Double-layer ammonium polyphosphate coated carbon fiber epoxy resin composite material and preparation method thereof

By using double-layer coating technology in carbon fiber epoxy resin composite materials, coating UiO-66-NH2@PUAPP solves the problem of poor flame retardancy and interface compatibility, significantly improves the flame retardant performance and mechanical properties, and is suitable for For applications with high fire safety requirements.

CN118772584AInactive Publication Date: 2024-10-15SHAANXI UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411034022.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The poor flame retardancy of carbon fiber epoxy resin composites and the poor interfacial compatibility between ammonium polyphosphate and epoxy resin limit its application in certain fields.

Method used

Using double-layer coating technology, first use polyurethane shell to coat ammonium polyphosphate to form PUAPP, then coat UiO-66-NH2 on its surface, evenly disperse it into epoxy resin, and prepare UiO-66-NH2@ by solvothermal method PUAPP improves the interfacial compatibility and flame retardant properties of ammonium polyphosphate and epoxy resin.

Benefits of technology

It significantly improves the flame retardant and mechanical properties of carbon fiber epoxy resin composites, reduces gas release, enhances fire resistance, and improves the interface compatibility between ammonium polyphosphate and epoxy resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772584A_ABST
    Figure CN118772584A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon fiber epoxy resin composite material with double layers coated with ammonium polyphosphate and a preparation method, and belongs to the technical field of flame-retardant modification of carbon fiber epoxy resin composites.The flame-retardant microcapsule PUAPP is prepared through an in-situ polymerization method, UiO-66-NH2-coated PUAPP is prepared on the ammonium polyphosphate coated with polyurethane through a solvothermal method, and the UiO-66-NH2-coated PUAPP is prepared. The process is simple, the reaction speed is high, the porous structure and the high surface area of UiO-66-NH2 are suitable for gas adsorption and storage, and gas release is reduced. The transition metal Zr catalyzes and stabilizes the formation of carbon, and inhibits the release of toxic smoke and gas. Organic ligands rich in aromatic rings and carboxyl groups are used as components of the IFR. In addition, amino groups on the organic ligands are beneficial to modification after synthesis of the MOF. After PUAPP is coated with UiO-66-NH2, the defect that ammonium polyphosphate is incompatible with an epoxy resin interface can be further overcome, so that the interface performance and the overall performance of the material are promoted to be improved, and the flame retardant property and the mechanical property of CFEP are synergistically improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardant modification of carbon fiber epoxy resin composite materials, and particularly relates to a carbon fiber epoxy resin composite material coated with double layers of ammonium polyphosphate and a preparation method thereof. Background Art

[0002] Carbon fiber epoxy composites (CFEP) have the advantages of light weight, high strength, high stiffness, corrosion resistance and high design freedom, so they are widely used in automobiles, ships, sporting goods, construction and other industrial fields. Carbon fiber (CF) is used as a reinforcing material in CFEP, thereby improving the mechanical properties of the composite material. Epoxy resin has excellent bonding properties, chemical resistance and high temperature resistance, which can effectively transfer loads and protect carbon fibers. The resin polymer is used as a matrix to bond the fibers to protect them from environmental influences. CFEP has become the preferred material for aerospace equipment because of its integration of structure and manufacturing materials, and the ease of achieving comprehensive performance of large-sized and complex components.

[0003] Epoxy resin and its composite materials can be used as a material with better performance in various aspects because of its high mechanical strength, excellent adhesion, chemical resistance and good electrical insulation, so as to be used as a framework structure in aerospace, automobile, shipbuilding and energy industries. However, due to the high heat released during its combustion process, the large amount of flammable gas and smoke, and the molten dripping during the combustion process, the limiting oxygen index (LOI) is low, only about 20%, and it is a flammable material. It also has defects such as high brittleness and weak resistance to external impact, which limits its application in some fields. Therefore, it is very necessary to develop epoxy resin with flame retardant effect and functionalize epoxy resin with flame retardant. However, some modification methods will affect the viscosity and curing time of epoxy resin, thereby changing the processing conditions of epoxy resin. At present, it is not only necessary to give epoxy resin a flame retardant effect, but also the greater challenge is to develop a flame retardant system that can improve its fire resistance without reducing the mechanical properties of polymer composites.

[0004] Ammonium polyphosphate (APP) is widely used in the field of polymer flame retardancy due to its low cost, low toxicity and good flame retardant effect. Ammonium polyphosphate (APP) is an environmentally friendly flame retardant widely used to improve the flame retardancy of polymers. During the combustion process, APP releases NH3, water and inorganic acids. Inorganic acids can react with hydroxyl groups to form phosphate esters. Coking occurs when the phosphate ester is dehydrated, and then an expanded carbonaceous structure is formed during the release of NH3 and water. The expanded carbonaceous structure serves as a barrier to reduce thermal radiation and isolate pyrolysis products. However, APP has weak water resistance, is easy to absorb moisture, and has poor compatibility with polymers, which limits its application. In addition, during the preparation of the polymer, APP produces a separation layer in the prepolymer, resulting in the destruction of mechanical properties, changes in glass transition temperature and a decrease in flame retardant efficiency. However, the flame retardant efficiency of PUAPP after polyurethane monolayer coating with ammonium polyphosphate is not significant when added to carbon fiber epoxy resin.

