Method for synthesizing aniline compound by synergism of bionic nano zero-valent iron and electroactive bacteria

By biomimetic modification of nano zero-valent iron with extracellular polymers of electroactive bacteria, a biomimetic nano-zero-valent iron-electroactive bacteria coupling system is constructed, which solves the problems of by-product generation and low efficiency in the synthesis of aniline compounds, and achieves high efficiency and high efficiency. Selective synthesis reduces the toxicity and material cost of nanoscale zero-valent iron.

CN118773271APending Publication Date: 2024-10-15UNIV OF SCI & TECH OF CHINA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410907325.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing technology has the problems of by-product generation, complex equipment, high economic costs and serious environmental pollution in the chemical synthesis of aniline compounds. The efficiency of microbial methods is low and the application of nano zero-valent iron in biological systems has problems such as easy surface passivation and Cell membrane damage problem.

Method used

By using the extracellular polymer (EPS) of electroactive bacteria to biomimetically modify nano-zero-valent iron, a biomimetic nano-zero-valent iron-electroactive bacteria coupling system is constructed to improve the biocompatibility and dispersion of nano-zero-valent iron and achieve high efficiency, Highly selective synthesis of aniline compounds.

Benefits of technology

It achieves the synthesis of aniline compounds with high selectivity and stable operation, reduces the toxicity of nano-zero-valent iron, improves electron transfer efficiency, and the synthetic materials are cheap and easy to obtain, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773271A_ABST
    Figure CN118773271A_ABST
Patent Text Reader

Abstract

The invention provides a method for synthesizing aniline compounds by virtue of bionic nano zero-valent iron and electroactive bacteria, and belongs to the technical field of biosynthesis. The extracellular polymeric substance is extracted from the electroactive bacteria and then used for bionic modification of the generated nano zero-valent iron, bionic nano zero-valent iron is obtained, the wrapping effect of the extracellular polymeric substance on the nano zero-valent iron effectively improves the biocompatibility of the nano zero-valent iron, the toxicity of microorganisms is reduced, the subsequent synergistic effect of the nano zero-valent iron and the electroactive bacteria is facilitated, and the biomimetic nano zero-valent iron is obtained. Moreover, the dispersity of the bionic nano zero-valent iron is also improved, agglomeration and surface passivation are avoided, electron transfer is facilitated, and the yield of the synthesized aniline compound is further improved; the preparation method comprises the following steps: preparing biomimetic nano zero-valent iron, adding the biomimetic nano zero-valent iron into an anaerobic inorganic salt culture medium containing electroactive bacteria, incubating, constructing a biomimetic nano zero-valent iron-electroactive bacteria coupling system, adding nitrobenzene compounds, and carrying out a biological reduction reaction, thereby realizing high-efficiency and high-selectivity synthesis of aniline compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biosynthesis, and in particular to a method for synthesizing aniline compounds in cooperation with bionic nano zero-valent iron and electroactive bacteria. Background Art

[0002] Aniline compounds are important organic intermediates and basic chemical raw materials, and are widely used in organic synthesis, pharmaceutical industry, agricultural chemicals and other fields. In industry, the traditional method for synthesizing aniline compounds mainly utilizes the chemical tandem reaction of nitration-reduction of benzene ring, but the reduction of nitrobenzene to synthesize aniline compounds is a multi-electron process, and the chemical reduction method is often accompanied by the generation of multiple by-products. In addition, the current chemical synthesis method of aniline compounds faces the problems of complex reaction equipment, high economic cost, and serious environmental pollution. Therefore, it is urgent to develop a green, efficient and highly selective method for synthesizing aniline compounds.

[0003] The biological reduction method is favored because of its low cost and high selectivity. Electroactive bacteria have cytochromes that can mediate extracellular redox reactions and have the ability to highly selectively reduce nitrobenzene to synthesize aniline compounds. However, since aniline production is a process in which a compound gains electrons and is reduced, a large amount of electrons is required. Although the microbial method has high selectivity, it is inefficient. Nano-zero-valent iron is widely used as an electron donor due to its small size, large surface area, and high theoretical electron utilization efficiency. Adding nano-zero-valent iron as an electron donor in the process of microbial reduction of nitrobenzene to synthesize aniline and constructing a nano-zero-valent iron-electroactive bacteria coupling system is expected to greatly increase the yield of aniline. However, there are still many problems in the application of nano-zero-valent iron in biological systems: high surface energy makes it easy to agglomerate, easy surface passivation leads to obstruction of electron transfer, and the total amount of available electrons decreases; contact with microorganisms causes cell membrane damage, leading to microbial inactivation, and ultimately reduces the yield of bacterial synthesis of aniline. Summary of the invention

[0004] The purpose of the present invention is to provide a method for synthesizing aniline compounds by using bionic nano zero-valent iron in collaboration with electroactive bacteria. The method provided by the present invention utilizes extracellular polymers (EPS) secreted by microorganisms themselves to biomimetically modify nano zero-valent iron to obtain biomimetic nano zero-valent iron, which can effectively improve the biocompatibility of nano zero-valent iron. The constructed biomimetic nano zero-valent iron-microorganism coupling system can realize efficient and highly selective synthesis of aniline compounds. The synthetic materials required for the method provided by the present invention are cheap and easily available. The construction of the coupling system is simple and easy to operate. The coupling system can not only operate stably, but also utilize nitrobenzene compounds to reduce and synthesize aniline compounds with a selectivity close to 100%.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for synthesizing aniline compounds by using bionic nano zero-valent iron in collaboration with electroactive bacteria, comprising the following steps:

[0007] (1) washing and extracting the electroactive bacteria in sequence to obtain extracellular polymers;

[0008] (2) mixing the extracellular polymer obtained in step (1) with water, iron salt and solvent and performing pretreatment to obtain a mixed solution;

[0009] In an inert atmosphere, the mixed solution is mixed with a sodium borohydride solution, and then subjected to a reduction reaction to obtain bionic nano zero-valent iron;

[0010] (3) adding the bionic nano zero-valent iron obtained in step (2) to an anaerobic inorganic salt culture medium containing electroactive bacteria for incubation to construct a bionic nano zero-valent iron-electroactive bacteria coupling system, and then adding nitrobenzene compounds to carry out a bioreduction reaction to obtain aniline compounds.

