Alkane diurea nucleating agent modified furyl polyester composition and preparation method thereof

By introducing an alkane diurea nucleating agent into furan-based polyester and utilizing its rigid structure and methylene structure, the problems of insufficient crystallization and barrier properties of furan-based polyester are solved, and the thermal stability and barrier properties of the material are achieved. Performance improvements.

CN118772591APending Publication Date: 2024-10-15YINGKOU KANGHUI PETROCHEM +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410770219.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the crystallization process of furan-based polyester, chain segment movement is hindered, resulting in failure to improve barrier properties, and inorganic nucleating agents lead to poor system compatibility and prone to agglomeration.

Method used

The furan-based polyester composition modified with an alkane diurea nucleating agent is used to introduce a rigid structure and a methylene structure to increase the crystallization temperature and heterogeneous nucleation effect, and improve the crystallization performance and barrier properties of the furan-based polyester.

Benefits of technology

Through the use of alkane biurea nucleating agents, the thermal stability and crystallization properties of furan-based polyester are improved, thereby improving its barrier properties, complying with the processing conditions of polyester materials, and simplifying the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772591A_ABST
    Figure CN118772591A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of biomass furyl polyester, and particularly relates to an alkane diurea nucleating agent modified furyl polyester composition and a preparation method thereof. The composition comprises the following components in parts by mass: 100 parts of furyl polyester and 1-5 parts of an alkane diurea nucleating agent. Wherein the alkane diurea nucleating agent contains a rigid cyclic structure and has excellent thermal stability; the symmetrical structure is easier to crystallize, so that the barrier property and the crystallization property of the furyl polyester are improved. The preparation method of the nucleating agent is simple, the product yield is high, harmful gas is not generated, and the nucleating agent is green and environment-friendly. By introducing a rigid structure into the nucleating agent, the alkane diurea nucleating agent is endowed with good thermal stability and relatively high crystallization temperature, so that a good heterogeneous nucleation effect is exerted, the high barrier property of a furyl polyester material is effectively improved, the melting point of the composition is increased, the application range of the furyl polyester composition is expanded, and the application prospect is broad. The market prospect is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomass furan-based polyesters, and in particular relates to a furan-based polyester composition modified by an alkane diurea nucleating agent and a preparation method thereof. Background Art

[0002] The development of bio-based materials from biomass sources has gradually received widespread attention. 5-Hydroxymethylfurfural is a biomass raw material that can be extracted from natural plants. After further preparation, it can be converted into furan dicarboxylic acid monomers. The furan-based polyesters prepared from this monomer have developed rapidly in recent years, among which the more typical ones are furan-based homopolymers and furan-based copolymers. Due to the presence of rigid ring structures in furan-based polyesters, its structure is difficult to reverse, making furan-based polyesters have both high mechanical strength and low barrier coefficients. Therefore, furan-based polyesters are hailed as ideal substitutes for petroleum-based benzene ring series polyesters. However, due to the low molecular symmetry and strong rigidity of the monomer 2,5-furan dicarboxylic acid, as well as the large intermolecular dipole effect, the movement of the chain segments of furan-based polyesters during the crystallization process is hindered, the crystallization rate is slow, and the barrier properties cannot be further improved.

[0003] The invention patent with publication number CN107118521 A discloses the use of inorganic fillers to study the nucleation of polyfuran dicarboxylic acid; the nucleating agent used is one or more of talc, sodium carbonate, silica, isosorbide, sodium benzoate, N,N-ethylene bislauramide and ionic polymer of ethylene-methacrylic acid. Inorganic nucleating agents and high addition amounts of nucleating agents make the system less compatible and prone to agglomeration, and the barrier properties of the system are studied. Therefore, developing a new process to change the current situation of poor barrier properties and slow crystallization rate of furan-based polyester is a technical problem that needs to be solved urgently. Summary of the invention

[0004] In view of the above technical problems, the present invention provides a furan-based polyester composition modified by an alkane diurea nucleating agent and a preparation method thereof. The preparation method has a simple process and low cost, and can simultaneously improve the crystallization performance and barrier performance of the furan-based polyester.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] In a first aspect, the present invention provides a furan-based polyester composition modified with an alkane diurea nucleating agent, which comprises, by weight, 100 parts of furan-based polyester and 1-5 parts of an alkane diurea nucleating agent.