[0005] Metal-organic frameworks (MOFs) derived flame retardants have recently emerged as a new class of additives in polymeric materials to reduce fire hazards during applications where high fire safety is required. They are formed by linking metal-containing units with organic linkers, using strong bonds to establish an open crystalline framework with permanent porosity. Due to the porous structure caused by organic ligands, MOFs have large specific surface areas, excellent adsorption properties and other outstanding advantages. The inorganic node-organic linker connection brings out a huge one-dimensional, two-dimensional or three-dimensional network. Summary of the invention

[0006] The purpose of the present invention is to solve the problems in the prior art and to provide a carbon fiber epoxy resin composite material with a double layer of ammonium polyphosphate coated thereon and a preparation method thereof, so as to solve the technical problems in the prior art such as poor flame retardancy of epoxy resin and poor interface compatibility between ammonium polyphosphate and epoxy resin.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A method for preparing a double-layer ammonium polyphosphate-coated carbon fiber epoxy resin composite material, comprising:

[0009] S1: using polyurethane shell to coat ammonium polyphosphate to prepare PUAPP;

[0010] S2: Coating UiO-66-NH2 on PUAPP to prepare UiO-66-NH2@PUAPP;

[0011] S3: The prepared UiO-66-NH2@PUAPP was evenly dispersed into the epoxy resin E-51 system, evenly applied on the carbon fiber cloth, and post-cured to obtain a carbon fiber epoxy resin composite material.

[0012] Preferably, the step S1 specifically includes the following steps:

[0013] S101: dissolving PEG2000 in a polyvinyl alcohol solution to obtain solution A;

[0014] S102: HDI trimer, emulsifier OP-10, ammonium polyphosphate, catalyst dibutyltin dilaurate and solvent dimethyl sulfoxide are mixed and stirred to obtain solution B after being evenly mixed, wherein HDI trimer and polyethylene glycol are prepared into polyurethane, and the core material is ammonium polyphosphate;

[0015] S103: adding solution B dropwise into solution A and mixing them, taking out the emulsion after dispersion and letting it stand to obtain a mixed solution C;

[0016] S104: The mixed solution C is slowly heated to 60° C. in a water bath, reacted for (0.5-1) h, the chain extender 1,4-butanediol is added, the temperature is raised to 80° C., reacted for (4-6) h, cooled to room temperature, and centrifuged to obtain PUAPP.

[0017] Preferably, in S101, the mass fraction of polyvinyl alcohol in the polyvinyl alcohol solution is 1.5%.

[0018] Preferably, the molar ratio of the HDI trimer in S102 to the PEG2000 in S101 is 1.2:1, and the mass ratio of the polyurethane wall material to the ammonium polyphosphate core material is 1:0.5.

[0019] Preferably, the addition of the chain extender 1,4-butanediol in S104 complies with a chain extension coefficient of 0.90.

[0020] Preferably, the step S2 specifically includes the following steps:

[0021] S201: Dissolve zirconium chloride and 2-aminoterephthalic acid in DMF to obtain a mixed solution D.

[0022] S202: dissolving PUAPP in DMF to obtain a mixed solution E;

[0023] S203: adding the mixed solution E dropwise into the mixed solution D, and then adding glacial acetic acid and deionized water to obtain a mixed solution F;

[0024] S204: Mixed solution F is heated to 100°C to 130°C for 3 to 6 hours, cooled to room temperature, and the supernatant is poured out, washed, and dried to obtain UiO-66-NH 2 @PUAPP.

[0025] Preferably, the usage ratio of zirconium chloride, 2-aminoterephthalic acid and DMF in S201 is (2-6) mmol: (2-6) mmol: (30-90) mL.

[0026] Preferably, the usage ratio of zirconium chloride, glacial acetic acid and deionized water in S203 is (2-6) mmol: (14-39) mL: (2.33-7.02) mL.

[0027] Preferably, the S3 specifically includes:

[0028] S301: Take UiO-66-NH2@PUAPP and evenly disperse it into the epoxy resin system. Stir the mixture in a water bath at 60°C for 2h, then add curing agent H256. The mass ratio of epoxy resin system to curing agent is 100:32. Then heat it in a water bath to make it flow and evenly apply it on the carbon fiber cloth.

[0029] S302: Place the coated carbon cloth into a mold preheated at 90° C., and place the mold in a hot press for curing to obtain a UiO-66-NH2@PUAPP / CF / EP composite material.

[0030] The present application also discloses a double-layer ammonium polyphosphate-coated carbon fiber epoxy resin composite material, which is prepared by any of the preparation methods described above.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The invention discloses a method for preparing a double-layer ammonium polyphosphate coated carbon fiber epoxy resin composite material, wherein the flame-retardant microcapsule PUAPP is prepared by an in-situ polymerization method, and UiO-66-NH 2 @PUAPP, its process is relatively simple and the reaction speed is relatively fast, among which UiO-66-NH 2 The porous structure and high surface area of ​​MOF are suitable for gas adsorption and storage, reducing gas release. The transition metal Zr has high catalytic activity and can catalyze the formation of stable carbon, inhibiting the release of toxic fumes and gases. The organic ligand rich in aromatic rings and carboxyl groups (2-aminoterephthalic acid) is also a good carbonizing agent and can be used as a component of IFR. In addition, the amino groups on the organic ligands are conducive to post-synthetic modification of MOF. Typically, UiO-66-NH 2 It is an ideal flame retardant that improves both flame retardancy and smoke suppression performance. 2 After coating with PUAPP, the incompatibility between ammonium polyphosphate and epoxy resin interfaces can be further improved, thereby promoting the improvement of interface performance and overall material performance, and synergistically improving the flame retardant properties and mechanical properties of CFEP. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0034] Figure 1 Infrared spectra; (a) is UiO-66-NH 2 IR spectra of PUAPP and UiO-66-NH 2 Infrared spectrum of @PUAPP;

