Solid block super-hydrophobic material as well as preparation method and application thereof
By modifying the silica particles with low surface energy and combining them with organic resins and silane coupling agents, a solid bulk superhydrophobic material was prepared, which solved the problem of degradation of existing coatings in harsh environments and achieved High mechanical strength and durability, suitable for superhydrophobic shells of electrical equipment and other devices.
Patent Information
- Application Number
- CN202410864273.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-30
AI Technical Summary
Existing superhydrophobic coatings are easily degraded in harsh environments such as high humidity, ultraviolet radiation, and chemical corrosion. They have low mechanical strength, insufficient wear resistance and durability, and cannot meet the long-term use needs of power equipment and other devices.
Silica particles are modified with low surface energy using fluoroalkyl compounds, mixed with organic resins and silane coupling agents, and processed through evaporation, air bubble elimination, curing, compression molding and post-curing to prepare silica particles with excellent ultra-high performance. Solid bulk superhydrophobic materials with hydrophobic properties and high mechanical strength.
The material has excellent superhydrophobic properties both on the surface and inside, improves wear resistance and durability, and can maintain superhydrophobic properties under mechanical load. It is suitable for superhydrophobic shells of power equipment and other devices, reducing the frequency of maintenance and replacement. Significantly reduces long-term operating costs.
Smart Images

Figure CN118772618A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of material preparation, and more specifically, relates to a solid block superhydrophobic material, a preparation method and application thereof. Background Art
[0002] The moisture, dust, etc. accumulated on the surface of electrical equipment will reduce the insulation capacity of the insulating material, increase the risk of leakage and short circuit, hinder heat dissipation, and thus cause equipment overheating, affecting the normal operation and life of the equipment. In addition, it may also cause the metal parts of the equipment to rust and corrode, weaken the structural strength of the equipment, cause poor contact, circuit breakage and other faults, and affect the stability and reliability of the equipment.
[0003] Super-hydrophobic materials refer to materials whose contact angle of water droplets on their surface is greater than 150°, and have excellent self-cleaning, waterproof, anti-fouling, anti-icing and other properties. At present, super-hydrophobic coatings are mainly formed by spraying or brushing super-hydrophobic materials on the surface of power equipment, thereby reducing the accumulation of moisture and dust, making it have anti-fouling flash, anti-corrosion, anti-icing and other properties. However, super-hydrophobic coatings have low mechanical strength, poor wear resistance and durability, and are prone to degradation in harsh environments such as high humidity, ultraviolet radiation, and chemical corrosion. During use, they are subject to bumps, scrapes, scratches or repeated friction and wear from external objects, which causes the super-hydrophobic properties to be lost. The weather resistance and service life of super-hydrophobic coatings do not meet actual needs.
[0004] Therefore, it is of great significance to prepare solid bulk superhydrophobic materials with superhydrophobic properties and high mechanical strength. Summary of the invention
[0005] In view of the defects of the prior art, the purpose of the present application is to provide a solid block superhydrophobic material, a preparation method and application thereof, aiming to provide a solid block superhydrophobic material having excellent superhydrophobic properties on the material surface and inside the matrix and high mechanical strength, which is suitable for superhydrophobic casings of devices such as power equipment.
[0006] To achieve the above object, the present application provides a method for preparing a solid block super-hydrophobic material, comprising the following steps:
[0007] S1, mixing a silica dispersion obtained by mixing silica particles and a solvent with a fluoroalkyl compound solution, so that the fluorine atoms in the fluoroalkyl compound solution replace the hydroxyl groups on the surface of the silica particles, and perform low surface energy modification to obtain a reaction solution containing modified silica particles;
[0008] S2, mixing and stirring the slurry obtained by evaporating the reaction solution, the organic resin solution, and the silane coupling agent to form a suspension;
[0009] S3, degassing, solidifying, pressing and post-curing the suspension to obtain a solid block super-hydrophobic material.
[0010] Preferably, in step S1, the particle size of the silicon dioxide particles is 50 nm to 300 nm.
[0011] Preferably, the fluoroalkyl compound solution is prepared by mixing a fluoroalkyl compound with a solvent, and the fluoroalkyl compound is selected from one or more of perfluorooctyltriethoxysilane, triethoxyfluorosilane, perfluorooctane sulfonic acid, perfluorobutylethyltriethoxysilane, perfluoroethyl vinyl ether and perfluorohexyl vinyl ether.
[0012] Preferably, the method for preparing the above silicon dioxide particles comprises the following steps: under a protective atmosphere, mixing a silicon source compound, an alcohol solvent, an alkaline environment regulator, deionized water and an auxiliary silicon source compound, stirring, centrifuging, washing and drying to obtain silicon dioxide particles.
[0013] Preferably, the silicon source compound is a silanol compound, selected from at least one of ethyl orthosilicate, propyl orthosilicate and tetraethoxysilane; and / or,
[0014] The auxiliary silicon source compound is selected from at least one of silicon halide hydrocarbons and trihalosilanes; and / or,
[0015] The volume ratio of the silicon source compound to the auxiliary silicon source compound is 1:(0.025-0.075); and / or,
[0016] The stirring temperature is 20°C to 40°C, and the stirring time is 4h to 6h.