[0007] The furan-based polyester is selected from polyethylene furandicarboxylate, polypropylene furandicarboxylate, polybutylene furandicarboxylate, polypentane furandicarboxylate, polyhexane furandicarboxylate, polyoctane furandicarboxylate, polyethylene terephthalate-2,5-furandicarboxylate copolyester, polypropylene terephthalate-2,5-furandicarboxylate copolyester, polybutylene terephthalate-2,5-furandicarboxylate copolyester, At least one of poly(adipate-2,5-furandicarboxylic acid ethylene glycol copolyester), poly(adipate-2,5-furandicarboxylic acid propylene glycol copolyester), poly(adipate-2,5-furandicarboxylic acid butylene glycol copolyester), poly(2,5-furandicarboxylic acid-cyclohexanedimethanol-ethylene glycol copolyester), poly(2,5-furandicarboxylic acid-cyclohexanedimethanol-propylene glycol copolyester), and poly(2,5-furandicarboxylic acid-cyclohexanedimethanol-butylene glycol copolyester.

[0008] Furthermore, the structural formula of the diurea nucleating agent containing methylene furan is:

[0009]

[0010] Wherein, n is a natural number ranging from 2 to 110.

[0011] Furthermore, the furan-based polyester composition modified with an alkane diurea nucleating agent comprises 100 parts of furan-based polyester and 2-3 parts of an alkane diurea nucleating agent, in parts by mass.

[0012] The beneficial effect of adopting the above further technical solution is that the present invention introduces a rigid structure to give the alkane diurea nucleating agent good thermal stability, and introduces a long-chain methylene structure in the structure with a higher crystallization temperature to exert a good heterogeneous nucleation effect, thereby improving the crystallization performance of the furan-based polyester material, thereby further improving the barrier performance. In addition, the alkane diurea nucleating agent in the present invention has good thermal stability and meets the processing conditions of polyester materials.

[0013] In a second aspect, the present invention provides a method for preparing a furan-based polyester composition modified by an alkane diurea nucleating agent, comprising pre-mixing the furan-based polyester and the alkane diurea nucleating agent in proportion; and then performing a melt blending process to obtain the furan-based polyester composition modified by the alkane diurea nucleating agent.

[0014] Furthermore, the melt blending process is: placing the pre-mixed furan-based polyester and alkane diurea nucleating agent in a twin-screw extruder for melt blending, the processing temperatures of the conveying section, melting section, mixing section, exhaust section, and homogenizing section of the twin-screw extruder are all 190-250°C, the head temperature is consistent with the processing temperature of the homogenizing section, and the screw speed is 140-160rpm.

[0015] Furthermore, the twin-screw processing temperature is 190°C, 220°C, 230°C, 245°C, 250°C, the die temperature is 250°C, and the screw speed is 150rpm.

[0016] Furthermore, the mass ratio of the furan-based polyester to the alkane diurea nucleating agent is 100:2-3.

[0017] Furthermore, before pre-mixing, the furan-based polyester and the alkane diurea nucleating agent are first placed in a vacuum oven at 80-100° C. for drying for 12-24 hours.

[0018] Furthermore, the preparation method of the alkane diurea nucleating agent comprises the following steps:

[0019] S1. Under the protection of inert gas, add furfurylamine, N,N'-carbonyldiimidazole and ether solvent into the reactor, and stir and react at 20-35°C for 1-4h;

[0020] S2. Under the protection of inert gas, add alkane diamine and react for 3 to 8 hours. After separation and purification, an alkane diurea nucleating agent is obtained.

[0021] Furthermore, the molar ratio of furfurylamine to N,N'-carbonyldiimidazole is 1:1 to 1.2.