[0035] Figure 2 It is the XRD analysis spectrum;

[0036] Figure 3 The scanning SEM images are shown in Figure 1. (a) is a scanning image of PUAPP, and (b) is a scanning image of UiO-66-NH 2 Scanning image of PUAPP coated;

[0037] Figure 4 The flame retardant performance test results of carbon fiber epoxy resin composites before and after adding double-layer coated ammonium polyphosphate, where (a) is the maximum heat release rate (PHRR) diagram; (b) is the maximum total heat release (THR) diagram; (c) is the fire performance index (FPI) and fire growth index (FGI) diagram. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0039] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0041] In the description of the embodiments of the present invention, it should be noted that if the terms "upper", "lower", "horizontal", "inner", etc. indicate an orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the invention is usually placed when in use, it is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.

[0042] In addition, if the term "horizontal" appears, it does not mean that the component is required to be absolutely horizontal, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", which does not mean that the structure must be completely horizontal, but can be slightly tilted.

[0043] In the description of the embodiments of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0044] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0045] The invention discloses a method for preparing a double-layer ammonium polyphosphate coated carbon fiber epoxy resin composite material, comprising:

[0046] S1: using polyurethane shell to coat ammonium polyphosphate to prepare PUAPP;

[0047] S2: UiO-66-NH2 was coated on PUAPP to prepare UiO-66-NH 2 @PUAPP;

[0048] S3: Prepared UiO-66-NH 2 @PUAPP is evenly dispersed in the epoxy resin E-51 system, evenly applied on the carbon fiber cloth, and then cured to obtain a carbon fiber epoxy resin composite material.

[0049] Preparation of UiO-66-NH by solvothermal method 2 Coating PUAPP has a simple process and a fast reaction speed. 2The porous structure and high surface area of ​​MOF are suitable for gas adsorption and storage, reducing gas release. The transition metal Zr has high catalytic activity and can catalyze the formation of stable carbon, inhibiting the release of toxic fumes and gases. The organic ligand rich in aromatic rings and carboxyl groups (2-aminoterephthalic acid) is also a good carbonizing agent and can be used as a component of IFR. In addition, the amino groups on the organic ligands are conducive to post-synthetic modification of MOF. Typically, UiO-66-NH 2 It is an ideal flame retardant that improves both flame retardancy and smoke suppression performance. 2 After coating with PUAPP, the incompatibility between ammonium polyphosphate and epoxy resin interfaces can be further improved, thereby promoting the improvement of interface performance and overall material performance, and synergistically improving the flame retardant properties and mechanical properties of CFEP.

[0050] In some embodiments, the S1 specifically includes the following steps:

[0051] S101: dissolving PEG2000 in a polyvinyl alcohol solution to obtain solution A;

[0052] S102: HDI trimer, emulsifier OP-10, ammonium polyphosphate, catalyst dibutyltin dilaurate and solvent dimethyl sulfoxide are mixed and stirred to obtain solution B after being evenly mixed, wherein HDI trimer and polyethylene glycol are prepared into polyurethane, and the core material is ammonium polyphosphate;

[0053] S103: adding solution B dropwise into solution A and mixing them, dispersing them in a homogenizer at a speed of (8000-10000) r / min for (10-30) min, taking out the emulsion and letting it stand for 20 min, and then adding it to a 250 mL three-necked flask to obtain a mixed solution C;

[0054] S104: The mixed solution C is slowly heated to 60° C. in a water bath, reacted for (0.5-1) h, the chain extender 1,4-butanediol is added, the temperature is raised to 80° C., reacted for (4-6) h, cooled to room temperature, and centrifuged to obtain PUAPP.

[0055] Further preferably, in S101, the mass fraction of polyvinyl alcohol in the polyvinyl alcohol solution is 1.5%.

[0056] Further preferably, the molar ratio of the HDI trimer in S102 to the PEG2000 in S101 is 1.2:1, and the mass ratio of the polyurethane wall material to the ammonium polyphosphate core material is 1:0.5.

[0057] In some embodiments, the addition of the chain extender 1,4-butanediol in S104 complies with a chain extension coefficient of 0.90.

[0058] In some embodiments, the step S2 specifically includes the following steps:

[0059] S201: Dissolve zirconium chloride and 2-aminoterephthalic acid in DMF to obtain a mixed solution D.

[0060] S202: dissolving PUAPP in DMF to obtain a mixed solution E;

[0061] S203: adding the mixed solution E dropwise into the mixed solution D, and then adding glacial acetic acid and deionized water to obtain a mixed solution F;

[0062] S204: Mixed solution F is heated to 100°C to 130°C for 3 to 6 hours, cooled to room temperature, and the supernatant is poured out, washed, and dried to obtain UiO-66-NH 2 @PUAPP.

[0063] Further preferably, the usage ratio of zirconium chloride, 2-aminoterephthalic acid and DMF in S201 is (2-6) mmol: (2-6) mmol: (30-90) mL.

[0064] Further preferably, the usage ratio of zirconium chloride, glacial acetic acid and deionized water in S203 is (2-6) mmol: (14-39) mL: (2.33-7.02) mL.