[0017] Preferably, in step S2, the solid content of the modified silicon dioxide particles in the slurry is 15% to 30%; and / or,
[0018] The organic resin solution is formed by mixing an organic resin and an organic solvent, and the organic resin is selected from one or more of polyurethane resin, epoxy resin, methyl silicone resin, polymethyl methacrylate and acrylic resin; and / or,
[0019] The silane coupling agent is selected from one or more of 3-(methacryloyloxy)propyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane and vinyltrimethoxysilane; and / or,
[0020] In the suspension, the mass ratio of the modified silica particles to the organic resin is 1:(2.5-3.5), and the mass ratio of the silane coupling agent to the organic resin is 1:(80-120).
[0021] Preferably, in step S3, the specific operation of removing bubbles is: placing the suspension in a mold with air holes, and evacuating the air bubbles, wherein the vacuum degree is -0.09MPa to 0.01MPa, and the evacuation time is 25min to 35min.
[0022] Preferably, in step S3, the curing temperature is 90° C. to 100° C., and the curing time is 16 h to 20 h; and / or,
[0023] The pressure of the above-mentioned pressing is 4MPa to 6MPa; and / or,
[0024] The post-curing temperature is 140° C. to 160° C., and the post-curing time is 3 h to 5 h.
[0025] The present application provides a solid block superhydrophobic material prepared according to the above preparation method.
[0026] The present application also provides the use of the above-mentioned solid block superhydrophobic material in preparing a superhydrophobic shell of a device.
[0027] The present application also provides a super-hydrophobic shell comprising the above-mentioned solid block super-hydrophobic material.
[0028] In general, the above technical solutions conceived by this application have the following technical advantages compared with the prior art:
[0029] (1) The preparation method of the solid block super-hydrophobic material provided by the present application is to modify the silicon dioxide with low surface energy by using a fluoroalkyl compound, then perform an evaporation treatment, mix the slurry obtained after evaporation with an organic resin solution and a silane coupling agent, and perform bubble removal, curing, compression molding and post-curing treatment to prepare a solid block super-hydrophobic material with excellent super-hydrophobic properties on the surface and inside of the material and high mechanical strength. The process for preparing the solid block super-hydrophobic material of the present application is simple, easy to operate, has low equipment requirements, and is suitable for large-scale production.
[0030] (2) Compared with the prior art, the present application can adjust the particle size of the silica particles by adding an appropriate amount of auxiliary silicon source compound when preparing silica particles, improve the dispersibility of the silica particles, without the need for additional grinding, sieving and other treatments, the processing method is simple, and the production cost is reduced. Further, the above-mentioned silica particles are subjected to low surface energy modification and evaporation treatment, and the solid content of the modified silica in the slurry is reasonably adjusted, and the mass ratio, curing temperature and time between the modified silica, organic resin and silane coupling agent in the suspension are coordinated and regulated at the same time, so that a solid block super-hydrophobic material can be prepared, and the hydrophobic performance, interface strength and mechanical stability of the solid block super-hydrophobic material can be improved, so that it is suitable for the super-hydrophobic shell of devices such as power equipment.
[0031] (3) the solid block super-hydrophobic material obtained by the present application can make up for the defects of coating while maintaining the advantages of super-hydrophobic coating, and improve the wear resistance and durability of super-hydrophobic material. In practical applications, when the surface of the above-mentioned solid block super-hydrophobic material is damaged, the inner layer material is exposed to the external environment, replaces the damaged part to continue to provide super-hydrophobicity, greatly improves the weather resistance and service life of super-hydrophobic material. In addition, the solid block super-hydrophobic material obtained by the present application has higher mechanical strength, can withstand larger mechanical load, and reduces the super-hydrophobic performance caused by bumping, scratching, scratching, wearing or impact. Compared with existing super-hydrophobic coating, the solid block super-hydrophobic material provided by the present application has stronger durability, can effectively reduce the frequency of maintenance, replacement, so as to significantly reduce long-term operation cost.
[0032] (4) The solid bulk superhydrophobic material provided in the present application exhibits excellent mechanical properties and outstanding mechanical stability. The above-mentioned solid bulk superhydrophobic material system can be pressed and molded into solid bulk superhydrophobic materials of different shapes, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a preparation flow chart of a solid block superhydrophobic material provided by the present application;
[0034] Figure 2 is the XPS spectrum of the modified silica nanoparticles prepared in Example 1 of the present application;
[0035] Figure 3 It is a solid block superhydrophobic material prepared in the embodiment of the present application;
[0036] Figure 4 The contact angle measurement results of the solid block superhydrophobic material prepared in Example 1 of the present application. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.
[0038] The purpose of the present application is to prepare a solid block super-hydrophobic material with excellent super-hydrophobicity and high mechanical strength on the surface and inside of the material, the amount of modified silica in the material has a significant effect on its hydrophobicity, initially try to improve the hydrophobicity of the material by increasing the amount of modified silica, then use the method of drying to prepare a solid block super-hydrophobic material, but the inventor of the present application finds that the amount of modified silica is increased, while improving the super-hydrophobicity of the material, the manufacturing difficulty is sharply increased, and it is impossible to effectively mix modified silica and organic resin, and the hydrophobic material obtained is a plasticine-like soft material, and a large amount of curing agents need to be added additionally to obtain solid block materials, but the hydrophobicity of the material can be reduced at the same time. Further, the method of compression molding is used to prepare, and the interfacial strength of the hydrophobic material obtained is low, and a predetermined hardness cannot be reached, and the hydrophobicity of the material is uneven. How to improve the hydrophobicity, interfacial strength and mechanical stability of the hydrophobic material while preparing the solid block hydrophobic material, so that it is suitable for the super-hydrophobic shell of devices such as power equipment, is the key problem to be solved in the present application. Based on this, the present application provides a method for preparing a solid block super-hydrophobic material, such as Figure 1 As shown, the following steps are included:
[0039] S1, mixing the silica particles and the solvent to obtain a silica dispersion and stirring the fluoroalkyl compound solution, so that the fluorine atoms in the fluoroalkyl compound solution replace the hydroxyl groups on the surface of the silica particles, and perform low surface energy modification to obtain a reaction solution containing modified silica particles;
[0040] S2, mixing the slurry obtained by evaporating the reaction solution, the organic resin solution and the silane coupling agent to form a suspension;
[0041] S3, degassing, solidifying, pressing and post-curing the suspension to obtain a solid block super-hydrophobic material.