[0022] Furthermore, the molar ratio of the alkane diamine to furfurylamine is 1:2 to 2.2.

[0023] Further, the alkane diamine is selected from one of 1,2-ethylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine and 1,10-decanediamine.

[0024] Furthermore, the ether solvent is at least one of diethyl ether, dipropyl ether, diisopropyl ether, ethyl butyl ether, dibutyl ether, dipentyl ether, tetrahydrofuran, 3-methylfuran, diisopentyl ether, dioxolane, 1,4-dioxane, 1,4-dichlorohexane, and ethylene chloride.

[0025] Furthermore, the inert gas is one of nitrogen or argon.

[0026] The specific synthetic route of the above preparation method is shown in the following formula:

[0027]

[0028] Wherein, n is a natural number ranging from 2 to 10.

[0029] Beneficial effects:

[0030] 1. The methylene furan-containing alkane diurea nucleating agent selected by the present invention contains a rigid cyclic structure, which can give the nucleating agent itself excellent thermal stability and meet the processing requirements of various polyesters.

[0031] 2. The structures of the present invention are all symmetrical structures, which are easier to crystallize and thus can be used as nucleating agents for polyesters.

[0032] 3. The preparation method of the methylene furan-containing alkane diurea nucleating agent of the present invention is simple, the raw material source is wide, the product yield is high, the crystallization effect is good and it is easy to industrialize. It can be used to modify polyester materials and can simultaneously improve the crystallization performance and barrier performance of polyester materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The synthetic route of the alkane diurea nucleating agent containing methylene furan prepared in Example 1;

[0034] Figure 2 The alkane diurea nucleating agent containing methylene furan obtained in Example 1 1 H NMR spectra. DETAILED DESCRIPTION

[0035] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.

[0036] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.

[0037] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0038] Various test methods:

[0039] (1) Gas barrier performance test: The prepared furan-based polyester was cut into circular sheets with a diameter of 5 cm for gas barrier performance test. The test standard was GB / T 1038-2000, the test temperature was 23° C., and the test humidity was 0% RH.

[0040] (2) Differential Scanning Calorimetry (DSC) Test: 2-5 mg of sample was placed in an aluminum crucible. The test procedure was to increase the temperature from 25°C to 250°C at a heating rate of 10°C / min, keep the temperature for 2 min, then cool it down to 25°C at a cooling rate of 10°C / min, keep the temperature for 2 min, and finally increase the temperature to 250°C at a heating rate of 10°C / min again. The melting temperature in the second heating was recorded.

[0041] Example 1 (Preparation of nucleating agent, dimethylene furan hexanediurea, n=6)

[0042] The round-bottomed reaction flask equipped with a magnetic rod was baked in advance, evacuated with nitrogen three times, and then a tetrahydrofuran solution containing 6.482g (4.040mmol) N,N'-carbonyldiimidazole and 3.882g (40mmol) furfurylamine were added in sequence under a nitrogen atmosphere. After reacting for 2 hours under vigorous stirring at 25°C, 2.323g (20mmol) 1,6-hexanediamine was added and reacted for 6 hours. After the reaction was completed, the filter cake was washed once with tetrahydrofuran and once with anhydrous ethanol. After drying, 6.93g of white powder was obtained, which was a polyester nucleating agent with a yield of 95.6%. The synthetic route is shown in FIG. Figure 1 .

[0043] The product was characterized by H NMR spectroscopy. Figure 2 .

[0044] Example 2 (Preparation of nucleating agent, dimethylene furanamide, n=4)

[0045] The round-bottomed reaction flask equipped with a magnetic rod was baked in advance, evacuated with nitrogen three times, and then a tetrahydrofuran solution containing 6.482g (40mmol) N,N'-carbonyldiimidazole and 3.882g (40mmol) furfurylamine were added in sequence under a nitrogen atmosphere. After reacting for 2 hours under vigorous stirring at 25°C, 1.762g (20mmol) 1,4-butanediamine was added and reacted for 6 hours. After the reaction was completed, the filter cake was filtered, washed once with tetrahydrofuran, and washed once with anhydrous ethanol, and 5.83g of white powder, i.e., polyester nucleating agent, was obtained after drying, with a yield of 92.1%.