[0065] In some embodiments, the S3 specifically includes:

[0066] S301: Take UiO-66-NH 2 @PUAPP is evenly dispersed in the epoxy resin system, and the mixture is stirred in a water bath at 60°C for 2 hours. Then, curing agent H256 is added. The mass ratio of epoxy resin system to curing agent is 100:32. Then, it is heated in a water bath to make it flowable and evenly applied on the carbon fiber cloth.

[0067] S302: Place the coated carbon cloth into a mold preheated at 90°C, and place the mold in a hot press to cure, thereby obtaining UiO-66-NH 2 @PUAPP / CF / EP composite material.

[0068] Preferably, the curing is performed in three stages, i.e., keeping the temperature at 90°C and normal pressure for 2 hours, then pressurizing to 5 MPa, then heating to 120°C and keeping the temperature for 2 hours, and in the third stage keeping the temperature at 150°C for 3 hours.

[0069] A carbon fiber epoxy resin composite material coated with double layers of ammonium polyphosphate is prepared by any one of the above-mentioned preparation methods.

[0070] In some embodiments, a method for preparing a double-layer ammonium polyphosphate-coated carbon fiber epoxy resin composite material comprises:

[0071] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.

[0072] (2) PUAPP was prepared by in situ polymerization.

[0073] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.25 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker, and magnetic stirring was performed for 30 minutes to obtain solution B after mixing evenly; then solution B was added dropwise to solution A and mixed, and dispersed in a homogenizer at a speed of 10000 r / min for 15 minutes, and the emulsion was taken out and allowed to stand for 20 minutes and then added to a 250 mL three-necked flask to obtain a mixed solution C;

[0074] Finally, the mixed solution C was slowly heated to 60°C in a water bath, reacted for 0.5h, 112μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80°C and maintained for 4h, cooled to room temperature, centrifuged to obtain PUAPP, and dried in a vacuum oven at 60°C for 24-48h.

[0075] (3)UiO-66-NH 2 @PUAPP was prepared by solvothermal method

[0076] First, 4.29mmol zirconium chloride and 4.29mmol 2-aminoterephthalic acid were dissolved in 66.7mL DMF, recorded as solution A; then 1g PUAPP was weighed and dispersed in 30mL DMF, recorded as solution B; solution B was added dropwise to solution A, recorded as mixed solution C. Finally, 29.41mL glacial acetic acid and 5mL deionized water were added to the mixed solution C, and the mixture was heated and stirred in an oil bath for 4h. After the reaction was completed, the mixture was cooled to room temperature, the supernatant was poured out, washed and dried to obtain UiO-66-NH 2 @PUAPP.

[0077] (4) UiO-66-NH 2 Preparation of PUAPP / CF / EP composites

[0078] Weigh UiO-66-NH 2@PUAPP is evenly dispersed in the epoxy resin system, and the mixture is stirred in a water bath at 60°C for 2h, and then the curing agent H256 is added to ensure that the mass ratio of resin and curing agent reaches 100:32, and then heated in a water bath to make it flow and evenly spread on a 10cm×10cm carbon fiber cloth, and then the sample is placed in a mold preheated at 90°C, and the mold is placed in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90°C normal pressure is kept for 2h, then pressurized to 5MPa, and then heated to 120°C and kept for 2h. In the third stage, the temperature is kept at 150°C for 3h. The mold is demoulded after cooling to room temperature, and the resulting composite material is UiO-66-NH 2 @PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut into appropriate sizes for testing.

[0079] This application starts from the perspective of flame retardant modification of carbon fiber epoxy resin composite materials. First, polyurethane is used to coat ammonium polyphosphate to form PUAPP, and then UiO-66-NH 2 Coating the surface of PUAPP to improve the morphology and flame retardant properties of PUAPP, thereby introducing UiO-66-NH 2 @PUAPP, in order to study the changing law of the flame retardant properties of composite materials. At the same time, SEM, FTIR, XRD, cone calorimetry and other performance tests were used to test the UiO-66-NH 2 @PUAPP surface microstructure and surface chemical properties. 2 The effect of adding @PUAPP on the flame retardant properties of carbon fiber epoxy resin composites is shown in the following examples:

[0080] Example 1

[0081] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.

[0082] (2) PUAPP was prepared by in situ polymerization.

[0083] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.25 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker and magnetically stirred for 30 min to obtain solution B after mixing evenly; then solution B was added dropwise to solution A. The mixture was mixed and dispersed in a homogenizer at a speed of 10000 r / min for 15 min. The emulsion was taken out and allowed to stand for 20 min, then added into a 250 mL three-necked flask to obtain a mixed solution C. Finally, the mixed solution C was slowly heated to 60°C in a water bath, reacted for 0.5 h, 112 μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80°C and maintained for 4 h, and after cooling to room temperature, PUAPP was obtained by centrifugation and dried in a vacuum oven at 60°C for 24 to 48 h.

[0084] (3)UiO-66-NH 2 @PUAPP was prepared by solvothermal method

[0085] First, 2mmol zirconium chloride and 2mmol 2-aminoterephthalic acid were dissolved in 30mL DMF, recorded as solution A; then 1g PUAPP was weighed and dispersed in 30mL DMF, recorded as solution B; solution B was added dropwise to solution A, recorded as mixed solution C. Finally, 14mL glacial acetic acid and 2.33mL deionized water were added to the mixed solution C, and the mixture was heated and stirred in an oil bath for 4h. After the reaction was completed, the mixture was cooled to room temperature, the supernatant was poured out, washed and dried to obtain UiO-66-NH 2 @PUAPP.