[0011] Preferably, the electroactive bacteria in step (1) include at least one of Shewanella bacteria and Geobacter bacteria.

[0012] Preferably, the extraction and treatment method in step (1) comprises at least one of high-speed centrifugation, ultrasound, resin and thermal extraction.

[0013] Preferably, the iron salt in step (2) is at least one of a divalent iron salt and a trivalent iron salt.

[0014] Preferably, the mass ratio of the extracellular polymer to the iron salt in step (2) is 1:(0.5-12).

[0015] Preferably, the reduction reaction in step (2) is carried out under an inert atmosphere with stirring.

[0016] Preferably, after the reduction reaction of step (2) is completed, the process further comprises: sequentially subjecting the product of the reduction reaction to magnetic separation, oxygen-free water washing, anhydrous ethanol washing, drying and grinding.

[0017] Preferably, in the anaerobic inorganic salt medium containing electroactive bacteria in step (3), the initial OD of the electroactive bacteria after inoculation is 600 It is 0.06~0.5.

[0018] Preferably, the anaerobic inorganic salt culture medium containing electroactive bacteria in step (3) comprises the following components per liter of culture solution: 9.07 g PIPES, 2.154 g NaOH, 0.68 g NaH2PO4·2H2O, 0.1 g KCl, 1.5 g NH4Cl, 18 mM sodium lactate, and 1 mL of trace element concentrate;

[0019] Each liter of the trace element concentrated solution includes the following components: 1.5g nitrilotriacetic acid, 30g MgSO4·7H2O, 5g MnSO4·H2O, 10g NaCl, 1g FeSO4·7H2O, 1g CaCl2·2H2O, 1g CoCl2·2H2O, 1.3g ZnCl2, 0.1g CuSO4·5H2O, 0.1g AlK(SO4)2·12H2O, 0.1g H3BO3, 0.25g Na2MoO4·2H2O, 0.25g NiCl2·6H2O, and 0.25g Na2WO4·2H2O.

[0020] Preferably, the nitrobenzene compound in step (3) is at least one of sodium m-nitrobenzene sulfonate and sodium p-nitrobenzene sulfonate.

[0021] The present invention provides a method for synthesizing aniline compounds by using bionic nano zero-valent iron in cooperation with electroactive bacteria. First, extracellular polymers are extracted by using electroactive bacteria, and then mixed with water, iron salt and solvent, and then pretreated to obtain a mixed solution. In an inert atmosphere, a sodium borohydride solution is added to perform a reduction reaction, and the nano zero-valent iron generated by bionic modification with EPS is obtained to obtain bionic nano zero-valent iron, that is, nano zero-valent iron wrapped with extracellular polymers (abbreviated as nZVI). bio ), the wrapping effect of extracellular polymers can effectively improve the biocompatibility of nano zero-valent iron, avoid contact with electroactive bacteria and other microorganisms to cause cell membrane damage and lead to microbial inactivation, reduce its toxicity to microorganisms, and facilitate the subsequent synergistic effect between it and electroactive bacteria to achieve high selectivity and high yield of aniline compounds. On the other hand, it improves the dispersibility of bionic nano zero-valent iron, avoids agglomeration and surface passivation, is conducive to electron transfer, maintains a high total amount of available electrons, and further improves the yield of synthesized aniline compounds; then the bionic nano zero-valent iron is added to the anaerobic inorganic salt culture medium containing electroactive bacteria for incubation to construct a bionic nano zero-valent iron-electroactive bacteria coupling system (abbreviated as nZVI bio-electroactive bacteria coupling system), and then adding nitrobenzene compounds to carry out biological reduction reaction, so as to realize efficient and highly selective synthesis of aniline compounds. The synthetic materials required for the method provided by the present invention are cheap and easily available, the construction of the coupling system is simple and easy to operate, and the bionic nano zero-valent iron-electroactive bacteria coupling system can not only operate stably, but also the selectivity of nitrobenzene compounds for reducing aniline compounds to be close to 100%. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a comparison chart of the yields of m-aminobenzenesulfonic acid synthesized in Examples 1 to 3 of the present invention and Comparative Examples 1 to 4;

[0023] Figure 2 Schematic diagram of the device for synthesizing m-aminobenzenesulfonic acid in Examples 1 to 3 and Comparative Examples 2 to 4 of the present invention;

[0024] Figure 3 nZVI prepared in Example 1 of the present invention bio and the transmission electron microscopy image of nZVI prepared in Comparative Example 2, wherein Figure 3 A in it is nZVI, Figure 3 B in the figure is nZVI bio ;

[0025] Figure 4 The control group of the present invention, nZVI of different concentrations and nZVI bio OD of electroactive bacteria 600 Trend graphs over time;

[0026] Figure 5 nZVI prepared in Example 1 of the present invention bio with scanning electron micrographs of electroactive bacteria;

[0027] Figure 6 is nZVI in Example 1 bio -The generation of intermediate aminobenzenesulfonic acid and the consumption of sodium m-nitrobenzenesulfonate in the electroactive bacteria coupled system over time;