[0046] Example 3 (Preparation of nucleating agent, dimethylene furanoindiurea, n=8)

[0047] The round-bottomed reaction flask equipped with a magnetic rod was baked in advance, evacuated with nitrogen three times, and then a tetrahydrofuran solution containing 6.482g (40mmol) N,N'-carbonyldiimidazole and 3.882g (40mmol) furfurylamine were added in sequence under a nitrogen atmosphere. After reacting for 2 hours under vigorous stirring at 25°C, 2.885g (20mmol) 1,8-octanediamine was added and reacted for 6 hours. After the reaction was completed, the filter cake was filtered, washed once with tetrahydrofuran, and washed once with anhydrous ethanol, and 7.83g of white powder was obtained after drying, i.e., polyester nucleating agent, with a yield of 94.5%.

[0048] Example 4 (Comparative Example: Preparation of Nucleating Agent, Dimethylenepyridine Hexanediurea)

[0049] The round-bottomed reaction flask equipped with a magnetic rod was baked in advance, evacuated with nitrogen three times, and then a tetrahydrofuran solution containing 6.482g (40mmol) N, N'-carbonyldiimidazole and 4.322g (40mmol) 2-aminomethylpyridine were added in sequence under a nitrogen atmosphere. After reacting for 2 hours under vigorous stirring at 25°C, 2.323g (20mmol) 1,6-hexanediamine was added and reacted for 6 hours. After the reaction was completed, the filter cake was filtered, washed once with tetrahydrofuran, and once with anhydrous ethanol, and 5.97g of white powder was obtained after drying, i.e., the comparative polyester nucleating agent, with a yield of 91.0%.

[0050] Example 5 (Comparative Example: Preparation of Nucleating Agent, Dimethylene Benzyl Hexane Diurea)

[0051] The round-bottomed reaction flask equipped with a magnetic rod was baked in advance, evacuated with nitrogen three times, and then a tetrahydrofuran solution containing 6.482g (40mmol) N, N'-carbonyldiimidazole and 4.283g (40mmol) benzylamine were added in sequence under a nitrogen atmosphere. After reacting for 2 hours under vigorous stirring at 25°C, 2.323g (20mmol) 1,6-hexanediamine was added and reacted for 6 hours. After the reaction was completed, the filter cake was filtered, washed once with tetrahydrofuran, and washed once with anhydrous ethanol, and 6.04g of white powder was obtained after drying, i.e., the comparative polyester nucleating agent, with a yield of 90.3%.

[0052] Example 6

[0053] The diurea nucleating agent containing methylene furan obtained in Example 1 was dried in an 80°C blast oven for 8 hours for use, and the polyethylene furan dicarboxylate was dried in an 80°C blast oven for 8 hours for use. The alkane diurea nucleating agent of methyl furan and polyethylene furan dicarboxylate were added to a twin-screw extruder for melt blending at a mass fraction of 1:100. The twin-screw extrusion temperature was 190-250°C, the speed was 150r / min, and the polyethylene furan dicarboxylate composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 221.3°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.0042barrer and the carbon dioxide permeability coefficient was 0.0037barrer. According to the tensile performance test, the tensile strength was 81.9Mpa.

[0054] Example 7

[0055] The parameters are consistent with those in Example 6, except that the addition amount of the diurea nucleating agent containing methylene furan is 3 parts. According to the DSC non-isothermal test, the melting temperature is 225.9°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient is 0.0036 barrer, and the carbon dioxide permeability coefficient is 0.0027 barrer. According to the tensile property test, the tensile strength is 85.2 Mpa.