[0086] (4)UiO-66-NH 2 Preparation of PUAPP / CF / EP composites

[0087] Weigh UiO-66-NH 2 @PUAPP is evenly dispersed in the epoxy resin system, and the mixture is stirred in a water bath at 60°C for 2h, and then the curing agent H256 is added to ensure that the mass ratio of resin and curing agent reaches 100:32, and then heated in a water bath to make it flow and evenly spread on a 10cm×10cm carbon fiber cloth, and then the sample is placed in a mold preheated at 90°C, and the mold is placed in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90°C normal pressure is kept for 2h, then pressurized to 5MPa, and then heated to 120°C and kept for 2h. In the third stage, the temperature is kept at 150°C for 3h. The mold is demoulded after cooling to room temperature, and the resulting composite material is UiO-66-NH 2@PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut into appropriate sizes for testing.

[0088] Example 2

[0089] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.

[0090] (2) PUAPP was prepared by in situ polymerization.

[0091] The specific operations are as follows:

[0092] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.3 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker and magnetically stirred for 30 min to obtain solution B after mixing evenly; then solution B was added dropwise to solution A. The mixture was mixed and dispersed in a homogenizer at a speed of 10000 r / min for 15 min. The emulsion was taken out and allowed to stand for 20 min, then added into a 250 mL three-necked flask to obtain a mixed solution C. Finally, the mixed solution C was slowly heated to 60° C. in a water bath, reacted for 0.5 h, 112 μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80° C. and maintained for 4 h. After cooling to room temperature, PUAPP was obtained by centrifugation and dried in a vacuum oven at 60° C. for 24 to 48 h.

[0093] (3)UiO-66-NH 2 @PUAPP was prepared by solvothermal method

[0094] First, 4.29mmol zirconium chloride and 4.29mmol 2-aminoterephthalic acid were dissolved in 66.7mL DMF, recorded as solution D; then 1g PUAPP was weighed and dispersed in 30mL DMF, recorded as solution E; solution E was added dropwise to solution D, recorded as mixed solution F. Finally, 29.41mL glacial acetic acid and 5mL deionized water were added to the mixed solution F, and the mixture was heated and stirred in an oil bath for 4h. After the reaction was completed, the mixture was cooled to room temperature, the supernatant was poured out, washed and dried, and UiO-66-NH 2 @PUAPP.

[0095] (4) UiO-66-NH 2Preparation of PUAPP / CF / EP composites

[0096] Weigh UiO-66-NH 2 @PUAPP is evenly dispersed in the epoxy resin system, and the mixture is stirred in a water bath at 60°C for 2h, and then the curing agent H256 is added to ensure that the mass ratio of resin and curing agent reaches 100:32, and then heated in a water bath to make it flow and evenly spread on a 10cm×10cm carbon fiber cloth, and then the sample is placed in a mold preheated at 90°C, and the mold is placed in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90°C normal pressure is kept for 2h, then pressurized to 5MPa, and then heated to 120°C and kept for 2h. In the third stage, the temperature is kept at 150°C for 3h. The mold is demoulded after cooling to room temperature, and the resulting composite material is UiO-66-NH 2 @PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut into appropriate sizes for testing.

[0097] Example 3

[0098] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.

[0099] (2) PUAPP was prepared by in situ polymerization.

[0100] The specific operations are as follows:

[0101] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.3 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker and magnetically stirred for 30 min to obtain solution B after mixing evenly; then solution B was added dropwise to solution A. The mixture was mixed and dispersed in a homogenizer at a speed of 10000 r / min for 15 min. The emulsion was taken out and allowed to stand for 20 min, then added into a 250 mL three-necked flask to obtain a mixed solution C. Finally, the mixed solution C was slowly heated to 60° C. in a water bath, reacted for 0.5 h, 112 μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80° C. and maintained for 4 h. After cooling to room temperature, PUAPP was obtained by centrifugation and dried in a vacuum oven at 60° C. for 24 to 48 h.

[0102] (3)UiO-66-NH 2 @PUAPP was prepared by solvothermal method

[0103] First, 6mmol zirconium chloride and 6mmol 2-aminoterephthalic acid were dissolved in 90mL DMF, recorded as solution D; then 0.5g PUAPP was weighed and dispersed in 30mL DMF, recorded as solution E; solution E was added dropwise to solution D, recorded as mixed solution F. Finally, 39mL glacial acetic acid and 7.02mL deionized water were added to the mixed solution F, and the mixture was heated and stirred in an oil bath for 4h. After the reaction was completed, the mixture was cooled to room temperature, the supernatant was poured out, washed and dried, and UiO-66-NH 2 @PUAPP.

[0104] (4)UiO-66-NH 2 Preparation of PUAPP / CF / EP composites

[0105] Weigh UiO-66-NH 2 @PUAPP is evenly dispersed in the epoxy resin system, and the mixture is stirred in a water bath at 60°C for 2h, and then the curing agent H256 is added to ensure that the mass ratio of resin and curing agent reaches 100:32, and then heated in a water bath to make it flow and evenly spread on a 10cm×10cm carbon fiber cloth, and then the sample is placed in a mold preheated at 90°C, and the mold is placed in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90°C normal pressure is kept for 2h, then pressurized to 5MPa, and then heated to 120°C and kept for 2h. In the third stage, the temperature is kept at 150°C for 3h. The mold is demoulded after cooling to room temperature, and the resulting composite material is UiO-66-NH 2 @PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut into appropriate sizes for testing.