[0042] In some embodiments, in step S1, the particle size of the silicon dioxide particles is 50 nm to 300 nm.
[0043] In a preferred embodiment, in step S1, the particle size of the silicon dioxide particles is 100 nm to 200 nm.
[0044] It is understandable that the above-mentioned silicon dioxide particles can be purchased from commercial products or prepared in the laboratory, as long as the particle size and particle size uniformity of the silicon dioxide particles are consistent with the present application.
[0045] In a preferred embodiment, the method for preparing the above-mentioned silicon dioxide particles in the present application comprises the following steps:
[0046] Select precursor material:
[0047] In some embodiments, the silicon source compound is a silanol compound, such as but not limited to tetraethyl orthosilicate (TEOS), propyl orthosilicate (TPS) and tetraethoxysilane (TEOSS). The auxiliary silicon source compound is a silicon halide hydrocarbon, a trihalosilane, such as but not limited to silicon tetrachloride (STC) and trichloromethylsilane (MTMS). The purity of the silicon source compound and the auxiliary silicon source compound is greater than 99.9%, and both can be hydrolyzed under alkaline conditions, wherein the hydrolysis performance of the silicon source compound is better than that of the auxiliary silicon source compound.
[0048] In a preferred embodiment, the volume ratio of the above-mentioned silicon source compound and the above-mentioned auxiliary silicon source compound is 1: (0.025 ~ 0.075). The inventors of the present application have found through experiments that adding an appropriate amount of auxiliary silicon source compound can adjust the particle size of the obtained silica particles and improve the dispersibility of the silica particles without the need for additional grinding, screening and other treatments. In practical applications, it can effectively shorten the production time and reduce production costs. Further experiments have found that when the amount of the auxiliary silicon source compound is too small, the dispersibility of the silica particles cannot be effectively improved; when the amount of the auxiliary silicon source compound is too large, a large number of halogen groups are introduced into the reaction system, and too many halogen groups may react with other components in the reaction system to produce side reactions, thereby making the reaction system more complicated and difficult to control. At the same time, halogen atoms have strong electronegativity, and excessive halogen groups can change the surface properties of the silica particles, affect the surface energy and hydrophilicity of the final product, and cause the super hydrophobic properties of the hydrophobic material obtained later to deteriorate. The present application has found through experiments that the auxiliary silicon source compound has a significant effect on the microscopic morphology of the silica particles, which will further affect the mechanical stability and superhydrophobic stability of the solid bulk superhydrophobic system, thereby affecting the macroscopic hydrophobic performance.
[0049] Preparation of silica particles:
[0050] Under a protective atmosphere, the silicon source compound, alcohol solvent, alkaline environment regulator, deionized water and auxiliary silicon source compound are mixed and stirred to allow the silicon source compound to undergo hydrolysis and condensation reactions, and then centrifuged, washed and dried to obtain silicon dioxide particles.
[0051] The present application does not limit the order of the above-mentioned "mixing and stirring". In some embodiments, it can be: the above-mentioned silicon source compound, alcohol solvent, alkaline environmental regulator and deionized water are mixed and stirred, and the auxiliary silicon source compound is added dropwise during the stirring process.
[0052] In some embodiments, the protective atmosphere includes one or more of nitrogen, argon, neon, helium, xenon or krypton.
[0053] The present application has no special limitation on the types of the above-mentioned alcohol solvents, and any alcohol solvent reported in the prior art may be used, such as but not limited to anhydrous ethanol, methanol, and isopropanol.
[0054] In the present application, the alkaline environment regulator is used to adjust the pH of the reaction system and create an alkaline environment. Any alkaline environment regulator reported in the prior art can be used, such as but not limited to ammonia water and tetramethylammonium hydroxide. In a specific embodiment of the present application, the pH value of the reaction system is controlled within the range of 7.2 to 8.0 by the alkaline environment regulator, so that the silicon source compound undergoes hydrolysis and condensation reaction in an alkaline environment to form silicon dioxide particles with a certain particle size.
[0055] In some embodiments, the volume ratio of the silicon source compound, the alcohol solvent, the alkaline environment conditioner and the deionized water is 1:(12-14):(1.75-2.25):(2.5-3.5).
[0056] In some embodiments, the temperature of the mixing and stirring is 20°C to 40°C, and the mixing and stirring time is 4h to 6h. It is understood that the present application does not limit the above-mentioned "mixing and stirring" method. Those skilled in the art can extend or shorten the stirring time according to the mixing and stirring method, which is within the protection scope of the present application.
[0057] In some embodiments, the centrifugal speed is 8000 rpm to 12000 rpm, and the centrifugal time is 10 min to 30 min.