[0056] Example 8

[0057] The diurea nucleating agent containing methylene furan obtained in Example 2 was dried in an air-blast oven at 80°C for 8h for use, and the polyethylene furan dicarboxylate was dried in an air-blast oven at 80°C for 8h for use. The alkane diurea nucleating agent containing methylene furan and polyethylene furan dicarboxylate were added to a twin-screw extruder for melt blending in a mass fraction of 1:100. The twin-screw extrusion temperature was 190-250°C, the speed was 150r / min, and the polyethylene furan dicarboxylate composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 217.3°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.0052barrer and the carbon dioxide permeability coefficient was 0.0043barrer. According to the tensile performance test, the tensile strength was 78.6Mpa.

[0058] Example 9

[0059] The parameters are consistent with those of Example 8, except that the addition amount of the diurea nucleating agent containing methylene furan is 3 parts. According to the DSC non-isothermal test, the melting temperature during the secondary heating process is 221.6°C. According to the gas barrier test, the oxygen permeability coefficient is 0.0041 barrer, and the carbon dioxide permeability coefficient is 0.0037 barrer. According to the tensile property test, the tensile strength is 82.2 Mpa.

[0060] Example 10 (Comparative Example)

[0061] The comparative example nucleating agent dimethylene pyridine hexane diurea obtained in Example 4 was dried in an 80°C blast oven for 8 hours for use, and polyethylene furandicarboxylate was dried in an 80°C blast oven for 8 hours for use. The nucleating agent and polyethylene furandicarboxylate were added to a twin-screw extruder for melt blending according to a mass fraction of 1:100. The twin-screw extrusion temperature was 190-250°C, the rotation speed was 150r / min, and the polyethylene furandicarboxylate composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 216.4°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.0061barrer and the carbon dioxide permeability coefficient was 0.0047barrer. According to the tensile performance test, the tensile strength was 77.4Mpa.

[0062] Example 11 (Comparative Example)

[0063] The comparative nucleating agent dimethylene benzyl hexane diurea obtained in Example 5 was dried in an 80°C blast oven for 8 hours for use, and polyethylene furandicarboxylate was dried in an 80°C blast oven for 8 hours for use. The nucleating agent and polyethylene furandicarboxylate were added to a twin-screw extruder for melt blending according to a mass fraction of 1:100. The twin-screw extrusion temperature was 190-250°C, the rotation speed was 150r / min, and the polyethylene furandicarboxylate composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 213.8°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.0068barrer and the carbon dioxide permeability coefficient was 0.0053barrer. According to the tensile performance test, the tensile strength was 72.9Mpa.

[0064] Example 12 (Comparative Example)

[0065] The polyethylene furandicarboxylate was dried in a blast oven at 80°C for 8 hours for later use. It was extruded and pelletized by a twin-screw extruder at a temperature of 190-250°C and a rotation speed of 150r / min. The DSC non-isothermal test showed that the melting temperature was not displayed during the secondary heating process. The gas barrier test showed that the oxygen permeability coefficient was 0.0073 barrer and the carbon dioxide permeability coefficient was 0.0068 barrer. The tensile strength test showed that the tensile strength was 71.5Mpa.

[0066] Example 13

[0067] The diurea nucleating agent containing methylene furan obtained in Example 1 was dried in an 80°C blast oven for 8 hours for use, and polyfuran dicarboxylic acid propylene glycol was dried in an 80°C blast oven for 8 hours for use. According to the mass fraction of 1:100, the diurea nucleating agent containing methylene furan and polyfuran dicarboxylic acid propylene glycol were added to the twin-screw extrusion melt blending, the twin-screw extrusion temperature was 190-250°C, the speed was 150r / min, and the polyfuran dicarboxylic acid propylene glycol composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 171.8°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.0059barrer and the carbon dioxide permeability coefficient was 0.0041barrer. According to the tensile performance test, the tensile strength was 73.4Mpa.