[0028] Figure 7 is nZVI in Example 1 of the present invention bio -A graph showing the yield change of m-aminobenzenesulfonic acid synthesized during the periodic cycle operation of the nZVI-electroactive bacteria coupling system in the electroactive bacteria coupling system and the comparative example 2. DETAILED DESCRIPTION

[0029] The present invention provides a method for synthesizing aniline compounds by using bionic nano zero-valent iron in collaboration with electroactive bacteria, comprising the following steps:

[0030] (1) washing and extracting the electroactive bacteria in sequence to obtain extracellular polymers;

[0031] (2) mixing the extracellular polymer obtained in step (1) with water, iron salt and solvent and performing pretreatment to obtain a mixed solution;

[0032] In an inert atmosphere, the mixed solution is mixed with a sodium borohydride solution, and then subjected to a reduction reaction to obtain bionic nano zero-valent iron;

[0033] (3) adding the bionic nano zero-valent iron obtained in step (2) to an anaerobic inorganic salt culture medium containing electroactive bacteria for incubation to construct a bionic nano zero-valent iron-electroactive bacteria coupling system, and then adding nitrobenzene compounds to carry out a bioreduction reaction to obtain aniline compounds.

[0034] In the present invention, unless otherwise specified, the raw materials used are conventional commercial products in the art.

[0035] The invention sequentially cleans and extracts the electroactive bacteria to obtain extracellular polymers.

[0036] In the present invention, the electroactive bacteria include at least one of Shewanella bacteria and Geobacter bacteria, more preferably at least one of Shewanella oneidensis MR-1 and Geobacter sulfurreducens. In the present invention, the electroactive bacteria are preferably obtained from activated sludge of a sewage treatment plant or conventional laboratory culture.

[0037] In the present invention, the cleaning agent is preferably a sodium chloride solution with a mass concentration of 0.9% (g / mL); the cleaning times are preferably 2 to 5 times. The present invention removes impurities by cleaning, which is conducive to obtaining extracellular polymers with higher purity later.

[0038] In the present invention, the extraction method includes at least one of high-speed centrifugation, ultrasound, resin and heat extraction, and more preferably heat extraction. In the present invention, the heat extraction method preferably includes: mixing the cleaned electroactive bacteria with ultrapure water, heat-treating under nitrogen aeration, and then centrifuging, filtering and freeze-drying in sequence to obtain extracellular polymers.

[0039] In the present invention, the temperature of the heat treatment is preferably 40-80°C; the time of the heat treatment is preferably 20-60 min. In the present invention, the centrifugation is preferably performed at a rotation speed of 7000-9000 rpm and 3-5°C for 10-30 min. The present invention removes the bottom precipitate by centrifugation and collects the supernatant containing extracellular polymers. In the present invention, the filter membrane used for the suction filtration is preferably a mixed fiber water filter membrane with a pore size of 0.22 μm. The present invention removes impurities in the supernatant obtained by the centrifugation by suction filtration. The present invention has no special restrictions on the freeze-drying method and can adopt the technical solutions well known in the art. In the present invention, the prepared extracellular polymers are preferably stored in a drying oven.

[0040] After obtaining the extracellular polymer, the present invention mixes the extracellular polymer with water, iron salt and solvent and performs pretreatment to obtain a mixed solution.

[0041] In the present invention, the iron salt is preferably at least one of a divalent iron salt and a trivalent iron salt, more preferably at least one of ferric chloride hexahydrate, ferrous chloride tetrahydrate, ferrous sulfate, and ferric sulfate, and further preferably ferric chloride hexahydrate. In the present invention, the mass ratio of the extracellular polymer and the iron salt is preferably 1: (0.5-12), more preferably 1: (1-10), and further preferably 1: (2-6). In the present invention, the solvent is preferably anhydrous ethanol. In the present invention, the mixing method of the extracellular polymer with water, iron salt and solvent is preferably: after mixing the extracellular polymer and water, a first ultrasound is performed to obtain an extracellular polymer solution; after mixing the extracellular polymer solution and the iron salt, a solvent is added, and a second ultrasound is performed to obtain a mixed solution.

[0042] The present invention has no particular limitation on the first ultrasonication and the second ultrasonication, as long as the components are mixed evenly.

[0043] In the present invention, the pretreatment is preferably performed by oscillating at a rate of 100 to 200 rpm for 10 to 16 hours. The present invention uses pretreatment to fully mix and avoid uneven mixing of the components, which is beneficial to the subsequent reduction reaction to generate nano zero-valent iron. The extracellular polymer completely coats the nano zero-valent iron, thereby obtaining biomimetic nano zero-valent iron with better performance.

[0044] After obtaining the mixed solution, the present invention mixes the mixed solution with a sodium borohydride solution in an inert atmosphere, and then performs a reduction reaction to obtain bionic nano zero-valent iron.

[0045] In the present invention, the inert atmosphere is preferably a nitrogen atmosphere. In the present invention, the mixing method of the mixed solution and the sodium borohydride solution is preferably to drop the sodium borohydride solution into the mixed solution under stirring at room temperature.

[0046] In the present invention, the stirring rate is preferably 200-400rpm, more preferably 250-350rpm. In the present invention, the dropping rate of the sodium borohydride solution is preferably 0.5-4mL / min, more preferably 1-2mL / min. The present invention controls the dropping rate of the sodium borohydride solution within the above range to avoid excessively fast addition of the sodium borohydride solution, which causes the generated nano zero-valent iron particles to aggregate severely or the particle size to be significantly uneven, thereby affecting the dispersibility and electron transfer performance of the prepared bionic nano zero-valent iron.