[0058] In some embodiments, the precipitate obtained after centrifugation is washed with deionized water and the above alcohol solvent, and the washing is repeated 2 to 5 times.
[0059] In some embodiments, the drying temperature is 50° C. to 80° C., and the drying time is 12 h to 48 h.
[0060] In some embodiments, step S1 includes the following steps:
[0061] S1-1. Preparation of silicon dioxide dispersion:
[0062] The silicon dioxide particles obtained in step S1 are mixed with a solvent to obtain a silicon dioxide dispersion.
[0063] In the present application, the above-mentioned solvent can make the silicon dioxide particles uniformly dispersed. The present application does not limit the type of the above-mentioned solvent, such as but not limited to anhydrous ethanol, methanol, and isopropanol.
[0064] It should be noted that the present application does not limit the mass ratio of the above-mentioned silicon dioxide particles to the above-mentioned solvent, as long as the above-mentioned silicon dioxide particles can be evenly dispersed in the above-mentioned solvent.
[0065] The present application does not limit the above-mentioned "mixing" method, such as but not limited to ultrasound, stirring and the like. In some embodiments, the above-mentioned mixing method is ultrasound. In a specific embodiment of the present application, the above-mentioned ultrasonic treatment time is 20min to 60min. In practical applications, shortening or extending the ultrasonic treatment time according to the adaptability of the ultrasonic equipment used is also within the scope of protection of the present application.
[0066] It is understandable that the above silicon dioxide dispersion can be obtained by mixing a commercially available product with a solvent, or by mixing silicon dioxide particles prepared by other experimental methods with a solvent.
[0067] S1-2. Modification of silica particles to reduce surface energy:
[0068] The silica dispersion and the fluoroalkyl compound solution are mixed and stirred so that the fluorine atoms in the fluoroalkyl compound solution replace the hydroxyl groups on the surface of the silica particles, thereby performing low surface energy modification to obtain a reaction solution containing modified silica particles.
[0069] In some embodiments, the fluoroalkyl compound solution is prepared by mixing the fluoroalkyl compound with a solvent, and the solvent may be, but is not limited to, ethanol, methanol, or ethyl acetate. The present application does not limit the source of the fluoroalkyl compound solution, which may be purchased from a commercial product or prepared in a laboratory.
[0070] In a specific embodiment, a fluoroalkyl compound is mixed with a solvent to prepare a fluoroalkyl compound solution. The present application does not limit the mass ratio of the fluoroalkyl compound to the solvent, as long as the fluoroalkyl compound can be evenly dispersed in the solvent, which can be (0.5-1.5):1.
[0071] In some embodiments, the fluoroalkyl compound includes one or more of perfluorooctyltriethoxysilane (HFOTES), triethoxyfluorosilane (TEFS), perfluorooctane sulfonic acid (PFOS), perfluorobutylethyltriethoxysilane, perfluoroethyl vinyl ether and perfluorohexyl vinyl ether.
[0072] In the present application, the mass ratio of the fluoroalkyl compound to the silica particles is not particularly limited and may be (0.1-1):1, ensuring that the fluorine atoms of the fluoroalkyl compound can fully replace the hydroxyl groups on the surface of the silica particles.
[0073] The present application does not limit the method of "mixing and stirring the silica dispersion and the fluoroalkyl compound solution". In some embodiments, the fluoroalkyl compound solution is slowly added dropwise to the silica dispersion and mixed and stirred.
[0074] In some embodiments, the dropping rate is 3 mL / min to 10 mL / min, the mixing temperature is 40°C to 60°C, and the mixing time is 3 h to 5 h, ensuring that the fluoroalkyl compound is in full contact and reacts with the silica particles to form a stable low surface energy coating on the surface of the silica particles, thereby achieving low surface energy modification of the silica particles.
[0075] In some embodiments, step S2 includes the following steps:
[0076] S2-1, evaporating the reaction solution obtained in step S1 to obtain slurry.
[0077] In some embodiments, the evaporation temperature is 48° C. to 52° C., and the evaporation time is 2 h to 3 h.
[0078] In some embodiments, the solid content of the modified silicon dioxide particles in the slurry is 15% to 30%.
[0079] In a preferred embodiment, the solid content of the modified silica particles in the slurry is 20% to 25%.
[0080] S2-2, the slurry, organic resin solution and silane coupling agent are mixed and stirred to form a suspension.
[0081] In some embodiments, the organic resin solution is formed by mixing an organic resin with an organic solvent, and the organic solvent may be, but is not limited to, acetone, xylene, or ethyl acetate. The present application does not limit the source of the organic resin solution, and the organic resin solution may be purchased from a commercial product or prepared in a laboratory.
[0082] The present application is directed to the main types and characteristics of the functional groups on the surface of the modified silica particles, and selects an organic resin that can form a strong bonding strength therewith for mixing. In some embodiments, the organic resin is selected from one or more of polyurethane resin (PU resin), epoxy resin, methyl silicone resin, polymethyl methacrylate and acrylic resin. It is understandable that the present application has no special requirements for the molecular weight of the organic resin, and any of the organic resins disclosed in the prior art may be used.
