are 200°C, 250°C, 300°C, 400°C, 500°C and 450°C, respectively, and the heating time of each temperature zone is 20 s. The film is then rolled up to obtain the film.
[0064] Comparative Example 5
[0065] A polyimide film, the preparation method of which is basically the same as that of Example 3, the only difference being the type of inorganic additive in step (3). In Comparative Example 5, only 1 part by weight of hexagonal boron nitride (average particle size of 0.5 μm) and 5 parts by weight of hexagonal flaky aluminum oxide (average particle size of 500 nm) are used.
[0066] Comparative Example 6
[0067] A polyimide film, the preparation method of which is basically the same as that of Example 3, the only difference being the type of inorganic additive in step (3). In Comparative Example 6, only 3.5 parts by weight of hexagonal boron nitride (average particle size of 0.5 μm) and 3 parts by weight of layered clay are used.
[0068] According to the GB / T13542.2-2021 standard, the thickness, tensile fracture resistance, corona resistance time and thermal conductivity of the polyimide film of the embodiment and the comparative example were tested. The test conditions for the corona resistance time are: experimental voltage 2kV, experimental frequency 20kHz, pulse rise time 50ns, bipolar pulse square wave, 6mm cylindrical electrode.
[0069] The test results are shown in Table 1 below.
[0070] Table 1 Performance test results of polyimide films of Examples and Comparative Examples
[0071]
[0072] It can be seen from Table 1 that, compared with using only two of them, at the same film thickness, the corona resistance time and thermal conductivity of the film prepared by the present invention using hexagonal flaky aluminum oxide, hexagonal boron nitride and layered clay as inorganic additives are greatly improved, indicating that the three materials synergistically form a better charge barrier and can effectively alleviate the accumulation of charge and heat, thereby improving the high temperature resistance and high voltage breakdown resistance of the film surface.
[0073] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and such modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily conceive of changes or substitutions within the technical scope disclosed by the present invention, and such changes or substitutions shall be within the scope of protection of the present invention.
Claims
1. A method for preparing a high voltage breakdown resistant polyimide film, characterized in that: The steps include: (1) 1200-1400 parts by weight of dimethylformamide, 50-70 parts by weight of 4,4-diaminodiphenyl ether and 15-20 parts by weight of p-phenylenediamine are stirred and mixed; (2) adding 75 to 100 parts by weight of pyromellitic anhydride to the material obtained in step (1), stirring and mixing, and continuously introducing nitrogen during the stirring process to obtain a mixture 1; (3) mixing an inorganic auxiliary agent with 50 to 100 parts by weight of dimethylformamide and stirring them uniformly to obtain a second mixture, wherein the inorganic auxiliary agent comprises 0.5 to 1.5 parts by weight of hexagonal boron nitride, 3 to 6 parts by weight of hexagonal flaky aluminum oxide and 3 to 5 parts by weight of layered clay; The average particle size of hexagonal boron nitride is 0.5~1μm, and the average particle size of hexagonal alumina is 200~500nm; (4) adding mixture 2 into mixture 1 and stirring to form a polyamic acid solution; (5) The polyamic acid solution is mixed with 750-1000 parts by weight of acetic anhydride and then mixed with 20-25 parts by weight of pyridine, and the mixture is spread and dried to form a film; (6) The film obtained in step (5) is introduced into an imidization furnace, and after high-temperature imidization, it is rolled up to obtain the film.
2. The preparation method according to claim 1, characterized in that The preparation method comprises the following steps: (1) 1280 parts by weight of dimethylformamide, 65 parts by weight of 4,4-diaminodiphenyl ether and 17 parts by weight of p-phenylenediamine were stirred and mixed; (2) adding 80 parts by weight of pyromellitic dianhydride to the material obtained in step (1), stirring and mixing, and continuously introducing nitrogen during the stirring process to obtain a mixture 1; (3) mixing an inorganic auxiliary agent with 80 parts by weight of dimethylformamide and stirring them uniformly to obtain a second mixture, wherein the inorganic auxiliary agent includes 1.1 parts by weight of hexagonal boron nitride, 5 parts by weight of hexagonal flaky aluminum oxide and 3.7 parts by weight of layered clay; (4) adding mixture 2 into mixture 1 and stirring to form a polyamic acid solution; (5) The polyamic acid solution is mixed with 800 parts by weight of acetic anhydride and then mixed with 23 parts by weight of pyridine, and the mixture is spread and dried to form a film; (6) The film obtained in step (5) is introduced into an imidization furnace, and after high-temperature imidization, it is rolled up to obtain the film.
3. The preparation method according to claim 1, characterized in that: In step (1), dimethylformamide is first added into a reactor and stirred for 5 to 10 minutes at a temperature of 8 to 10° C. and a stirring speed of 100 to 200 r / min; then 4,4-diaminodiphenyl ether and p-phenylenediamine are added and stirred together for 20 to 40 minutes at a temperature of 8 to 15° C. and a stirring speed of 200 to 500 r / min.
4. The preparation method according to claim 1, characterized in that: In step (2), the addition time of pyromellitic anhydride is 30-60 min, the temperature is 8-15° C., and the stirring speed is 300-400 r / min.
5. The preparation method according to claim 1, characterized in that: In step (4), the stirring time is 60-130 min, the temperature is 8-15° C., and the stirring speed is 400-500 r / min.
6. The preparation method according to claim 1, characterized in that: Step (4) further comprises defoaming the polyamic acid solution obtained by stirring.
7. The preparation method according to claim 1, characterized in that: Step (5) specifically comprises conveying the defoamed polyamic acid solution to a storage tank of a casting nozzle, mixing the polyamic acid solution and acetic anhydride at low temperature in the storage tank, controlling the system temperature to be maintained at 0-5°C, then conveying the mixed solution in the storage tank to a needle bar mixer of a die head, mixing with pyridine at -5-0°C, and then taking it away through a scraper in front of the casting nozzle, taking out a film using a film laying machine, drying the film, and performing imidization film formation.
8. The preparation method according to claim 1, characterized in that: In step (6), the film passes through the first temperature zone, the second temperature zone, the third temperature zone, the fourth temperature zone, the fifth temperature zone and the sixth temperature zone in the imidization furnace in sequence, and the heating temperatures of each temperature zone are 200~220℃, 250~300℃, 300~350℃, 400~450℃, 500~550℃ and 450~500℃ in sequence, and the heating time of each temperature zone is 10~20s.
9. A polyimide film prepared by the preparation method according to any one of claims 1 to 8.