[0068] Embodiment 14

[0069] The parameters are consistent with those of Example 13, except that the addition amount of the diurea nucleating agent containing methylene furan is 3 parts. According to the DSC non-isothermal test, the melting temperature during the secondary heating process is 176.1°C. According to the gas barrier test, the oxygen permeability coefficient is 0.0049 barrer, and the carbon dioxide permeability coefficient is 0.0037 barrer. According to the tensile property test, the tensile strength is 75.6 MPa.

[0070] Embodiment 15

[0071] The diurea nucleating agent containing methylene furan obtained in Example 2 was dried in an 80°C blast oven for 8h for standby use, and polyfuran dicarboxylic acid propylene glycol was dried in an 80°C blast oven for 8h for standby use. The diurea nucleating agent containing methylene furan and polyfuran dicarboxylic acid propylene glycol were added to a twin-screw extruder for melt blending at a mass fraction of 1:100. The twin-screw extrusion temperature was 190-250°C, the speed was 150r / min, and the polyfuran dicarboxylic acid propylene glycol composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 168.2°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.0064barrer and the carbon dioxide permeability coefficient was 0.0053barrer. According to the tensile performance test, the tensile strength was 71.8Mpa.

[0072] Example 16

[0073] The parameters are consistent with those of Example 15, except that the addition amount of the diurea nucleating agent containing methylene furan is 3 parts. According to the DSC non-isothermal test, the melting temperature during the secondary heating process is 175.9°C. According to the gas barrier test, the oxygen permeability coefficient is 0.0057 barrer, and the carbon dioxide permeability coefficient is 0.0044 barrer. According to the tensile property test, the tensile strength is 74.1 MPa.

[0074] Example 17 (Comparative Example)

[0075] The comparative example nucleating agent dimethylene pyridine hexane diurea obtained in Example 4 was dried in an 80°C blast oven for 8 hours for use, and poly(propylene furan dicarboxylate) was dried in an 80°C blast oven for 8 hours for use. The nucleating agent and poly(propylene furan dicarboxylate) were added to a twin-screw extruder for melt blending according to a mass fraction of 1:100. The twin-screw extrusion temperature was 190-250°C, the speed was 50r / min, and the poly(propylene furan dicarboxylate) composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 168.7°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.0071barrer and the carbon dioxide permeability coefficient was 0.0058barrer. According to the tensile performance test, the tensile strength was 72.9Mpa.

[0076] Example 18 (Comparative Example)

[0077] The comparative nucleating agent dimethylene benzyl hexane diurea obtained in Example 5 was dried in an 80°C blast oven for 8 hours for use, and poly(propylene furan dicarboxylate) was dried in an 80°C blast oven for 8 hours for use. The nucleating agent and poly(propylene furan dicarboxylate) were added to a twin-screw extruder for melt blending in a mass fraction of 1:100. The twin-screw extrusion temperature was 190-250°C, the rotation speed was 150r / min, and the poly(propylene furan dicarboxylate) composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 165.4°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.0079barrer and the carbon dioxide permeability coefficient was 0.0062barrer. According to the tensile performance test, the tensile strength was 70.3Mpa.

[0078] Example 19 (Comparative Example)

[0079] The poly(propylene furandicarboxylate) was dried in a blast oven at 80°C for 8 hours for later use. It was extruded and pelletized by a twin-screw extruder at a temperature of 190-250°C and a rotation speed of 150r / min. The DSC non-isothermal test showed that the melting temperature was not displayed during the secondary heating process. The gas barrier test showed that the oxygen permeability coefficient was 0.0084 barrer and the carbon dioxide permeability coefficient was 0.0077 barrer. The tensile strength test showed that the tensile strength was 66.7Mpa.

[0080] Embodiment 20

[0081] The diurea nucleating agent containing methylene furan obtained in Example 1 was dried in an 80°C blast oven for 8h for standby use, and the polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester was dried in an 80°C blast oven for 8h for standby use. The alkane diurea nucleating agent containing methylene furan and polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester were added to a twin-screw extruder for melt blending in a ratio of 1:100 by mass. The twin-screw extrusion temperature was 190-250°C, the speed was 150r / min, and the polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 216.2°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.056barrer and the carbon dioxide permeability coefficient was 0.047barrer. According to the tensile property test, the tensile strength was 68.9Mpa.

