Solid clay stabilizer and preparation method thereof
Through the preparation method of solid clay stabilizer, a coordination polymer of metal ions and organic cations is used to form an adsorption layer to prevent the hydration expansion and dispersion migration of clay, which solves the problem of poor selectivity and synthesis process of clay stabilizer in the existing technology. Complex problems have been achieved to effectively protect oil and gas reservoirs and improve development efficiency.
Patent Information
- Application Number
- CN202410982633.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-15
AI Technical Summary
Existing clay stabilizers have problems with poor selectivity, complex synthesis processes, poor erosion resistance, and poor timeliness during oil field water injection, acidification, and fracturing processes, resulting in reduced reservoir permeability and easy hydration, expansion, and dispersion of clay. transport.
The preparation method of solid clay stabilizer is adopted, by mixing the prefabricated base material, ammonium salt and organic aluminum in proportion, adding hydrocarbon halides, oxygen-containing heterocyclic compounds and modifying reagents, and then recrystallizing and drying to form a double stabilizer. Composite polymer hybrid materials in the active field utilize coordination polymers of metal ions and organic cations to form an adsorption layer to prevent clay from hydrating, swelling and dispersing.
It effectively protects the permeability of clay in oil and gas reservoirs, improves the stability and development efficiency of clay, significantly inhibits the hydration expansion and dispersion migration of clay, and has good anti-swelling performance, water resistance and salt resistance.
Smart Images

Figure SMS_13 
Figure SMS_14 
Figure SMS_15
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of stabilizers, and in particular relates to a solid clay stabilizer and a preparation method thereof. Background Art
[0002] During the development process of oil field water injection, acidification, fracturing, etc., minerals such as kaolinite, montmorillonite, chlorite, etc. contained in the oil reservoir are prone to hydration expansion and dispersed migration when encountering external water or water-based substances, which leads to blockage of pore throats, reduces soil permeability, and causes damage to the reservoir.
[0003] The clay stabilizers used in the prior art are mainly divided into inorganic salt clay stabilizers and organic polymer clay stabilizers. Inorganic salt clay stabilizers have the advantages of low cost and easy use, but they are not resistant to erosion and have poor timeliness. They can only temporarily stabilize the clay and are prone to lose stability when the external environment changes. The Na in the formation water + Re-ion exchange to the initial water-sensitive state, and because it cannot produce multi-point adsorption similar to polymers. Organic polymer clay stabilizers can hydrolyze positively charged high molecular cations, which can replace low-valent cations on the surface of adsorbed particles. In addition, there are hydrogen bonds and intermolecular forces between organic polymers and clay particles, which can form a protective layer on the surface of clay particles, neutralizing the surface charge of clay, isolating water and clay particles, and preventing clay particles from swelling and migration. It has the characteristics of low dosage and high adsorption. At the same time, organic polymer clay stabilizers are less affected by environmental pH and can be applied to a variety of formations. However, there are technical problems in the technical solution, such as poor selectivity of stabilizers and complex synthesis processes. Summary of the invention
[0004] The technical solution of the present invention aims at solving the technical problems such as poor selectivity of stabilizers and complex synthesis process, and provides a solid clay stabilizer and a preparation method thereof.
[0005] The main purposes of the present invention are: 1. To provide permeability protection measures for oil and gas reservoir clay.
[0006] 2. Effectively ensure the safety and stability of oil and gas reservoir clay.
[0007] 3. Improve the efficiency level of clay development and utilization in oil and gas reservoirs.
[0008] To achieve the above objectives, the present invention adopts the following technical solutions.
[0009] A method for preparing a solid clay stabilizer comprises: (1) uniformly mixing a prefabricated substrate, an ammonium salt and an organic aluminum in proportion to prepare the substrate.
[0010] (2) The base material, hydrocarbon halide, oxygen-containing heterocyclic compound and modifying agent are mixed uniformly in proportion to prepare a crude product, which is then recrystallized and dried to obtain a solid clay stabilizer.
[0011] Preferably, the prefabricated substrate in step (1) contains polyacrylamide and allyltrimethylammonium chloride; the content of allyltrimethylammonium chloride in the prefabricated substrate is 0.1-0.3 wt %, and the balance is polyacrylamide.