[0083] In the present application, the silane coupling agent is used as a surfactant to improve the dispersibility of the modified silica particles in the suspension and promote better bonding between the modified silica particles and the organic resin. The present application does not specifically limit the type of the above-mentioned silane coupling agent, and specifically can be selected from one or more of 3-(methacryloyloxy)propyltrimethoxysilane (γ-MPS), 3-aminopropyltriethoxysilane (APTES), 3-aminopropyltrimethoxysilane (APTMS) and vinyltrimethoxysilane (VTMS).
[0084] In some embodiments, in the above suspension, the mass ratio of the modified silica particles to the organic resin is 1:(2.5-3.5), and the mass ratio of the silane coupling agent to the organic resin is 1:(80-120).
[0085] The purpose of the present application is to prepare a solid block super-hydrophobic material with super-hydrophobicity and high mechanical strength. It is found that when the solid content of modified silica particles in the slurry is too low, in order to ensure the super-hydrophobicity of the material, it is necessary to add a large amount of slurries when the suspension is prepared in the follow-up, and finally the obtained product is a plasticine-like soft material, and a solid block super-hydrophobic material cannot be obtained, so that it meets the application scenario requirements of the super-hydrophobic shell of devices such as electrical equipment. Attempt to increase the amount of modified silica by increasing the super-hydrophobicity of the material, but the inventor of the present application finds that the solid content of modified silica in the slurry is increased or the mass fraction of modified silica in the suspension is increased, although the hydrophobicity of the material can be improved, and a super-hydrophobic material is obtained, but the difficulty of manufacturing is also increased at the same time, and modified silica and organic resin cannot be effectively mixed, and the interfacial strength of the hydrophobic material is low, and a predetermined hardness cannot be reached.
[0086] In some embodiments, step S3 includes the following steps:
[0087] The suspension is subjected to degassing, solidification, compression molding, and post-solidification treatments to obtain a solid block super-hydrophobic material.
[0088] In some embodiments, the specific operation of removing bubbles is: placing the suspension in a mold with air holes, and evacuating the air bubbles, wherein the vacuum degree is -0.09MPa to 0.01MPa, and the evacuation time is 25min to 35min.
[0089] In some embodiments, the curing temperature is 90°C to 100°C, and the curing time is 16h to 20h. This is because when the curing temperature is low, the curing speed is slow, and the obtained product is a soft material like plasticine, and a solid block super-hydrophobic material cannot be obtained; when the curing temperature is high, the curing speed of the material is not significantly improved, and the super-hydrophobic performance of the solid block super-hydrophobic material deteriorates.
[0090] In some embodiments, the pressure of the pressing molding is 4 MPa to 6 MPa, the purpose of which is to form a bulk material and increase the interface bonding between the modified silica particles and the organic resin matrix.
[0091] In some embodiments, the post-curing temperature is 140° C. to 160° C., and the post-curing time is 3 h to 5 h, in order to further enhance the mechanical strength of the superhydrophobic material.
[0092] While adjusting the solid content of modified silica in the slurry, the present application coordinately controls the mass ratio, curing temperature and time, etc. between the modified silica, organic resin and silane coupling agent in the suspension, thereby preparing a solid block superhydrophobic material while improving the hydrophobic properties, interface strength and mechanical stability of the solid block superhydrophobic material, making it suitable for superhydrophobic shells of devices such as power equipment.
[0093] The present application also provides a solid block superhydrophobic material prepared according to the above preparation method.
[0094] The application also provides the application of the above-mentioned solid block super-hydrophobic material in the super-hydrophobic shell of the device for preparing.The solid-state super-hydrophobic material provided by the application can be applied to various device surfaces, including but not limited to power equipment.The application does not limit the application mode of the above-mentioned solid block super-hydrophobic material, for example, the solid block super-hydrophobic material can be fixed to the device surface by a binder to form a super-hydrophobic shell, and the solid block super-hydrophobic material can also be fixed to the device surface by using a fixture to form a super-hydrophobic shell, and versatility is strong, which is beneficial to the wide application of products.
[0095] Based on this, the present application also provides a super-hydrophobic shell comprising the above-mentioned solid block super-hydrophobic material.
[0096] It is understandable that the present application does not limit the shape and thickness of the super-hydrophobic shell. In practical applications, technicians with the skill in the art can select a suitable shape and thickness according to actual needs.
[0097] In some embodiments, the thickness of the super hydrophobic shell is 5 mm to 30 mm.
[0098] In a preferred embodiment, the thickness of the super hydrophobic shell is 10 mm to 20 mm.
[0099] The above technical solutions are described in detail below in conjunction with specific embodiments. It should be understood that these are merely exemplary and are not intended to limit the present application. Materials identical or similar to the types, models, qualities, properties or functions of the following reagents and instruments can be used to implement the present application. The experimental methods used in the following embodiments are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following embodiments, unless otherwise specified, can all be obtained from commercial sources.
[0100] The following are examples and comparative examples:
[0101] Example 1
[0102] The method for preparing a solid block super-hydrophobic material provided in the embodiment of the present application comprises the following steps:
[0103] Tetraethyl orthosilicate (TEOS) was selected as the main precursor material (silicon source compound) and silicon tetrachloride (STC) was selected as the auxiliary silicon source compound. The purity of the above reagents was 99.9%.