[0047] In the present invention, the reduction reaction is carried out under an inert atmosphere and under stirring; the temperature of the reduction reaction is room temperature; and the time of the reduction reaction is 20 to 80 minutes, more preferably 30 to 60 minutes.

[0048] After the reduction reaction is completed, the present invention preferably sequentially performs magnetic separation, oxygen-free water washing, anhydrous ethanol washing, drying and grinding on the product of the reduction reaction.

[0049] The present invention has no special restrictions on the magnetic separation method, and the technical solutions well known in the art can be used. In the present invention, the number of oxygen-free water washing is preferably 2 to 5 times, more preferably 3 times; the number of anhydrous ethanol washing is preferably 2 to 5 times, more preferably 3 times. In the present invention, the drying method is preferably nitrogen purging or natural drying overnight in an anaerobic environment; the drying time is preferably 50 to 100 minutes; the drying temperature is preferably room temperature. The present invention removes residual solvent by drying and avoids bionic nano zero-valent iron oxidation. In the present invention, the grinding is preferably carried out under anaerobic conditions. In the present invention, the prepared bionic nano zero-valent iron oxide is preferably sealed and stored in an inert atmosphere.

[0050] After obtaining the bionic nano zero-valent iron, the present invention adds the bionic nano zero-valent iron to an anaerobic inorganic salt culture medium containing electroactive bacteria for incubation to construct a bionic nano zero-valent iron-electroactive bacteria coupling system, and then adds nitrobenzene compounds to perform a bioreduction reaction to obtain aniline compounds.

[0051] In the present invention, the bionic nano zero-valent iron is preferably added in the form of an oxygen-free water suspension of bionic nano zero-valent iron; the concentration of the oxygen-free water suspension of bionic nano zero-valent iron is preferably 1-8 g / L, more preferably 2-5 g / L. In the present invention, the concentration of bionic nano zero-valent iron in the bionic nano zero-valent iron-electroactive bacteria coupling system is preferably 10-150 mg / L, more preferably 20-100 mg / L. The present invention controls the concentration of bionic nano zero-valent iron to ensure the bacterial activity in the bionic nano zero-valent iron-electroactive bacteria coupling system, while maximizing the superiority of the bionic modified nano zero-valent iron material over the original material.

[0052] In the present invention, the preparation method of the anaerobic inorganic salt culture medium containing electroactive bacteria is preferably: centrifuging the electroactive bacterial suspension to obtain an electroactive bacterial precipitate; washing the electroactive bacterial precipitate with a sodium chloride solution with a mass concentration of 0.9% (g / mL), and then resuspending it in a sodium chloride solution with a mass concentration of 0.9% (g / mL) to obtain a pretreated electroactive bacterial suspension; mixing the pretreated electroactive bacterial suspension with an anaerobic inorganic salt culture medium to obtain an anaerobic inorganic salt culture medium containing electroactive bacteria.

[0053] In the present invention, the centrifugation is preferably carried out at a rotation speed of 5000-8000 rpm and a temperature of 2-6° C. for 2-10 min; and the washing with the sodium chloride solution is preferably performed 2-5 times.

[0054] In the present invention, the initial OD value of the electroactive bacteria in the anaerobic inorganic salt medium containing electroactive bacteria after inoculation is 600 The present invention controls the initial OD of the electroactive bacteria after inoculation. 600 , in order to better adapt to the concentration of bionic nano zero-valent iron materials and highlight the superiority of the coupling system.

[0055] In the present invention, the anaerobic inorganic salt culture medium containing electroactive bacteria preferably includes the following components per liter of culture solution: 9.07g PIPES, 2.154g NaOH, 0.68g NaH2PO4·2H2O, 0.1g KCl, 1.5g NH4Cl, 18mM sodium lactate, and 1mL trace element concentrate. The present invention controls the composition of the culture solution within the above range to ensure that the bacteria maintain better activity during the coupling process and reduction reaction process of constructing the coupling system.

[0056] In the present invention, each liter of the trace element concentrated solution preferably includes the following components: 1.5 g nitrilotriacetic acid, 30 g MgSO4·7H2O, 5 g MnSO4·H2O, 10 g NaCl, 1 g FeSO4·7H2O, 1 g CaCl2·2H2O, 1 g CoCl2·2H2O, 1.3 g ZnCl2, 0.1 g CuSO4·5H2O, 0.1 g AlK(SO4)2·12H2O, 0.1 g H3BO3, 0.25 g Na2MoO4·2H2O, 0.25 g NiCl2·6H2O, 0.25 g Na2WO4·2H2O. The present invention provides the elements necessary for the growth of electroactive bacteria through the trace element concentrated solution.

[0057] In the present invention, the nitrobenzene compound is at least one of sodium m-nitrobenzene sulfonate and sodium p-nitrobenzene sulfonate. In the present invention, the concentration of the nitrobenzene compound in the bionic nano zero-valent iron-electroactive bacteria coupling system is preferably 50-300 mg / L, more preferably 80-280 mg / L. The present invention controls the concentration of nitrobenzene compounds to maximize the synergistic effect of the bionic nano zero-valent iron-electroactive bacteria coupling system, promote the bioreduction reaction, and achieve efficient and highly selective preparation of high-yield aniline compounds.

[0058] In the present invention, the temperature of the bioreduction reaction is preferably room temperature; the time of the bioreduction reaction is preferably 40 to 60 hours, more preferably 45 to 55 hours, and further preferably 48 hours.