[0012] The ammonium salt in step (1) is methacryloyloxyethyl trimethylammonium chloride.
[0013] The organic aluminum in step (1) is aluminum trifluoromethanesulfonate.
[0014] Preferably, in step (1), the prefabricated substrate, ammonium salt and organic aluminum are uniformly mixed in a mass ratio of 8:(1-3):(3-5).
[0015] Preferably, the process for preparing the substrate in step (1) is as follows: adding the prefabricated substrate, ammonium salt and organoaluminum to a solvent, stirring for 1 to 3 hours at a temperature of 75 to 80 °C and a rotation speed of 200 to 300 r / min, then adding an initiator at room temperature, and continuing stirring for 3 to 5 hours; wherein: the solvent is deionized water or distilled water; the initiator is ammonium persulfate, and the amount of the initiator used is 0.1 to 0.3 wt% of the prefabricated substrate.
[0016] Preferably, the hydrocarbon halide in step (2) is 1,7-dibromoheptane.
[0017] The oxygen-containing heterocyclic compound in step (2) is pyridine.
[0018] Preferably, the method for preparing the modifying reagent in step (2) is as follows: N, N, N-trimethyloctadecane-1-ammonium iodide, N, N-dimethylformamide and potassium iodide are uniformly mixed in a mass ratio of 3: (1.3-1.7): (2-2.5), and acetonitrile is used as a solvent to prepare a modifying agent; the amount of acetonitrile used is 2.5-3.5 times the volume of N, N-dimethylformamide.
[0019] Preferably, in step (2), the substrate, hydrocarbon halide, oxygen-containing heterocyclic compound and modifying agent are uniformly mixed in a mass ratio of 5: (1.8-2.2): (1.4-1.6): 3.
[0020] Preferably, the crude product prepared in step (2) is stirred and reacted at a temperature of 80 to 90° C. for 8 to 12 hours.
[0021] Preferably, the recrystallization in step (2) is performed using diethyl ether and methanol in sequence.
[0022] A solid clay stabilizer.
[0023] The solid clay stabilizer provided in the scheme of the present invention transmits the structural information of the organic structure to the inorganic skeleton through the synergistic interaction between the interfaces of inorganic molecules and organic components, thereby forming a twin active field and obtaining a composite polymer hybrid material with a special structure.
[0024] In the technical solution of the present invention, the core lies in that metal ions and organic cations can have highly regular coordination polymer materials under certain conditions. In the technical solution of the present invention, affinity is particularly reflected at the interface between the polar group and the oil phase, and the adsorption of the twin active domain at the interface is regulated. First, the constraint effect produced by the linking group, and secondly, the stabilizer molecule shows overall affinity at the interface. When the constraint effect is dominant, the twin center is connected at the interface in a linear or nearly linear adsorption mode; when the affinity effect is relatively strong, the twin center will be adsorbed at the interface position in a curved or irregular ring form.
[0025] In the technical solution of the present invention, there is a special amphiphilic molecular structure on the stabilizer group. The hydrophilic group makes the stabilizer have a natural tendency to move toward the inside of the water system. At the same time, the stabilizer also has a hydrophobic group, which tends to migrate from the inside to the outside. When the interaction generated by the two groups reaches equilibrium, the stabilizer will be enriched inside the water system, wherein the hydrophilic group extends into the water system and the hydrophobic group extends into the air. The resulting macroscopic phenomenon is that the stabilizer is dispersed inside the system and constructs a monolayer with an adsorption effect. When the adsorption of the stabilizer reaches saturation, the stabilizer will no longer continue to be enriched, and the hydrophobic effect of the hydrophobic group will still prompt the stabilizer to self-polymerize, that is, after the adsorption of the stabilizer is saturated, the hydrophobic group self-polymerizes to form a core. The clay stabilizer provided by the technical solution of the present invention can ionize cationic groups after being dissolved in the solution system. At this time, the organic cations exchange and adsorb with the cations on the mineral clay, and exchange the ions that undergo hydration and expansion on the clay for cations that are not easy to hydrate and expand, and adsorb to the surface of the clay particles. At the same time, the organic chain can penetrate into the mineral clay crystal layers, and construct an adsorption layer with hydrophobic properties, so that the surface of the clay particles is hydrophobically modified, resulting in the weakening of the wetting ability of water molecules between the mineral clay, and it is difficult for water molecules to enter between the clay crystal layers, resulting in the hydration and expansion of the clay and the dispersion and migration being inhibited. At the same time, the cations generated by ionization are adsorbed on the surface of the mineral clay particles and free from the negative charge generated by friction, reducing the repulsion between the crystal layers, further stabilizing the clay particles, and preventing hydration and expansion and dispersion. As the stabilizer adsorption reaches saturation, the organic polymer long chain is driven by the hydrophobic group, so that the interaction between the stabilizer and the clay removes the electrostatic effect, and also includes a stronger van der Waals force. The organic polymer long chain can also effectively block other smaller cations from entering the adsorption center, enhancing the stability of the saturated stabilizer system.