[0106] Example 4

[0107] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.

[0108] (2) PUAPP was prepared by in situ polymerization.

[0109] The specific operations are as follows:

[0110] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.3 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker and magnetically stirred for 30 min to obtain solution B after mixing evenly; then solution B was added dropwise to solution A. The mixture was mixed and dispersed in a homogenizer at a speed of 10000 r / min for 15 min. The emulsion was taken out and allowed to stand for 20 min, then added into a 250 mL three-necked flask to obtain a mixed solution C. Finally, the mixed solution C was slowly heated to 60° C. in a water bath, reacted for 0.5 h, 112 μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80° C. and maintained for 4 h. After cooling to room temperature, PUAPP was obtained by centrifugation and dried in a vacuum oven at 60° C. for 24 to 48 h.

[0111] (3)UiO-66-NH 2 @PUAPP was prepared by solvothermal method

[0112] First, 4.29mmol zirconium chloride and 4.29mmol 2-aminoterephthalic acid were dissolved in 66.7mL DMF, recorded as solution D; then 1g PUAPP was weighed and dispersed in 30mL DMF, recorded as solution E; solution E was added dropwise to solution D, recorded as mixed solution F. Finally, 29.41mL glacial acetic acid and 5mL deionized water were added to the mixed solution F, and the mixture was heated and stirred in an oil bath for 4h. After the reaction was completed, the mixture was cooled to room temperature, the supernatant was poured out, washed and dried, and UiO-66-NH 2 @PUAPP.

[0113] (4)UiO-66-NH 2 Preparation of PUAPP / CF / EP composites

[0114] Weigh UiO-66-NH 2 @PUAPP is evenly dispersed in the epoxy resin system, and the mixture is stirred in a water bath at 60°C for 2h, and then the curing agent H256 is added to ensure that the mass ratio of resin and curing agent reaches 100:32, and then heated in a water bath to make it flow and evenly spread on a 10cm×10cm carbon fiber cloth, and then the sample is placed in a mold preheated at 90°C, and the mold is placed in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90°C normal pressure is kept for 2h, then pressurized to 5MPa, and then heated to 120°C and kept for 2h. In the third stage, the temperature is kept at 150°C for 3h. The mold is demoulded after cooling to room temperature, and the resulting composite material is UiO-66-NH 2@PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut into appropriate sizes for testing.

[0115] Example 5

[0116] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.

[0117] (2) PUAPP was prepared by in situ polymerization.

[0118] The specific operations are as follows:

[0119] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.3 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker and magnetically stirred for 30 min to obtain solution B after mixing evenly; then solution B was added dropwise to solution A. The mixture was mixed and dispersed in a homogenizer at a speed of 10000 r / min for 15 min. The emulsion was taken out and allowed to stand for 20 min, then added into a 250 mL three-necked flask to obtain a mixed solution C. Finally, the mixed solution C was slowly heated to 60° C. in a water bath, reacted for 0.5 h, 112 μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80° C. and maintained for 4 h. After cooling to room temperature, PUAPP was obtained by centrifugation and dried in a vacuum oven at 60° C. for 24 to 48 h.

[0120] (3)UiO-66-NH 2 @PUAPP was prepared by solvothermal method

[0121] First, 4.29mmol zirconium chloride and 4.29mmol 2-aminoterephthalic acid were dissolved in 66.7mL DMF, recorded as solution D; then 1.5g PUAPP was weighed and dispersed in 30mL DMF, recorded as solution E; solution E was added dropwise to solution D, recorded as mixed solution F. Finally, 29.41mL glacial acetic acid and 5mL deionized water were added to the mixed solution F, and the mixture was heated and stirred in an oil bath for 4h. After the reaction was completed, the mixture was cooled to room temperature, the supernatant was poured out, washed and dried, and UiO-66-NH 2 @PUAPP.

[0122] (4) UiO-66-NH 2Preparation of PUAPP / CF / EP composites

[0123] Weigh UiO-66-NH 2 @PUAPP is evenly dispersed in the epoxy resin system, and the mixture is stirred in a water bath at 60°C for 2h, and then the curing agent H256 is added to ensure that the mass ratio of resin and curing agent reaches 100:32, and then heated in a water bath to make it flow and evenly spread on a 10cm×10cm carbon fiber cloth, and then the sample is placed in a mold preheated at 90°C, and the mold is placed in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90°C normal pressure is kept for 2h, then pressurized to 5MPa, and then heated to 120°C and kept for 2h. In the third stage, the temperature is kept at 150°C for 3h. The mold is demoulded after cooling to room temperature, and the resulting composite material is UiO-66-NH 2 @PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut into appropriate sizes for testing.

[0124] Example 6

[0125] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.

[0126] (2) PUAPP was prepared by in situ polymerization.

[0127] The specific operations are as follows:

[0128] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.3 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker and magnetically stirred for 30 min to obtain solution B after mixing evenly; then solution B was added dropwise to solution A. The mixture was mixed and dispersed in a homogenizer at a speed of 10000 r / min for 15 min. The emulsion was taken out and allowed to stand for 20 min, then added into a 250 mL three-necked flask to obtain a mixed solution C. Finally, the mixed solution C was slowly heated to 60° C. in a water bath, reacted for 0.5 h, 112 μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80° C. and maintained for 4 h. After cooling to room temperature, PUAPP was obtained by centrifugation and dried in a vacuum oven at 60° C. for 24 to 48 h.