[0059] According to the method provided by the present invention, the EPS of microorganisms is cheap and easy to obtain, the preparation operation of the bionic nano zero-valent iron is simple, and the bionic nano zero-valent iron-microorganism coupling system is easy to construct; and compared with single biosynthesis, the bionic nano zero-valent iron-electroactive bacteria coupling system prepared by the present invention is stable and efficient, and can achieve high selectivity and high yield in the preparation of aniline compounds. Moreover, the method provided by the present invention does not require special devices and equipment, is simple to operate, and is suitable for large-scale production and application.

[0060] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0061] Example 1

[0062] The method for synthesizing aniline compounds by using biomimetic nano zero-valent iron in collaboration with electroactive bacteria comprises the following steps:

[0063] (1) Pour 40 mL of the electroactive bacterial suspension of Shewanella oneidensis MR-1 cultured in the laboratory into a centrifuge tube, then centrifuge at 6000 rpm and 4°C for 5 min, pour off the supernatant, wash the precipitated electroactive bacteria three times with a sodium chloride solution with a mass concentration of 0.9% (g / mL), resuspend the washed electroactive bacteria in ultrapure water, then heat treat at 60°C for 30 min, during which nitrogen aeration is used instead of stirring, and centrifuge the heat-treated suspension at 8000 rpm and 4°C for 15 min. Use a suction filtration device to pass the supernatant obtained by centrifugation through a 0.22 μm mixed fiber water filter membrane to obtain a filtrate, freeze-dry to obtain the extracellular polymer EPS, and store it in a drying oven for use;

[0064] (2) weighing 0.1 g of the EPS solid powder obtained in step (1) into a beaker, adding 100 mL of deionized water, and performing a first ultrasonic dissolution to obtain an EPS solution; then weighing 1.9307 g of FeCl3·6H2O into the EPS solution, adding 90 mL of anhydrous ethanol, and performing a second ultrasonic dissolution. After the dissolution is complete, the mixture is placed in a shaker and shaken at 150 rpm for 12 h to obtain a mixed solution;

[0065] The mass ratio of the extracellular polymer to the iron salt FeCl3·6H2O is 1:1.93;

[0066] Weigh 1.52 g NaBH4, 0.1 g NaOH and 20 mL deionized water to prepare a sodium borohydride solution;

[0067] The mixed solution was transferred to a three-necked flask, and the sodium borohydride solution was drawn into the flask using a large syringe under a nitrogen atmosphere and a stirring rate of 250 rpm. The syringe was placed on a syringe pump, and the dropping rate of the sodium borohydride solution was set to 1 mL / min. The sodium borohydride solution was added dropwise to the mixed solution, and nitrogen was continuously aerated during the dropping to maintain an oxygen-free environment in the three-necked flask. After the dropping was completed, the syringe pump was removed, and the glass bottle stopper was plugged. The reduction reaction was carried out at room temperature for 30 minutes while maintaining stirring and nitrogen aeration conditions, so that the product of the reduction reaction was further aged and stabilized. At this time, the solution in the three-necked flask had been reduced from the initial orange-yellow iron ion solution to a black suspension of biomimetic nano zero-valent iron;

[0068] After the reduction reaction is completed, the mixture is allowed to stand, and a magnet is used for magnetic separation. The supernatant is poured out, oxygen-free water is added, and the mixture is fully mixed and washed with oxygen-free water. This operation is repeated three times, and then the mixture is washed twice with anhydrous ethanol. The supernatant is poured out, and only the black solid precipitate at the bottom is retained. The mixture is then naturally dried overnight under anaerobic conditions in an anaerobic glove box. Afterwards, the dried black solid is transferred to a mortar in the anaerobic glove box, and the solid is fully ground with a grinding rod to obtain bionic nano zero-valent iron. The solid is then divided into sealed polypropylene centrifuge tubes filled with nitrogen for standby use.

[0069] (3) 40 mL of the electroactive bacterial suspension of Shewanella oneidensis MR-1 cultured in the laboratory was poured into a centrifuge tube, and then centrifuged at 6000 rpm and 4°C for 5 min. The supernatant was discarded, and the precipitated electroactive bacteria were washed three times with a sodium chloride solution with a mass concentration of 0.9% (g / mL), and then resuspended in a sodium chloride solution with a mass concentration of 0.9% (g / mL) to obtain a pretreated electroactive bacterial suspension, which was then added to 50 mL of an anaerobic inorganic salt culture medium. The initial OD of the electroactive bacteria after inoculation was 600=0.1, to obtain an anaerobic inorganic salt medium containing electroactive bacteria;

[0070] In the anaerobic inorganic salt culture medium used for the anaerobic inorganic salt culture medium containing electroactive bacteria, the components in each liter of culture solution include: 9.07g PIPES, 2.154g NaOH, 0.68g NaH2PO4·2H2O, 0.1g KCl, 1.5g NH4Cl, 18mM sodium lactate, and 1mL trace element concentrate; the components in each liter of the trace element concentrate include: 1.5g nitrilotriacetic acid, 30g MgSO4·7H2O, 5g MnSO4·H2O, 10g NaCl, 1g FeSO4·7H2O, 1g CaCl2·2H2O, 1g CoCl2·2H2O, 1.3g ZnCl2, 0.1g CuSO4·5H2O, 0.1g AlK(SO4)2·12H2O, 0.1g H3BO3, 0.25gNa2MoO4·2H2O, 0.25gNiCl2·6H2O, 0.25gNa2WO4·2H2O;

[0071] Weigh 0.1 g of the biomimetic nano zero-valent iron prepared in step (2) and dissolve it in 20 mL of anaerobic water, and evenly disperse it by ultrasonication to obtain a biomimetic nano zero-valent iron anaerobic water suspension with a concentration of 5 g / L. Add 0.2 mL of the biomimetic nano zero-valent iron anaerobic water suspension to the anaerobic inorganic salt culture medium containing electroactive bacteria for incubation to construct a biomimetic nano zero-valent iron-electroactive bacteria coupling system, and then add sodium m-nitrobenzene sulfonate to carry out a bioreduction reaction at room temperature for 48 hours to obtain m-aminobenzenesulfonic acid.