[0026] In the technical solution of the present invention, the solid clay stabilizer can be used as a positively charged macromolecular chain that can produce a strong interaction with clay mineral particles. After encountering water, the organic molecular chain is electrolyzed to produce numerous positively charged groups and electrostatic attraction between the negatively charged centers. More importantly, the stabilizer forms an adsorption zone on the surface of the adsorbed clay mineral particles. During the formation of the adsorption zone, the organic long chain can be adsorbed with multiple particle grain boundaries, construct multiple adsorption sites, generate extremely strong intermolecular forces, strengthen the stability of the system formed after the stabilizer is saturated and adsorbed, and make the stabilizer have extremely strong chemical stability during use. In addition, when multiple saturated adsorption systems are close to each other, the adsorption zones overlap under the effect of like charges repelling each other, forming a thin double electric layer at the interface between the two, squeezing the adsorbed particles and compressing the particle space, so that the clay mineral particles are tightly combined and not easy to expand when encountering water.
[0027] In the technical solution of the present invention, ammonium persulfate is selected as an initiator, the reaction conditions are reduced during the polymerization reaction, the occurrence of side reactions is effectively reduced in a mild polymerization environment, and the purity and performance stability of the substrate are guaranteed. In addition, if the polymer has a link decomposition, it will lead to a decrease in molecular weight and performance degradation. In the present invention, ammonium persulfate only acts as an initiator and will not have a negative impact on the polymer chain. Polymer chain transfer and branching are key factors affecting the polymer structure, and the residual ammonium persulfate has a negligible effect on the branching and transfer effects of the polymer long chain, ensuring that the polymer has an ideal molecular structure and excellent performance. In summary, the initiator has the advantages of mild polymerization conditions, does not participate in inducing polymer decomposition, and does not affect product chain transfer and branching.
[0028] In the present invention, a special modification agent is proposed and prepared. After the substrate is modified, there are three types of structural groups, hydrophobic groups, ionic head groups, and linking groups, to construct a twin active center. The special property of the active center is that the linking group and the hydrophobic bond work together. When the linking group of the twin active center is a flexible hydrophilic group, the critical micelle concentration of the system is the smallest; when the linking group is a flexible hydrophobic group, the critical micelle concentration of the system is slightly higher. The reason for this phenomenon is that the hydrophilic linking group is easy to form hydrogen bonds, and the flexible carbon chain in the material makes the group as a whole shift toward the water phase to form a micelle surface, increase the average occupied area of the modification agent for the substrate molecules at the interface, strengthen the connection of the amphiphilic molecules through the chemical bond of the linking group, and can play a role in dispersion, wetting and chelation during the use of the stabilizer, especially in the water environment.
[0029] In the present invention, metal ions and organic cations can form coordination polymers, wherein the pyridine ligands coordinate with the metal ions in a protonated form in a bidentate structure, and the coordination structure forms a coordination empty orbital, which is beneficial for the protons to form reverse diffusion during the diffusion process, and becomes an adhesive connecting the mineral ions and the organic ligands, and forms a transfer carrier. In clay minerals, due to the abnormal activity of metal cations, the transfer carrier in the present invention is static in the water system, and the metal cations can jump along the hydrogen bonds through the infinite hydrogen bond network and move between the carrier molecules, thereby strengthening the chelation effect of the stabilizer. By intentionally regulating the properties of the spacer group between the iodinated metal and the functional ligand on the ligand, the spatial structure of the resulting coordination polymer can be adjusted. At higher relative humidity, the spatial structure only weakly interacts with the nitrogen atoms in the ligand. In a disordered water molecule environment, the water molecules can act as temporary carriers to guide the cations to jump and shorten the saturation time of the stabilizer.