[0129] (3)UiO-66-NH 2 @PUAPP was prepared by solvothermal method

[0130] First, 4.29mmol zirconium chloride and 4.29mmol 2-aminoterephthalic acid were dissolved in 66.7mL DMF, recorded as solution A; then 2g PUAPP was weighed and dispersed in 30mL DMF, recorded as solution B; solution B was added dropwise to solution A, recorded as mixed solution C. Finally, 29.41mL glacial acetic acid and 5mL deionized water were added to the mixed solution C, and the mixture was heated and stirred in an oil bath for 4h. After the reaction was completed, the mixture was cooled to room temperature, the supernatant was poured out, washed and dried, and UiO-66-NH 2 @PUAPP.

[0131] (4) UiO-66-NH 2 Preparation of PUAPP / CF / EP composites

[0132] Weigh UiO-66-NH 2 @PUAPP is evenly dispersed in the epoxy resin system, and the mixture is stirred in a water bath at 60°C for 2h, and then the curing agent H256 is added to ensure that the mass ratio of resin and curing agent reaches 100:32, and then heated in a water bath to make it flow and evenly spread on a 10cm×10cm carbon fiber cloth, and then the sample is placed in a mold preheated at 90°C, and the mold is placed in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90°C normal pressure is kept for 2h, then pressurized to 5MPa, and then heated to 120°C and kept for 2h. In the third stage, the temperature is kept at 150°C for 3h. The mold is demoulded after cooling to room temperature, and the resulting composite material is UiO-66-NH 2 @PUAPP / CF / EP composite material. According to the test requirements, the obtained samples are cut into appropriate sizes for testing.

[0133] In order to characterize the morphological features, the target product was tested by Fourier transform infrared spectroscopy (FTIR), see Figure 1 , at UiO-66-NH 2 In the infrared spectrum, 3460-3350cm -1 It is the stretching vibration of -OH and -NH 2 The cooperative absorption band between the symmetric and asymmetric vibrations of the group is 1659 cm -1 Yes-NH 2 Deformation vibration peak, 1606-1485cm -1 The intervening band is attributed to aromatic CC ring vibration, 658 cm -1 The symmetric and asymmetric stretching vibration peaks of Zr-(OC) are located at the bottom.2 The successful synthesis of UiO-66-NH 2 In the infrared spectrum of @PUAPP, at 3540-3162cm -1 The stretching vibration of -OH and -NH 2 The cooperative absorption bands between the symmetric and asymmetric vibrations of the group are at 1257, 1020 and 881 cm -1 The PO absorption peak of ammonium polyphosphate, the symmetric vibration peaks of PO2 and PO3, and the asymmetric stretching vibration peak of PO appeared at 669cm -1 The Zr-(OC) symmetric vibration peak appeared, which preliminarily proved that UiO-66-NH 2 Successful synthesis of @PUAPP.

[0134] In order to verify the crystal structure characteristics of the material, the product was tested by X-ray powder diffraction (XRD). Figure 2 UiO-66-NH 2 XRD spectra of @PUAPP, PUAPP and APP, UiO-66-NH 2 In the XRD pattern of @PUAPP, the diffraction peak at 7.4° corresponds to the crystal plane (111), and the diffraction peak at 8.5° corresponds to the crystal plane (002), which is consistent with the previously reported literature, proving that UiO66-NH 2 The crystal structure of UiO-66-NH is synthesized without impurities. The (200) and (110) crystal planes of APP appear at 14.6° and 15.4°. It can be seen from XRD that the 2 After coating, the lattice growth of APP was inhibited, but the diffraction peak still appeared, proving that the use of UiO-66-NH 2 After coating, the performance of ammonium polyphosphate itself will not be affected.

[0135] Figure 3 UiO-66-NH 2 @PUAPP Scanning diagram before and after coating. You can see a lot of UiO-66-NH on PUAPP 2 Nanoparticles were loaded on its surface, proving that the coating was successful.

[0136] Figure 4 The flame retardant performance test. (a) is the maximum heat release rate (PHRR) graph; (b) is the maximum total heat release (THR) graph; (c) is the fire performance index (FPI) and fire growth index (FGI) bar graph. It can be observed from the figure that the carbon fiber epoxy composite material without any flame retardant has the highest maximum heat release rate (PHRR) and maximum total heat release (THR), and the addition of UiO-66-NH 2After @PUAPP, its PHRR decreased by 53.2% and THR decreased by 22.25%. In addition, FPI also showed an upward trend, while FGI showed a downward trend, proving that its fire hazard was greatly reduced and the flame retardant performance was improved.

[0137] Table 3-1 CONE test results of composites

[0138]

[0139] Referring to Table 3-1, the present invention enhances the interfacial compatibility between epoxy resin and ammonium polyphosphate without sacrificing the original performance of ammonium polyphosphate, and improves the flame retardant properties of carbon fiber epoxy composite materials. First, a flame retardant microcapsule with polyurethane as shell material and ammonium polyphosphate as core material is prepared, and then UiO-66-NH 2 Coated on the surface of PUAPP, added into carbon fiber epoxy resin composite material. 2 @PUAPP changes in morphology, thermal stability and flame retardancy when applied to carbon fiber epoxy matrix. 2 After coating, the poor water resistance of APP was changed, the compatibility with epoxy resin matrix was improved, and UiO-66-NH 2 (Zr) can absorb a large amount of gas, reduce the release of smoke and combustible gas, and in UiO-66-NH 2 Before the (Zr) structure collapses, its porous structure and high specific surface area provide reaction space for active pyrolysis products and complicate the transport path. 2 After the (Zr) structure collapses, ZrO 2 It catalyzes the formation of a protective carbon layer in the condensation matrix to achieve a synergistic flame retardant effect. It builds a bridge between the APP and epoxy resin matrix to significantly improve the flame retardancy of carbon fiber epoxy resin composites.