[0082] Embodiment 21

[0083] The parameters are consistent with those of Example 20, except that the addition amount of the diurea nucleating agent containing methylene furan is 3 parts. According to the DSC non-isothermal test, the melting temperature during the secondary heating process is 219.2°C. According to the gas barrier test, the oxygen permeability coefficient is 0.048 barrer, and the carbon dioxide permeability coefficient is 0.041 barrer. According to the tensile property test, the tensile strength is 71.3 Mpa.

[0084] Embodiment 22

[0085] The diurea nucleating agent containing methylene furan obtained in Example 2 was dried in a blast oven at 80°C for 8h for standby use, and the polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester was dried in a blast oven at 80°C for 8h for standby use. The alkane diurea nucleating agent containing methylene furan and polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester were added to a twin-screw extruder for melt blending at a mass ratio of 1:100. The twin-screw extrusion temperature was 190-250°C, the speed was 150r / min, and the polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 211.7°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.066barrer and the carbon dioxide permeability coefficient was 0.058barrer. After tensile performance testing, the tensile strength is 62.4Mpa.

[0086] Embodiment 23

[0087] The parameters are consistent with those of Example 22, except that the addition amount of the diurea nucleating agent containing methylene furan is 3 parts. According to the DSC non-isothermal test, the melting temperature during the secondary heating process is 214.6°C. According to the gas barrier test, the oxygen permeability coefficient is 0.051 barrer, and the carbon dioxide permeability coefficient is 0.049 barrer. According to the tensile property test, the tensile strength is 67.7 MPa.

[0088] Example 24 (Comparative Example)

[0089] The comparative example nucleating agent dimethylene pyridine hexane diurea obtained in Example 4 was dried in an 80°C blast oven for 8 hours for use, and the polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester was dried in an 80°C blast oven for 8 hours for use. The nucleating agent and polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester were added to a twin-screw extruder for melt blending at a mass ratio of 1:100. The twin-screw extrusion temperature was 190-250°C, the speed was 150r / min, and the polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 211.7°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.069barrer and the carbon dioxide permeability coefficient was 0.057barrer. According to the tensile property test, the tensile strength was 65.2Mpa.

[0090] Example 25 (Comparative Example)

[0091] The comparative nucleating agent dimethylene benzyl hexane diurea obtained in Example 5 was dried in an 80°C blast oven for 8h for standby use, and the polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester was dried in an 80°C blast oven for 8h for standby use. The nucleating agent and polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester were added to a twin-screw extruder for melt blending in a mass fraction of 1:100. The twin-screw extrusion temperature was 190-250°C, the speed was 150r / min, and the polyethylene terephthalate-2,5-furan dicarboxylic acid glycol copolyester composite material was pelletized. According to the DSC non-isothermal test, the melting temperature was 209.4°C during the secondary heating process. According to the gas barrier test, the oxygen permeability coefficient was 0.071barrer and the carbon dioxide permeability coefficient was 0.062barrer. According to the tensile property test, the tensile strength was 63.1Mpa.

[0092] Example 26 (Comparative Example)

[0093] The polyethylene terephthalate-2,5-furandicarboxylate copolyester was dried in a blast oven at 80°C for 8 hours for use. It was extruded and pelletized by a twin-screw extrusion, and the twin-screw extrusion temperature was 190-250°C and the speed was 150r / min. After DSC non-isothermal test, no melting temperature was shown during the secondary heating process. After gas barrier test, the oxygen permeability coefficient was 0.089 barrer and the carbon dioxide permeability coefficient was 0.071 barrer. After tensile performance test, the tensile strength was 60.1Mpa.

[0094] Although the above describes the specific implementation mode of the present invention in conjunction with the accompanying drawings, it is not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art on the basis of the technical solution of the present invention without creative work are still within the scope of protection of the present invention.