[0030] The solid clay stabilizer prepared by the present invention is mainly composed of a polymer, the polymer has a large cationic degree, has a unique rigid structure, can enter the interlayer of clay minerals, and under the interaction of electrostatic action and chemical bonds, obviously plays a role in preventing the hydration expansion and dispersion migration of clay minerals in the reservoir, and plays a role in clay stabilization and anti-swelling. In addition, under the dissolution of water molecules, the clay stabilizer can precipitate positively charged groups with a high positive charge density from the solution, and exchange reactions with high-valent cations on the clay surface. In this process, the huge attraction of the electrostatic effect causes the positively charged groups to be adsorbed on the clay surface, and then produces a neutralization effect with the negative charge, reduces the electrostatic repulsion, and further inhibits the hydration expansion of the clay.
[0031] The advantages of the present invention are: the present invention protects the clay of the oil and gas reservoir through the synergistic effect of the organic cationic polymer and the inorganic molecules, and improves the working efficiency of the stabilizer to improve the development efficiency of the oil and gas layer. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0033] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.
[0034] Example 1: A method for preparing a solid clay stabilizer, the method comprising: (1) uniformly mixing polyacrylamide and allyltrimethylammonium chloride in a mass ratio of 99.9:0.1 to obtain a prefabricated substrate.
[0035] (2) The prefabricated substrate, methacryloyloxyethyl trimethylammonium chloride and aluminum trifluoromethanesulfonate were mixed uniformly in a mass ratio of 8:1:3 and a solvent was added, and the mixture was stirred at a temperature of 75 °C and a rotation speed of 200 r / min for 3 h. Subsequently, an initiator was added at room temperature, and the mixture was stirred for 5 h. The mixture was filtered and dried to obtain a substrate, wherein the solvent in the substrate preparation process was deionized water, and the amount used was 20 mL deionized water / 0.01 g aluminum trifluoromethanesulfonate. The initiator was ammonium persulfate, and the amount used was 0.1 wt% of the prefabricated substrate.
[0036] (3) N, N, N-trimethyloctadecane-1-ammonium iodide, N, N-dimethylformamide and potassium iodide were uniformly mixed in a mass ratio of 3:1.3:2, and acetonitrile with a volume of 3 times that of N, N-dimethylformamide was used as a solvent to prepare a modifier.
[0037] (4) The substrate, 1,7-dibromoheptane, pyridine and modification reagent were mixed uniformly in a mass ratio of 5:1.8:1.4:3, and stirred for reaction at 80 °C for 12 h to prepare a crude product, which was recrystallized using ether and methanol in sequence and dried to obtain a solid clay stabilizer.
[0038] The solid clay stabilizer prepared in the example was subjected to performance testing, and the specific characterization results are as follows.
[0039] Anti-swelling performance test: 3.00 g of bentonite was accurately weighed and placed in a 50 mL centrifuge tube, 0.05 g of the clay stabilizer prepared in the example was added, the volume was fixed with deionized water, the mixture was fully shaken, and the mixture was stored at room temperature for 2 h. The mixture was placed in a centrifuge and centrifuged at a speed of 1500 r / min for 15 min. The volume of the bentonite after swelling was read. .
[0040] Repeat the above steps, replacing the clay stabilizer with 50 mL of water, and measure the swelling volume of bentonite in water. .
[0041] Repeat the above steps, replace the clay stabilizer with 50 mL of kerosene, and measure the swelling volume of bentonite in kerosene. .
[0042] The anti-swelling property of clay stabilizer is calculated according to the following formula: .
[0043] Where: B is the anti-swelling rate of clay stabilizer, %.
[0044] ——The expansion volume of bentonite in kerosene, mL.
[0045] ——Expansion volume of bentonite in clay stabilizer, mL.