[0104] Under nitrogen protection, 100mL TEOS, 1.3L anhydrous ethanol, 200mL ammonia and 300mL deionized water were mixed (the pH value of the reaction system was 7.5), stirred at 35°C for 2h, and then 5mL STC was slowly added and stirred for 3h to complete the hydrolysis and condensation reaction. The reaction solution was then centrifuged using a centrifuge, with the centrifugal speed set to 10000rpm and the centrifugal time set to 20min. The precipitate obtained by centrifugation was then washed with deionized water and anhydrous ethanol for a total of 3 times to remove unreacted raw materials and by-products. Finally, the washed precipitate was dried at 65°C for 24h to obtain nano-silica particles with a particle size range of 130nm to 170nm and an average particle size of 150nm.
[0105] S1. Mix the above-mentioned nano-silica particles and anhydrous ethanol, and use an ultrasonic processor to ultrasonically treat for 40 minutes to enhance the dispersibility of the particles to obtain a dispersion of silica particles. Mix the fluoroalkyl compound (HFOTES) and ethanol in a mass ratio of 0.5:1 to form a uniform modifier solution, and then slowly add it to the dispersion of the above-mentioned silica particles at a rate of 5mL / min, and stir at 50°C for 4h to ensure that the modifier (fluoroalkyl compound) is in full contact and reaction with the nano-silica particles to form a stable low surface energy coating, and obtain a reaction solution containing modified silica particles. The modified silica particles were characterized using an X-ray photoelectron spectrometer (XPS). Figure 2 It can be seen that the characteristic absorption peak of CF bond appears on the surface of modified silica particles, indicating that HFOTES reacts with the surface of silica nanoparticles to form fluoroalkyl groups with low surface energy on the surface of silica particles.
[0106] S2. The reaction solution obtained in step S1 is placed in a 50°C water bath for evaporation and thickening treatment, and the evaporation time is 2.5 hours. The solid content of the slurry obtained by evaporation is measured by sampling and drying to constant weight. The results show that the solid content of the modified silica particles in the slurry is 22%. PU resin (molecular weight 88, product model F0401, purchased from Shenzhen Yoshida Chemical Co., Ltd.) is dissolved in acetone to obtain a PU resin dispersion, and then the above slurry, PU resin dispersion and silane coupling agent (3-(methacryloyloxy)propyltrimethoxysilane) are mixed uniformly under stirring conditions according to the mass ratio of modified silica particles to PU resin of 1:3 and the mass ratio of silane coupling agent to PU resin of 1:100 to obtain a suspension.
[0107] S3, place the above suspension in a square mold with air holes, use a vacuum pump to evacuate and remove bubbles, wherein the vacuum degree is -0.09Mpa, and the vacuuming time is 30min to ensure that the bubbles in the suspension are completely removed. Then place it in a 95℃ vacuum oven for curing for 18h, and then press it under a pressure of 5Mpa to obtain a formed block material with a Shore hardness of 70. Finally, place the above block material in a 150℃ vacuum oven for post-curing treatment for 4h to obtain a solid block superhydrophobic material with a Shore hardness of 85 ( Figure 3 ).
[0108] Testing the super-hydrophobic properties of the solid block super-hydrophobic material provided in the embodiment of the present application:
[0109] The solid block superhydrophobic material is cut into appropriate sizes, cleaned with deionized water and dried, and then the water contact angles of different surfaces are measured using a contact angle meter, and the rolling angle is measured using a rolling angle meter to evaluate the hydrophobic properties of the solid superhydrophobic material. According to the Cassie-Baxter model, when the contact angle between the material surface and water is greater than 150° and the rolling angle is less than 10°, the material is considered to be superhydrophobic.
[0110] The test results show that ( Figure 4 ), the solid block superhydrophobic material prepared in the embodiment of the present application has a contact angle with water of 151.113° and a rolling angle of 3.0°, and has excellent superhydrophobic properties.
[0111] Example 2
[0112] The method for preparing a solid block super-hydrophobic material provided in the embodiment of the present application comprises the following steps:
[0113] Tetraethyl orthosilicate (TEOS) was selected as the main precursor material (silicon source compound) and trichloromethylsilane (MTMS) was selected as the auxiliary silicon source compound. The purity of the above reagents was 99.9%.
[0114] Under the protection of helium gas, 100mL TEOS, 1.4L anhydrous ethanol, 175mL ammonia water and 250mL deionized water were mixed (the pH value of the reaction system was 8), stirred at 35°C for 1.5h, and then 2.5mL MTMS was slowly added and stirred for 4.5h to complete the hydrolysis and condensation reaction. Then the reaction solution was centrifuged using a centrifuge, the centrifugal speed was set to 8000rpm, and the centrifugal time was 30min. Then the precipitate obtained by centrifugation was washed with deionized water and anhydrous ethanol for a total of 5 times to remove unreacted raw materials and by-products. Finally, the washed precipitate was dried at 50°C for 48h to obtain nano-silica particles with a range of 140nm to 180nm and an average particle size of 160nm.
[0115] S1. Mix the above-mentioned nano-silica particles and anhydrous ethanol, and use an ultrasonic processor to ultrasonically treat for 30 minutes to enhance the dispersibility of the particles to obtain a dispersion of silica particles. Mix the fluoroalkyl compound (TEFS) and anhydrous ethanol in a mass ratio of 1:1 to form a uniform modifier solution, and then slowly add it to the dispersion of the above-mentioned silica particles at a rate of 10mL / min, and stir at 60°C for 3h to ensure that the modifier (fluoroalkyl compound) is fully in contact with the nano-silica particles and fully reacts to form a stable low surface energy coating to obtain a reaction solution containing modified silica particles.