[0072] The concentration of bionic nano zero-valent iron in the bionic nano zero-valent iron-electroactive bacteria coupling system is 20 mg / L, and the concentration of sodium m-nitrobenzene sulfonate in the bionic nano zero-valent iron-electroactive bacteria coupling system is 200 mg / L.

[0073] Example 2

[0074] The m-aminobenzenesulfonic acid was prepared according to the method of Example 1, except that the amount of the oxygen-free water suspension of bionic nano zero-valent iron with a concentration of 5 g / L added in step (3) was 0.5 mL, and the concentration of the bionic nano zero-valent iron in the bionic nano zero-valent iron-electroactive bacteria coupling system was 50 mg / L.

[0075] Example 3

[0076] The aminobenzenesulfonic acid was prepared according to the method of Example 1, except that the amount of the oxygen-free water suspension of bionic nano zero-valent iron with a concentration of 5 g / L added in step (3) was 1.0 mL, and the concentration of the bionic nano zero-valent iron in the bionic nano zero-valent iron-electroactive bacteria coupling system was 100 mg / L.

[0077] The ability of the bionic nano zero-valent iron-electroactive bacteria coupling system described in Examples 1 to 3 to synthesize aniline compounds was tested by high performance liquid chromatography, and the yields of m-aminobenzenesulfonic acid prepared in Examples 1 to 3 were measured to be 99.3%, 93.6% and 98.6%, respectively.

[0078] Comparative Example 1

[0079] The method for synthesizing aniline compounds using Shewanella oneidensis MR-1 electroactive bacteria comprises the following steps:

[0080] 40 mL of the laboratory-cultured Shewanella oneidensis MR-1 electroactive bacterial suspension was poured into a centrifuge tube, and then centrifuged at 6000 rpm and 4°C for 5 min. The supernatant was discarded, and the precipitated electroactive bacteria were washed three times with a sodium chloride solution with a mass concentration of 0.9% (g / mL). The washed electroactive bacteria were resuspended in ultrapure water and then added to 50 mL of anaerobic inorganic salt culture medium to make the initial OD of the electroactive bacteria after inoculation 600 =0.1, to obtain an anaerobic inorganic salt medium containing electroactive bacteria, then add sodium m-nitrobenzene sulfonate, and carry out reduction reaction at room temperature for 48 hours to obtain aniline compounds,

[0081] The composition of the culture solution of the anaerobic inorganic salt culture medium used in Comparative Example 1 is the same as that in Example 1.

[0082] The ability of the electroactive bacteria Shewanellaoneidensis MR-1 alone in Comparative Example 1 to synthesize aniline compounds was tested in the same manner as in Example 1, and the yield of m-aminobenzenesulfonic acid prepared in Comparative Example 1 was found to be 44%.

[0083] Comparative Example 2

[0084] The method for synthesizing aniline compounds using nano zero-valent iron comprises the following steps:

[0085] (1) Weigh 1.9307 g of FeCl3·6H2O into a three-necked flask, add 100 mL of deionized water and 90 mL of anhydrous ethanol and ultrasonically dissolve to obtain a mixed solution;

[0086] Weigh 1.52 g NaBH4, 0.1 g NaOH and 20 mL deionized water to prepare a sodium borohydride solution;

[0087] The mixed solution was transferred to a three-necked flask, and the sodium borohydride solution was drawn into the flask using a large syringe under a nitrogen atmosphere and a stirring rate of 250 rpm. The syringe was placed on a syringe pump, and the dropping rate of the sodium borohydride solution was set to 1 mL / min. The sodium borohydride solution was added dropwise to the mixed solution, and nitrogen was continuously aerated during the dropping to maintain an oxygen-free environment in the three-necked flask. After the dropping was completed, the syringe pump was removed, and the glass bottle stopper was plugged. The reduction reaction was carried out at room temperature for 30 minutes while maintaining stirring and nitrogen aeration conditions, so that the product of the reduction reaction was further aged and stabilized. At this time, the solution in the three-necked flask had been reduced from the initial orange-yellow iron ion solution to a black suspension of biomimetic nano zero-valent iron;

[0088] After the reduction reaction is completed, the mixture is allowed to stand, and a magnet is used for magnetic separation. The supernatant is poured out, oxygen-free water is added, and the mixture is fully mixed and washed with oxygen-free water. This operation is repeated three times, and then the mixture is washed twice with anhydrous ethanol. The supernatant is poured out, and only the black solid precipitate at the bottom is retained. The mixture is then naturally dried overnight under anaerobic conditions in an anaerobic glove box. After that, the dried black solid is transferred to a mortar in the anaerobic glove box, and the solid is fully ground with a grinding rod to obtain unmodified nano zero-valent iron (abbreviated as nZVI), and finally the solid is dispensed into airtight polypropylene centrifuge tubes filled with nitrogen for standby use.