[0046] ——Expansion volume of bentonite in water, mL.
[0047] Water resistance evaluation: 1. Accurately weigh 3.00 g of bentonite, put it into a 50 mL centrifuge tube, add 0.06 g of the clay stabilizer prepared in Example, use deionized water to make up the volume, shake it well, let it stand at room temperature for 2 h, put it into a centrifuge, and centrifuge it at a speed of 1500 r / min for 15 min; 2. Discard the supernatant, use deionized water to make up the volume, shake it well and let it stand for 2 h, put it into a centrifuge, and centrifuge it at a speed of 1500 r / min for 15 min; 3. Repeat 2 operations twice and read the expansion volume of bentonite in water , and the water resistance of clay stabilizer is calculated using the following formula: .
[0048] Where: W——water resistance of clay stabilizer, %.
[0049] ——Expansion volume of bentonite in clay stabilizer, mL.
[0050] ——Expansion volume of bentonite in water, mL.
[0051] ——The expansion volume of bentonite after washing, mL.
[0052] Critical micelle concentration detection: Prepare a series of clay stabilizer solutions (0.01-10 μg / mL) and add an equal amount of pyrene to make the final concentration of pyrene 6.0×10 -7 mol / L, the sample was shaken at 37 °C and 30 rpm for 1 h, kept away from light for 8 h, and the critical micelle concentration was detected using a fixed emission wavelength of 390 nm and a scanning wavelength of 300-350 nm.
[0053]
[0054] From the above characterization results, it can be seen that the clay stabilizer of the present invention has very good anti-swelling performance and water resistance, and can effectively stabilize and protect the clay under the condition of extremely low dosage, producing corresponding effects.
[0055] Temperature resistance test: Referring to the above clay stabilizer evaluation method, the anti-swelling rate of the clay stabilizer solution with the same concentration at 20 ℃, 35 ℃, 50 ℃, 75 ℃, and 90 ℃ was determined. The specific test steps are as follows: 3.00 g bentonite and 0.05 g clay stabilizer were accurately weighed and water was added to 50 mL to mix evenly, and the mixture was placed in a water bath at the required temperature of the test environment for 2 h. After cooling, the anti-swelling rate was tested by centrifugation, and the results were compared. The specific characterization results are as follows.
[0056]
[0057] Salt resistance test: Calcium chloride: magnesium chloride: sodium chloride were mixed in a mass ratio of 3:2:15, and standard saline solutions with different mineralizations (4000, 12000, 24000, 35000, 40000 mg / L) were prepared. A solution with a clay stabilizer concentration of 2.0 wt% was prepared using standard saline solutions of different concentrations as solvents. Referring to the above anti-swelling performance test, 3.00 g of bentonite was placed in a 50 mL centrifuge tube and fixed to volume with a clay stabilizer solution with a concentration of 2.0 wt%. The anti-swelling effect of the clay stabilizer was measured, and the characterization results are as follows.
[0058]
[0059] Analysis of the above characterization results shows that the clay stabilizer prepared in the example has good anti-swelling rate and water resistance, and still has extremely high anti-swelling properties in high temperature and alkaline environments, which shows that the clay stabilizer prepared in the example has good temperature resistance and salt resistance.
[0060] Example 2: A method for preparing a solid clay stabilizer, the method comprising: (1) uniformly mixing polyacrylamide and allyltrimethylammonium chloride in a mass ratio of 99.8:0.2 to obtain a prefabricated substrate.
[0061] (2) The prefabricated substrate, methacryloyloxyethyltrimethylammonium chloride and aluminum trifluoromethanesulfonate were mixed in a mass ratio of 8:2:4 and a solvent was added. The mixture was stirred at 78 °C and 250 r / min for 2 h. Then, an initiator was added at room temperature. The mixture was stirred for 4 h and then filtered and dried to obtain a substrate. The solvent in the substrate preparation process was deionized water, and the amount was 20 mL deionized water / 0.01 g aluminum trifluoromethanesulfonate. The initiator was ammonium persulfate, and the amount was 0.2 wt% of the prefabricated substrate.