[0140] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a double-layer ammonium polyphosphate coated carbon fiber epoxy resin composite material, characterized in that: include: S1: using polyurethane shell to coat ammonium polyphosphate to prepare PUAPP; S2: Coating UiO-66-NH2 on PUAPP to prepare UiO-66-NH2@PUAPP; S3: The prepared UiO-66-NH2@PUAPP was evenly dispersed into the epoxy resin E-51 system, evenly applied on the carbon fiber cloth, and post-cured to obtain a carbon fiber epoxy resin composite material.

2. The method for preparing a double-layer ammonium polyphosphate-coated carbon fiber epoxy resin composite material according to claim 1, characterized in that: The S1 specifically includes the following steps: S101: dissolving PEG2000 in a polyvinyl alcohol solution to obtain solution A; S102: HDI trimer, emulsifier OP-10, ammonium polyphosphate, catalyst dibutyltin dilaurate and solvent dimethyl sulfoxide are mixed and stirred to obtain solution B after being evenly mixed, wherein HDI trimer and polyethylene glycol are prepared into polyurethane, and the core material is ammonium polyphosphate; S103: adding solution B dropwise into solution A and mixing them, taking out the emulsion after dispersion and letting it stand to obtain a mixed solution C; S104: The mixed solution C is slowly heated to 60° C. in a water bath, reacted for (0.5-1) h, the chain extender 1,4-butanediol is added, the temperature is raised to 80° C., reacted for (4-6) h, cooled to room temperature, and centrifuged to obtain PUAPP.

3. The method for preparing a double-layer ammonium polyphosphate-coated carbon fiber epoxy resin composite material according to claim 2, characterized in that: In the S101, the mass fraction of polyvinyl alcohol in the polyvinyl alcohol solution is 1.5%.

4. The method for preparing a double-layer ammonium polyphosphate coated carbon fiber epoxy resin composite material according to claim 2, characterized in that: The molar ratio of HDI trimer in S102 and PEG2000 in S101 is 1.2:1, and the mass ratio of polyurethane wall material and ammonium polyphosphate core material is 1:0.

5.

5. The method for preparing a double-layer ammonium polyphosphate coated carbon fiber epoxy resin composite material according to claim 2, characterized in that: The addition of chain extender 1,4-butanediol in S104 complies with the chain extension coefficient of 0.

90.

6. The method for preparing a double-layer ammonium polyphosphate coated carbon fiber epoxy resin composite material according to claim 1, characterized in that: The S2 specifically includes the following steps: S201: Dissolve zirconium chloride and 2-aminoterephthalic acid in DMF to obtain a mixed solution D. S202: dissolving PUAPP in DMF to obtain a mixed solution E; S203: adding the mixed solution E dropwise into the mixed solution D, and then adding glacial acetic acid and deionized water to obtain a mixed solution F; S204: The mixed solution F is heated to 100° C. to 130° C. for reaction for 3 to 6 hours. After cooling to room temperature, the supernatant is poured out, washed, and dried to obtain UiO-66-NH2@PUAPP.

7. The method for preparing a double-layer ammonium polyphosphate coated carbon fiber epoxy resin composite material according to claim 6, characterized in that: The usage ratio of zirconium chloride, 2-aminoterephthalic acid and DMF in the S201 is (2-6) mmol: (2-6) mmol: (30-90) mL.

8. The method for preparing a double-layer ammonium polyphosphate coated carbon fiber epoxy resin composite material according to claim 6, characterized in that: The dosage ratio of zirconium chloride, glacial acetic acid and deionized water in the S203 is (2-6) mmol: (14-39) mL: (2.33-7.02) mL.

9. The method for preparing a double-layer ammonium polyphosphate coated carbon fiber epoxy resin composite material according to claim 1, characterized in that: The S3 specifically includes: S301: Take UiO-66-NH2@PUAPP and evenly disperse it into the epoxy resin system. Stir the mixture in a water bath at 60°C for 2h, then add curing agent H256. The mass ratio of epoxy resin system to curing agent is 100:

32. Then heat it in a water bath to make it flow and evenly apply it on the carbon fiber cloth. S302: Place the coated carbon cloth into a mold preheated at 90° C., and place the mold in a hot press for curing to obtain a UiO-66-NH2@PUAPP / CF / EP composite material.

10. A carbon fiber epoxy resin composite material coated with double layers of ammonium polyphosphate, characterized in that: The method is prepared by any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for preparing microencapsulated ammonium polyphosphate

    CN101362836A

  • Halogen-free flame retardant in-situ modified solvent-free polyurethane resin film with core-shell structure and preparation method thereof

    CN114058051A

  • Surface-modified carbon fiber, modification method and epoxy composite material thereof

    CN116641227A

  • Carbon fiber multi-scale reinforcement, preparation method and epoxy composite material thereof

    CN116876224A