[0089] (2) 40 mL of the laboratory-cultured Shewanella oneidensis MR-1 bacterial suspension was poured into a centrifuge tube, and then centrifuged at 6000 rpm and 4°C for 5 min. The supernatant was discarded, and the precipitated electroactive bacteria were washed three times with a sodium chloride solution with a mass concentration of 0.9% (g / mL), and then resuspended in a sodium chloride solution with a mass concentration of 0.9% (g / mL) to obtain a pretreated electroactive bacterial suspension, which was then added to 50 mL of an anaerobic inorganic salt culture medium. The initial OD of the electroactive bacteria after inoculation was 600 =0.1, to obtain an anaerobic inorganic salt medium containing electroactive bacteria;

[0090] Weigh 0.1 g of the nano zero-valent iron prepared in step (1) and dissolve it in 20 mL of anaerobic water, and evenly disperse it by ultrasonication to obtain an anaerobic water suspension of nano zero-valent iron with a concentration of 5 g / L. Add 0.2 mL of the anaerobic water suspension of biomimetic nano zero-valent iron to the anaerobic inorganic salt culture medium containing electroactive bacteria for incubation to construct a nano zero-valent iron-electroactive bacteria coupling system (referred to as nZVI-electroactive bacteria coupling system), then add sodium m-nitrobenzene sulfonate, and perform a bioreduction reaction at room temperature for 48 hours to obtain m-aminobenzenesulfonic acid.

[0091] The concentration of nano zero-valent iron in the nano zero-valent iron-electroactive bacteria coupling system is 20 mg / L, and the concentration of sodium m-nitrobenzene sulfonate in the nano zero-valent iron-electroactive bacteria coupling system is 200 mg / L.

[0092] The composition of the culture solution of the anaerobic inorganic salt culture medium used in Comparative Example 2 is the same as that in Example 1.

[0093] Comparative Example 3 and Comparative Example 4

[0094] According to the method of Comparative Example 2, Comparative Examples 3 and Comparative Example 4 were set up. The difference from Comparative Example 2 was that the amount of the oxygen-free water suspension of nano zero-valent iron with a concentration of 5 g / L in Comparative Examples 3 and Comparative Example 4 was 0.5 and 1.0 mL of nano zero-valent iron, respectively. The concentrations of nano zero-valent iron in the nano zero-valent iron-electroactive bacteria coupling system in Comparative Examples 3 and Comparative Example 4 were 50 mg / L and 100 mg / L, respectively.

[0095] The ability of the nano-zero-valent iron alone in Comparative Examples 2 to 4 to synthesize aniline compounds was tested in the same manner as in Example 1. The yields of m-aminobenzenesulfonic acid prepared in Comparative Examples 2 to 4 were measured to be 79.3%, 57.0% and 48.8%, respectively.

[0096] Figure 1 is a comparison chart of the yields of m-aminobenzenesulfonic acid prepared in Examples 1 to 3 and Comparative Examples 1 to 4, Figure 1 It can be seen that the yield of m-aminobenzenesulfonic acid prepared in Examples 1 to 3 is significantly higher than that in Comparative Examples 1 to 4. In Example 1, a low dose of 20 mg / mL of nZVI is added. bio When nZVI was added to the system, the yield of m-aminobenzenesulfonic acid synthesized by the bionic nano zero-valent iron-electroactive bacteria coupling system was close to 100%; the production efficiency of m-aminobenzenesulfonic acid by the nano zero-valent iron-electroactive bacteria coupling system was better than that by the electroactive bacteria alone, but with the increase of nZVI dosage, the output rate of m-aminobenzenesulfonic acid by the nano zero-valent iron-electroactive bacteria coupling system gradually decreased. These indicate that nZVI can supply electrons to promote the synthesis of aniline compounds by electroactive bacteria, but nZVI is highly toxic. When the dosage increases, it will be toxic to microorganisms, and the performance of the nZVI-electroactive bacteria coupling system will deteriorate.

[0097] Figure 2 Schematic diagram of the device for synthesizing m-aminobenzenesulfonic acid in Examples 1 to 3 and Comparative Examples 2 to 4 of the present invention, comprising Figure 2 As shown, the device is mainly composed of a nitrogen aeration tube, a three-necked flask, a mechanical stirrer and a syringe pump.

[0098] The nZVI prepared in Example 1 of the present invention was observed by transmission electron microscopy. bio The transmission electron microscopy images of nZVI prepared in Comparative Example 2 are as follows: Figure 3As shown, Figure 3 A in it is nZVI, Figure 3 B in the figure is nZVI bio ,Depend on Figure 3 It can be seen that nZVI has a typical chain structure with a diameter ranging from 50 to 100 nm, while nZVIbio does not show a beaded shape and is surrounded by a low-contrast EPS halo. bio Dispersibility is higher than nZVI bio , the nZVI was alleviated by biomimetic modification of nano-zero-valent iron with extracellular polymers bio reunion.

[0099] The nZVI prepared in Example 1 was investigated by a bacterial exposure and resuscitation experiment. bio The toxicity of nZVI prepared in Example 2 to the microbial electroactive bacteria Shewanella oneidensis MR-1 cultured in the laboratory was as follows: bio 1 ml of the bacterial suspension was added to 20 ml of fresh LB medium, and the bacterial growth was monitored at different time points. The unexposed bacteria were used as the control group to obtain the control group, different concentrations of nZVI and nZVI. bio OD of electroactive bacteria 600 The trend chart over time is as follows Figure 4 As shown. Figure 4 It can be seen that when nZVI is 20 mg / L, nZVI has almost no inhibition on the growth of microorganisms, but when the concentration is increased to 50 and 100 mg / L, nZVI almost completely inhibits the growth of microorganisms; compared with nZVI, nZVI bio The toxicity to microorganisms is greatly reduced. bio When the concentration reaches 50 and 100 mg / L, there is only a slight inhibition on the growth of microorganisms.