[0062] (3) N, N, N-trimethyloctadecane-1-ammonium iodide, N, N-dimethylformamide and potassium iodide were uniformly mixed in a mass ratio of 3:1.5:2.3, and acetonitrile with a volume of 3 times that of N, N-dimethylformamide was used as a solvent to prepare a modifier.
[0063] (4) The substrate, 1,7-dibromoheptane, pyridine and modification reagent were mixed uniformly in a mass ratio of 5:2:1.5:3, and stirred for reaction at 85 °C for 10 h to prepare a crude product, which was recrystallized using ether and methanol in sequence and dried to obtain a solid clay stabilizer.
[0064] The clay stabilizer prepared in the example was subjected to the same performance test as in Example 1, and the specific characterization results are as follows.
[0065]
[0066]
[0067]
[0068] Analysis of the above characterization results shows that the clay stabilizer prepared in the example has good anti-swelling rate and water resistance, and still has extremely high anti-swelling properties in high temperature and alkaline environments, which shows that the clay stabilizer prepared in the example has good temperature resistance and salt resistance.
[0069] Example 3: A method for preparing a solid clay stabilizer, the method comprising: (1) uniformly mixing polyacrylamide and allyltrimethylammonium chloride in a mass ratio of 99.7:0.3 to obtain a prefabricated substrate.
[0070] (2) The prefabricated substrate, methacryloyloxyethyl trimethylammonium chloride and aluminum trifluoromethanesulfonate were mixed in a mass ratio of 8:3:5 and a solvent was added. The mixture was stirred at 80 °C and 300 r / min for 1 h. Then, an initiator was added at room temperature. The mixture was stirred for 3 h and then filtered and dried to obtain a substrate. The solvent in the substrate preparation process was deionized water, and the amount was 20 mL deionized water / 0.01 g aluminum trifluoromethanesulfonate. The initiator was ammonium persulfate, and the amount was 0.3 wt% of the prefabricated substrate.
[0071] (3) N, N, N-trimethyloctadecane-1-ammonium iodide, N, N-dimethylformamide and potassium iodide were uniformly mixed in a mass ratio of 3:1.7:2.5, and acetonitrile with a volume of 3 times that of N, N-dimethylformamide was used as a solvent to prepare a modifier.
[0072] (4) The substrate, 1,7-dibromoheptane, pyridine and modification reagent were mixed uniformly in a mass ratio of 5:2.2:1.6:3, and stirred for reaction at 90 °C for 8 h to prepare a crude product, which was recrystallized using ether and methanol in sequence and dried to obtain a solid clay stabilizer.
[0073] The clay stabilizer prepared in the example was subjected to the same performance test as in Example 1, and the specific characterization results are as follows.
[0074]
[0075]
[0076]
[0077] Analysis of the above characterization results shows that the clay stabilizer prepared in the example has good anti-swelling rate and water resistance, and still has extremely high anti-swelling properties in high temperature and alkaline environments, which shows that the clay stabilizer prepared in the example has good temperature resistance and salt resistance.
[0078] Comprehensive analysis of the test data of Examples 1, 2, and 3 shows that the critical micelle concentration is the concentration when the stabilizer solution begins to form micelles in large quantities. The smaller the test value, the stronger the ability of the stabilizer to aggregate and form micelles. In the technical solution of the present invention, the modified connecting group generates a twin active field, the interaction between organic molecules is enhanced, and the hydrophobic effect of the carbon-hydrogen bond is enhanced. At the same time, the connecting group offsets the electrostatic repulsion effect on the end group of the organic molecule, making it easier for the stabilizer to aggregate and form micelles in an aqueous environment. In addition, in the aqueous system, the two hydrophobic chains of the stabilizer undergo a phase transition (solid phase→liquid phase→micelle phase) at the same time, resulting in a larger free energy transition, thereby reducing the critical micelle concentration value of the stabilizer during use in an aqueous environment. The clay stabilizers prepared in Examples 1, 2, and 3 can maintain a relatively high retention rate after three water washes, which can reflect that the clay stabilizers synthesized in the examples have good water resistance. In addition, Example 3 is subjected to additional performance testing (increasing the concentration of the clay stabilizer). With the increase of the clay stabilizer concentration, the change in the anti-swelling rate after three water washes decreases. Therefore, a higher clay stabilizer can be selected to obtain better water resistance. In view of the limited increase in the anti-swelling rate when the clay stabilizer is used in excessive amounts, it can be added to water in practical applications to prepare a 1.5-3 wt% solution, thereby achieving economy while maintaining the effectiveness of the clay stabilizer. In the salt resistance test of Examples 1, 2, and 3, the overall anti-swelling rate does not change much at the inorganic salt concentration and fluctuates around 94.7%. Due to the strong anionic and hydrophilic functional groups on the organic polymer long chain, it has good water solubility and salt resistance, so that the synthesized quaternary polymer has good salt resistance.