[0116] S2, the reaction solution obtained in step S1 is placed in a 48 ° C water bath for evaporation thickening treatment, and the evaporation time is 3h. The solid content of the slurry obtained by evaporation is measured by sampling and drying to constant weight. The result shows that the solid content of the modified silica particles in the slurry is 25%. The epoxy resin (product model is E44, purchased from Hunan Yuehua Chemical Co., Ltd.) is dissolved in acetone to obtain an epoxy resin dispersion, and then under stirring, the above-mentioned slurry, epoxy resin dispersion and silane coupling agent (3-aminopropyl triethoxysilane) are mixed uniformly according to the mass ratio of modified silica particles to epoxy resin of 1:2.5 and the mass ratio of silane coupling agent to epoxy resin of 1:120 to obtain a suspension.
[0117] S3, place the above suspension in a square mold with air holes, use a vacuum pump to evacuate and remove bubbles, wherein the vacuum degree is 0.01Mpa, and the vacuuming time is 25min to ensure that the bubbles in the suspension are completely removed. Then place it in a 90℃ vacuum oven for curing for 20h, and then press it under a pressure of 4Mpa to obtain a formed block material with a Shore hardness of 65. Finally, place the above block material in a 160℃ vacuum oven for post-curing treatment for 3h to obtain a solid block superhydrophobic material with a Shore hardness of 80 ( Figure 3 ).
[0118] The superhydrophobic performance test results of the solid block superhydrophobic material show that the solid block superhydrophobic material prepared in the embodiment of the present application has a contact angle with water of 151.0° and a rolling angle of 3.5°, and has excellent superhydrophobic performance.
[0119] Example 3
[0120] The method for preparing a solid block super-hydrophobic material provided in the embodiment of the present application comprises the following steps:
[0121] Tetraethyl orthosilicate (TEOS) was selected as the main precursor material (silicon source compound) and silicon tetrachloride (STC) was selected as the auxiliary silicon source compound. The purity of the above reagents was 99.9%.
[0122] Under the protection of argon gas, 100mL TEOS, 1.2L anhydrous ethanol, 225mL ammonia water and 350mL deionized water were mixed (the pH value of the reaction system was 7.5), placed at 35°C and stirred for 2.5h, 7.5mL STC was slowly added, and stirring was continued for 1.5h to complete the hydrolysis and condensation reaction. Then the reaction solution was centrifuged using a centrifuge, the centrifugal speed was set to 12000rpm, and the centrifugal time was 10min. Then the precipitate obtained by centrifugation was washed with deionized water and anhydrous ethanol for a total of 3 times to remove unreacted raw materials and by-products. Finally, the washed precipitate was dried at 80°C for 12h to obtain nano-silica particles with a particle size range of 120nm to 160nm and an average particle size of 140nm.
[0123] S1. Mix the above-mentioned nano-silica particles and anhydrous ethanol, and use an ultrasonic processor to ultrasonically treat for 50 minutes to enhance the dispersibility of the particles to obtain a dispersion of silica particles. Mix the fluoroalkyl compound (PFOS) and anhydrous ethanol in a mass ratio of 1.5:1 to form a uniform modifier solution, and then slowly add it to the dispersion of the above-mentioned silica particles at a rate of 3mL / min, and stir at 40°C for 5h to ensure that the modifier (fluoroalkyl compound) is fully in contact with the nano-silica particles and fully reacts to form a stable low surface energy coating to obtain a reaction solution containing modified silica particles.
[0124] S2. The reaction solution obtained in step S1 is placed in a 52°C water bath for evaporation and thickening treatment, and the evaporation time is 2h. The solid content of the slurry obtained by evaporation is measured by sampling and drying to constant weight. The results show that the solid content of the modified silicon dioxide particles in the slurry is 20%. Methyl silicone resin (product model 077, purchased from Shandong Ruderui New Materials Co., Ltd.) is dissolved in acetone to obtain a methyl silicone resin dispersion, and then the above slurry, methyl silicone resin dispersion and silane coupling agent (3-aminopropyltriethoxysilane) are mixed under stirring according to the mass ratio of modified silicon dioxide particles to methyl silicone resin of 1:3.5 and the mass ratio of silane coupling agent to methyl silicone resin of 1:80, and a suspension is obtained.
[0125] S3, place the above suspension in a square mold with air holes, use a vacuum pump to evacuate and remove bubbles, wherein the vacuum degree is -0.09Mpa, and the vacuuming time is 35min to ensure that the bubbles in the suspension are completely removed. Then place it in a 100℃ vacuum oven for curing for 16h, and then press it under a pressure of 6Mpa to obtain a formed block material with a Shore hardness of 75. Finally, place the above block material in a 140℃ vacuum oven for post-curing treatment for 5h to obtain a solid block superhydrophobic material with a Shore hardness of 85 ( Figure 3 ).
[0126] The superhydrophobic performance test results of the solid bulk superhydrophobic material show that the solid bulk superhydrophobic material prepared in the embodiment of the present application has a contact angle with water of 151.2° and a rolling angle of 3.3°, and has excellent superhydrophobic performance.
[0127] Comparative Example 1
[0128] In step S2, the evaporation time is 1 hour, the solid content of the modified silicon dioxide particles in the slurry is 10%, and the other operations are the same as those in Example 1. The hydrophobic material finally obtained is a soft material like plasticine, and a solid block superhydrophobic material cannot be obtained.