[0100] Scanning electron microscopy observation of nZVI constructed in Example 1 bio -Electroactive bacteria coupling system, to obtain nZVI prepared in Example 1 bio Scanning electron microscopy images of electroactive bacteria Figure 5 As shown by Figure 5 It can be seen that nZVI prepared in Example 1 bio Close contact with electroactive bacteria provides convenient conditions for direct electron donation, which is beneficial to improve the constructed nZVI bio -Yields of aniline compounds synthesized by electroactive bacterial coupled system.

[0101] Figure 6 is nZVI in Example 1 bio-The generation of intermediate aminobenzenesulfonic acid and the consumption of sodium m-nitrobenzenesulfonate in the electroactive bacterial coupling system over time, by Figure 6 It can be seen that nZVI in Example 1 bio -The electroactive bacteria coupling system can reduce sodium m-nitrobenzenesulfonate to 100% m-aminobenzenesulfonic acid without other by-products.

[0102] To detect nZVI bio - Stability of the electroactive bacteria coupling system and the nZVI-electroactive bacteria coupling system. m-Aminobenzenesulfonic acid was synthesized according to the methods of Example 1 and Comparative Example 2. At the same time, sodium m-nitrobenzenesulfonate was added again at the end of each cycle with two days as a cycle. Five cycles, i.e., ten days, were run continuously to obtain nZVI. bio The yield change of m-aminobenzenesulfonic acid synthesized during the periodic cycle operation of the nZVI-electroactive bacteria coupling system and the nZVI-electroactive bacteria coupling system is shown in the figure Figure 7 As shown by Figure 7 It can be seen that nZVI bio -Electroactive bacteria coupling system can always maintain nearly 100% m-aminobenzenesulfonic acid output rate, while the m-aminobenzenesulfonic acid output rate of nZVI-electroactive bacteria coupling system is only 20% to 60%.

[0103] In summary, compared with nZVI, nZVI prepared in Examples 1 to 3 of the present invention bio With higher biocompatibility, nZVI bio nZVI composed of electroactive bacteria bio -The electroactive bacteria-coupled system can synthesize aniline compounds more stably and efficiently.

[0104] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for synthesizing aniline compounds by using bionic nano zero-valent iron in collaboration with electroactive bacteria, characterized in that: The following steps are involved: (1) washing and extracting the electroactive bacteria in sequence to obtain extracellular polymers; (2) mixing the extracellular polymer obtained in step (1) with water, iron salt and solvent and performing pretreatment to obtain a mixed solution; In an inert atmosphere, the mixed solution is mixed with a sodium borohydride solution, and then subjected to a reduction reaction to obtain bionic nano zero-valent iron; (3) adding the bionic nano zero-valent iron obtained in step (2) to an anaerobic inorganic salt culture medium containing electroactive bacteria for incubation to construct a bionic nano zero-valent iron-electroactive bacteria coupling system, and then adding nitrobenzene compounds to carry out a bioreduction reaction to obtain aniline compounds.

2. The method according to claim 1, characterized in that: The electroactive bacteria in step (1) include at least one of Shewanella bacteria and Geobacter bacteria.

3. The method according to claim 1, characterized in that The extraction method in step (1) includes at least one of high-speed centrifugation, ultrasound, resin and thermal extraction.

4. The method according to claim 1, characterized in that: The iron salt in step (2) is at least one of a divalent iron salt and a trivalent iron salt.

5. The method according to claim 1, characterized in that The mass ratio of the extracellular polymer to the iron salt in the step (2) is 1:(0.5-12).

6. The method according to claim 1, characterized in that: The reduction reaction in step (2) is carried out under an inert atmosphere and stirring conditions.

7. The method according to claim 1, characterized in that: After the reduction reaction in step (2) is completed, the process further includes: sequentially subjecting the product of the reduction reaction to magnetic separation, oxygen-free water washing, anhydrous ethanol washing, drying and grinding.

8. The method according to claim 1, characterized in that In the anaerobic inorganic salt medium containing electroactive bacteria in step (3), the initial OD of the electroactive bacteria after inoculation is 600 It is 0.06~0.

5.

9. The method according to claim 1, characterized in that: The anaerobic inorganic salt culture medium containing electroactive bacteria in step (3) comprises the following components per liter of culture solution: 9.07 g PIPES, 2.154 g NaOH, 0.68 g NaH2PO4·2H2O, 0.1 g KCl, 1.5 g NH4Cl, 18 mM sodium lactate, and 1 mL of trace element concentrate; Each liter of the trace element concentrated solution includes the following components: 1.5g nitrilotriacetic acid, 30g MgSO4·7H2O, 5g MnSO4·H2O, 10g NaCl, 1g FeSO4·7H2O, 1g CaCl2·2H2O, 1g CoCl2·2H2O, 1.3g ZnCl2, 0.1g CuSO4·5H2O, 0.1g AlK(SO4)2·12H2O, 0.1g H3BO3, 0.25g Na2MoO4·2H2O, 0.25g NiCl2·6H2O, and 0.25g Na2WO4·2H2O.

10. The method according to claim 1, characterized in that The nitrobenzene compound in step (3) is at least one of sodium m-nitrobenzene sulfonate and sodium p-nitrobenzene sulfonate.

Citation Information

Patent Citations

  • Method for coupling and passivating nano zero-valent iron system by using reinforced iron reducing bacteria

    CN111115841A

  • Method for cyclically degrading nitrobenzene in wastewater by utilizing extracellular polymeric substances to reinforce nano zero-valent iron

    CN111377518A

  • Shewanella extracellular polymer coated nano-iron material as well as preparation method and application thereof

    CN118164621A