[0079] Comparative Example 1: A method for preparing a solid clay stabilizer. The specific preparation method is the same as that of Example 1. In the comparative example, only the unique substrate of the present invention is changed. An equal amount of polyacrylamide is used to replace the substrate prepared in the unique step (2) to prepare the clay stabilizer. The clay stabilizer prepared in the comparative example is partially tested for performance in the same manner as in Example 1. The characterization results are as follows.
[0080]
[0081]
[0082] Analysis of the above characterization results shows that the clay stabilizer prepared in the comparative example has good temperature resistance, but the anti-swelling rate and water resistance are significantly reduced. After further in-depth research, the anti-swelling performance of a single substrate polymer is poor, its flocculation ability is weak, and the degree of improvement on the overall performance of the system is limited. In addition, when encountering high-valent inorganic cations such as magnesium ions and calcium ions in an aqueous environment, precipitation is prone to occur.
[0083] Comparative Example 2: A method for preparing a solid clay stabilizer. The specific preparation method is the same as that of Example 1. The comparative example only does not use organic aluminum to perform metal coordination modification on the prefabricated substrate to prepare the clay stabilizer. The clay stabilizer prepared in the comparative example is partially tested for performance in the same manner as in Example 1, and the characterization results are as follows.
[0084]
[0085]
[0086]
[0087] Analysis of the above characterization results shows that the clay stabilizer prepared in the comparative example has good temperature resistance, but the anti-swelling rate and water resistance are significantly reduced. After further in-depth research, it is found that appropriate metal cations can show a synergistic effect with organic polymer long chains. This effect significantly improves the activity of the system. At the same time, affected by the active field of the twins, the critical micelle concentration in the system environment is reduced. In addition, polymers that have not been modified by metal coordination hydrolyze in an alkaline environment. When the degree of hydrolysis is too high, it will cause too much negative charge on the polymer chain, causing the suspended particles in the system to repel each other, reducing the flocculation effect of the stabilizer.
[0088] Comparative Example 3: A method for preparing a solid clay stabilizer, the specific preparation method is the same as that of Example 1, except that the clay stabilizer is prepared without preparing and using the modifying agent unique to the present invention. The clay stabilizer prepared in the comparative example is partially tested for performance in the same manner as in Example 1, and the characterization results are as follows.
[0089]
[0090]
[0091] Analysis of the above characterization results shows that the clay stabilizer prepared in the comparative example has good temperature resistance, but the anti-swelling rate and water resistance are significantly reduced. After further in-depth research, the dosage of the stabilizer is continued to increase. In theory, the cation concentration will increase, but in actual operation, the viscosity of the amine group on the side chain of the organic molecule increases, and at the same time, the steric hindrance will reduce the cation concentration, which reduces the effect of inhibiting soil swelling.
[0092] Comparative Example 4: A commercially available inorganic clay stabilizer, wherein the commercially available inorganic clay stabilizer component is 10 wt% sodium chloride and the balance is water. The commercially available clay stabilizer was subjected to partial performance testing in the same manner as in Example 1, and the characterization results are as follows.
[0093]
[0094]
[0095] Analyzing the above characterization results, commercially available clay stabilizers have the characteristics of wide supply, low price, and easy use and maintenance. However, they can only temporarily stabilize clay particles. When the actual application environment changes, such stabilizers will undergo cation exchange, causing the clay to return to its original water-sensitive state. In addition, compared with the polymer provided by the present invention, commercially available clay stabilizers cannot achieve multi-point adsorption, so the effect of preventing clay migration is not significant.