Claims

1. A furan-based polyester composition modified by an alkane diurea nucleating agent, characterized in that: Calculated by weight, it includes 100 parts of furan-based polyester and 1-5 parts of alkane diurea nucleating agent; The structural formula of the alkane diurea nucleating agent is: Wherein, n is a natural number, and its value range is a natural number from 2 to 10.

2. The furan-based polyester composition according to claim 1, characterized in that The furan-based polyester is selected from polyethylene furandicarboxylate, polypropylene furandicarboxylate, polybutylene furandicarboxylate, polypentane furandicarboxylate, polyhexane furandicarboxylate, polyoctane furandicarboxylate, polyethylene terephthalate-2,5-furandicarboxylate copolyester, polypropylene terephthalate-2,5-furandicarboxylate copolyester, polybutylene terephthalate-2,5-furandicarboxylate copolyester, At least one of poly(adipate-2,5-furandicarboxylic acid ethylene glycol copolyester), poly(adipate-2,5-furandicarboxylic acid propylene glycol copolyester), poly(adipate-2,5-furandicarboxylic acid butylene glycol copolyester), poly(2,5-furandicarboxylic acid-cyclohexanedimethanol-ethylene glycol copolyester), poly(2,5-furandicarboxylic acid-cyclohexanedimethanol-propylene glycol copolyester), and poly(2,5-furandicarboxylic acid-cyclohexanedimethanol-butylene glycol copolyester.

3. The furan-based polyester composition according to claim 1, characterized in that Calculated by weight, it includes 100 parts of furan-based polyester and 2-3 parts of alkane diurea nucleating agent.

4. A method for preparing a furan-based polyester composition according to any one of claims 1 to 2, characterized in that: The furan-based polyester and the alkane diurea nucleating agent are pre-mixed in a ratio of 100:1-5; and then a melt blending process is performed to obtain the furan-based polyester composition modified by the alkane diurea nucleating agent.

5. The preparation method according to claim 4, characterized in that: The melt blending process is as follows: pre-mixed furan-based polyester and alkane diurea nucleating agent are placed in a twin-screw extruder for melt blending to obtain a masterbatch; the processing temperatures of the conveying section, melting section, mixing section, exhaust section and homogenizing section of the twin-screw extruder are all 190-250°C, the head temperature is consistent with the processing temperature of the homogenizing section, and the screw speed is 140-160rpm.

6. The preparation method according to claim 5, characterized in that: The twin-screw processing temperature is 190°C, 220°C, 230°C, 245°C, 250°C, the die temperature is 248°C, and the screw speed is 150rpm.

7. The preparation method according to claim 4, characterized in that: Before pre-mixing, the furan-based polyester and the alkane diurea nucleating agent are first placed in a vacuum oven at 80-100° C. to dry for 12-24 hours.

8. The furan-based polyester composition according to claim 1, characterized in that The alkane diurea nucleating agent is prepared according to the following steps: S1. Under the protection of inert gas, add furfurylamine, N,N'-carbonyldiimidazole and ether solvent into the reactor, and stir and react at 20-35°C for 1-4h; S2. Under the protection of inert gas, add alkane diamine, react for 3 to 8 hours, and obtain an alkane diurea nucleating agent after separation and purification; The molar ratio of furfurylamine to N,N'-carbonyldiimidazole is 1:1-1.2; The molar ratio of the alkane diamine to the furfurylamine is 1:2 to 2.

2.

9. The furan-based polyester composition according to claim 8, characterized in that The alkane diamine is selected from one of 1,2-ethylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine and 1,10-decanediamine.

10. The furan-based polyester composition according to claim 8, characterized in that The ether solvent is at least one of diethyl ether, dipropyl ether, diisopropyl ether, ethyl butyl ether, dibutyl ether, dipentyl ether, tetrahydrofuran, 3-methylfuran, diisopentyl ether, dioxolane, 1,4-dioxane, 1,4-dichlorohexane and ethylene chloride.