[0129] Comparative Example 2
[0130] In step S2, the evaporation time is 1 h, the solid content of the modified silica particles in the slurry is 40%, and the other operations are the same as in Example 1. It was found during the experiment that the slurry was difficult to disperse, which resulted in increased production difficulty and production cost in actual production. At the same time, the interface strength of the hydrophobic material obtained was low, and the Shore hardness was 55.
[0131] Comparative Example 3
[0132] In step S2, the PU resin dispersion and the slurry are mixed according to a mass ratio of modified silica particles to PU resin of 1:4, and other operations are the same as those in Example 1.
[0133] The superhydrophobic performance test results show that the contact angle of the prepared hydrophobic material with water is 110.0°, and the hydrophobic performance is poor.
[0134] Comparative Example 4
[0135] In step S2, the PU resin dispersion was mixed with the slurry in a mass ratio of modified silica particles to PU resin of 1:2, and other operations were the same as those in Example 1. The interface strength of the hydrophobic material finally obtained was low, with a Shore hardness of 50, which could not reach the predetermined hardness.
[0136] Comparative Example 5
[0137] In step S3, the curing temperature is 70° C., and other operations are the same as those in Example 1. The hydrophobic material finally obtained is a soft material like plasticine.
[0138] Comparative Example 6
[0139] In step S3, the curing temperature is 150°C, and other operations are the same as those in Example 1. The color of the hydrophobic material finally obtained is darker, and the super hydrophobic performance test results show that the contact angle of the hydrophobic material with water is 105°, and the hydrophobic performance is poor.
[0140] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A method for preparing a solid block superhydrophobic material, It is characterized in that The steps include: S1, mixing a silica dispersion obtained by mixing silica particles and a solvent with a fluoroalkyl compound solution, so that the fluorine atoms in the fluoroalkyl compound solution replace the hydroxyl groups on the surface of the silica particles, and perform low surface energy modification to obtain a reaction solution containing modified silica particles; S2, mixing and stirring the slurry obtained by evaporating the reaction solution, the organic resin solution, and the silane coupling agent to form a suspension; S3, degassing, solidifying, pressing and post-curing the suspension to obtain a solid block super-hydrophobic material.
2. The preparation method according to claim 1, It is characterized in that In step S1, the particle size of the silicon dioxide particles is 50 nm to 300 nm; and / or, The fluoroalkyl compound solution is prepared by mixing a fluoroalkyl compound with a solvent, and the fluoroalkyl compound is selected from one or more of perfluorooctyltriethoxysilane, triethoxyfluorosilane, perfluorooctane sulfonic acid, perfluorobutylethyltriethoxysilane, perfluoroethylvinyl ether and perfluorohexylvinyl ether.
3. The preparation method according to claim 1 or 2, It is characterized in that The method for preparing silicon dioxide particles comprises the following steps: in a protective atmosphere, a silicon source compound, an alcohol solvent, an alkaline environment regulator, deionized water and an auxiliary silicon source compound are mixed, stirred, centrifuged, washed and dried to obtain silicon dioxide particles.
4. The preparation method according to claim 3, It is characterized in that The silicon source compound is a silanol compound, selected from at least one of ethyl orthosilicate, propyl orthosilicate and tetraethoxysilane; and / or, The auxiliary silicon source compound is selected from at least one of silicon halide hydrocarbons and trihalosilanes; and / or, The volume ratio of the silicon source compound to the auxiliary silicon source compound is 1:(0.025-0.075); and / or, The stirring temperature is 20° C. to 40° C., and the stirring time is 4 h to 6 h.
5. The preparation method according to claim 1, It is characterized in that In step S2, the solid content of the modified silicon dioxide particles in the slurry is 15% to 30%; and / or, The organic resin solution is formed by mixing an organic resin and an organic solvent, wherein the organic resin is selected from one or more of polyurethane resin, epoxy resin, methyl silicone resin, polymethyl methacrylate and acrylic resin; and / or, The silane coupling agent is selected from one or more of 3-(methacryloyloxy)propyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane and vinyltrimethoxysilane; and / or, In the suspension, the mass ratio of the modified silica particles to the organic resin is 1:(2.5-3.5).
6. The preparation method according to claim 1, It is characterized in that In step S3, the specific operation of removing bubbles is: placing the suspension in a mold with air holes, and evacuating the air bubbles, wherein the vacuum degree is -0.09MPa to 0.01MPa, and the evacuation time is 25min to 35min.
7. The preparation method according to claim 1, It is characterized in that In step S3, the curing temperature is 90° C. to 100° C., and the curing time is 16 h to 20 h; and / or, The compression molding pressure is 4MPa to 6MPa; and / or, The post-curing temperature is 140° C. to 160° C., and the post-curing time is 3 h to 5 h.
8. A solid block superhydrophobic material prepared according to the preparation method according to any one of claims 1 to 7.
9. Use of the solid block superhydrophobic material according to claim 8 in preparing a superhydrophobic shell of a device.
10. A superhydrophobic shell comprising the solid bulk superhydrophobic material of claim 8.
Citation Information
Patent Citations
Epoxy resin composition for moisture-resistant molding compound and preparation method
CN111087763A
High-strength stretchable super-hydrophobic polyamide-imide composite film and preparation method thereof
CN115368613A
Pressure-induced infiltration state and shape-controllable super-hydrophobic silicone rubber elastomer and preparation method thereof
CN118254315A
Method for surface-treating of mesoporous silica, and method for producing slurry composition for adding to resin, filler for resin and resin composition
JP2009190909A