[0096] Comparative Example 5: A commercially available organic clay stabilizer, wherein the commercially available organic clay stabilizer component is 15 wt% dodecyltrimethylammonium chloride and the balance is water. The commercially available clay stabilizer was subjected to partial performance testing in the same manner as in Example 1, and the characterization results are as follows.
[0097]
[0098]
[0099] Analyzing the above characterization results, the commercially available clay stabilizer is a multi-core hydroxyl bridge complex ion clay stabilizer. As an efficient clay stabilizer, it has the characteristics of long-term stability. It can effectively inhibit the migration of particles and prevent the harm caused by clay hydration and expansion. At the same time, the stabilizer is suitable for reservoir treatment in a wide area to ensure the stability and safety of the reservoir. However, the organic long chain of the commercially available clay stabilizer exhibits negative charge, which weakens its adsorption on the clay surface, and the anti-swelling property is relatively low compared to the stabilizer prepared in the embodiment.
Claims
1. A method for preparing a solid clay stabilizer, characterized in that: The method comprises: (1) uniformly mixing a prefabricated substrate, an ammonium salt and an organic aluminum in proportion to prepare a substrate; (2) uniformly mixing a substrate, a hydrocarbon halide, an oxygen-containing heterocyclic compound and a modifying agent in proportion to prepare a crude product, and then recrystallizing and drying the product to obtain a solid clay stabilizer; the prefabricated substrate in step (1) contains polyacrylamide and allyltrimethylammonium chloride; the content of allyltrimethylammonium chloride in the prefabricated substrate is 0.1-0.3 wt%, and the balance is polyacrylamide.
2. The method for preparing a solid clay stabilizer according to claim 1, characterized in that: The ammonium salt in step (1) is methacryloyloxyethyl trimethylammonium chloride; and the organic aluminum in step (1) is aluminum trifluoromethanesulfonate.
3. The method for preparing a solid clay stabilizer according to claim 1 or 2, characterized in that: In step (1), the prefabricated substrate, ammonium salt and organic aluminum are uniformly mixed in a mass ratio of 8:(1-3):(3-5).
4. The method for preparing a solid clay stabilizer according to claim 1, characterized in that: The process of preparing the substrate in step (1) is as follows: adding the prefabricated substrate, ammonium salt and organoaluminum to a solvent, stirring for 1 to 3 hours at a temperature of 75 to 80°C and a rotation speed of 200 to 300 r / min, then adding an initiator at room temperature, and continuing to stir for 3 to 5 hours; wherein: the solvent is deionized water or deionized water; the initiator is ammonium persulfate, and the amount of the initiator used is 0.1 to 0.3 wt% of the prefabricated substrate.
5. The method for preparing a solid clay stabilizer according to claim 1, characterized in that: The hydrocarbon halide in step (2) is 1,7-dibromoheptane; and the oxygen-containing heterocyclic compound in step (2) is pyridine.
6. The method for preparing a solid clay stabilizer according to claim 1, characterized in that: The preparation method of the modifying reagent in step (2) is as follows: N, N, N-trimethyloctadecane-1-ammonium iodide, N, N-dimethylformamide and potassium iodide are uniformly mixed in a mass ratio of 3: (1.3-1.7): (2-2.5), and acetonitrile is used as a solvent to prepare a modifying agent; the amount of acetonitrile used is 2.5-3.5 times the volume of N, N-dimethylformamide.
7. The method for preparing a solid clay stabilizer according to claim 1 or 6, characterized in that: In step (2), the substrate, hydrocarbon halide, oxygen-containing heterocyclic compound and modifying agent are uniformly mixed in a mass ratio of 5: (1.8-2.2): (1.4-1.6):
3.
8. The method for preparing a solid clay stabilizer according to claim 1, characterized in that: The crude product prepared in step (2) is stirred and reacted at a temperature of 80 to 90° C. for 8 to 12 hours.
9. The method for preparing a solid clay stabilizer according to claim 1, characterized in that: The recrystallization in step (2) is performed by sequentially using ether and methanol.
10. A solid clay stabilizer obtained by the method according to any one of claims 1 to 9.
Citation Information
Cited By
Polymer clay stabilizer and preparation method thereof
CN119060342A