Control method for removing high-temperature alloy inclusions

By designing the addition amount of active elements and bottom-blown argon process parameters in high-temperature alloy smelting, using the Reynolds number formula to calculate the floating speed of inclusions, and combining high-purity argon gas and bottom-blown argon systems to quickly remove small non-metallic inclusions and solve the current problem. The technology eliminates the problems of low efficiency and high cost and achieves high purity and low-cost production of high-temperature alloys.

CN118773399APending Publication Date: 2024-10-15INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310584501.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing high-temperature alloy smelting process is difficult to effectively remove small non-metallic inclusions, resulting in damage to material properties, and increasing the refining time or using conventional slag filtering technology cannot significantly improve the removal efficiency and increase production costs.

Method used

By designing the addition amount of active elements and bottom-blown argon process parameters, and using the Reynolds number formula to calculate the ultimate floating speed of inclusions, combined with high-purity argon and bottom-blown argon systems, the intermediate liquid steel floats, and the inclusions are in contact with the crucible, achieving Quick removal.

Benefits of technology

Significantly reduce the O, N, and S content in the alloy, reduce the percentage of secondary remelting dross, improve the purity of the alloy, ensure the quality of the finished alloy, and reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004242785460000011
    Figure FDA0004242785460000011
  • Figure FDA0004242785460000012
    Figure FDA0004242785460000012
  • Figure FDA0004242785460000013
    Figure FDA0004242785460000013
Patent Text Reader

Abstract

The invention belongs to the field of high-temperature alloy purification smelting, and particularly relates to a control method for high-temperature alloy inclusion removal. The method comprises the steps of designing the adding amount of purification elements, the adding process and bottom argon blowing process parameters, calculating the designed adding amount of the purification elements such as the active element Ca through an empirical formula and alloy components, adding the purification elements in the production process step, and calculating the bottom argon blowing process parameters according to the empirical formula and smelting related parameters. By controlling the adding amount of the active elements, the tiny inclusions in the molten steel are modified to form large-size low-density inclusions while the residual amount of the active elements meets the standard requirements of the mother alloy, so that the floating speed of the inclusions is increased. And meanwhile, the bottom argon blowing process is matched, so that inclusions in the molten steel float upwards more quickly and make contact with a crucible, the purpose of separating from the molten steel is achieved, the percentage of secondary remelting scum of the mother alloy can be effectively reduced, the purity of the alloy is improved, and the yield of subsequent castings can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention belongs to the field of high-temperature alloy purification smelting, and in particular relates to a control method for removing high-temperature alloy inclusions. Background technology:

[0002] High-temperature alloys have good high-temperature oxidation resistance, high-temperature mechanical properties and corrosion resistance, so they are widely used in aerospace, energy development and other fields. High-temperature alloys account for 40% of high-temperature materials used in various aerospace engines. With the development of the aerospace industry, high-temperature alloys are used more and more widely, the service conditions are becoming more and more harsh, and the requirements for material performance are becoming higher and higher. At present, the production of high-temperature alloys mostly adopts vacuum induction smelting process, or adopts two-way or three-way process assisted by electroslag remelting or vacuum consumable. Among them, the important role of vacuum induction melting and electroslag remelting process is to remove harmful impurity elements in the alloy and reduce the content of alloy inclusions. The vacuum induction melting process has a good vacuum atmosphere, which is conducive to the removal of gas elements. At the same time, the cleanliness of the alloy produced by vacuum induction melting will also directly affect the removal efficiency of non-metallic inclusions during the electroslag remelting process. It can be seen that vacuum induction melting is a key process for manufacturing high-purity alloys. The production assisted by multiple processes has no obvious effect on the removal efficiency of alloy inclusions, and its production cost is significantly increased.

[0003] When using vacuum induction smelting technology to produce high-temperature alloys, on the one hand, the degassing efficiency of the alloy smelting process can be improved by increasing the vacuum degree of the smelting environment, thereby achieving the purpose of reducing the gas content of the alloy; on the other hand, through a reasonable high-temperature refining process, some impurity elements can be promoted to form non-metallic inclusions, which can be removed from the alloy through crucible adsorption or reasonable slag blocking technology during the stirring and pouring process. However, for non-metallic inclusions of small size, their floating rate in molten steel is slow, and they cannot be removed by conventional slag blocking technology. Such non-metallic inclusions enter the alloy ingot, which will destroy the continuity of the alloy matrix and greatly affect the strength, fatigue, toughness, plasticity and other properties of the material; and increasing the floating time of non-metallic inclusions in molten steel by increasing the refining time not only greatly increases the alloy smelting cost, but also has little effect on improving the efficiency of inclusion removal. At the same time, increasing the contact time between molten steel and refractory materials such as crucibles under high temperature conditions is very likely to introduce new inclusions into the molten steel, reducing the quality of the molten steel. Summary of the invention:

[0004] In order to solve the shortcomings and deficiencies of the prior art, the purpose of the present invention is to provide a control method for removing inclusions from high-temperature alloys, which can effectively control production costs while improving the removal efficiency and improve the purity of high-temperature alloy master alloys.

[0005] The technical solution adopted by the present invention is:

[0006] A control method for removing inclusions from a high-temperature alloy comprises the following steps:

[0007] The first step is to design the amount of active elements to be added according to equations (1) to (7), and wrap them with Ni foil or Al foil for later use;

[0008] For fine non-metallic inclusions in molten steel, the relationship between the drag coefficient of the inclusions and the Reynolds number is divided into the Stokes law region, the transition region, and the Newton law region according to the size of the Reynolds number. In different regions, the limit floating rate of non-metallic inclusions meets the requirements of equations (1)-(3):

[0009] (1) Stokes' law region, Reynolds number Re<1

[0010]

[0011] (2) Transition zone, 1<Re<500

[0012]

[0013] (3) Newton’s law area, 500<Re<2×10 5

[0014]

[0015] Reynolds number formula:

[0016] Where, v is the limit floating velocity of inclusions, m / s; ρ f —Steel liquid density, kg / m 3 ρ k —Inclusion density, kg / m 3 ; g—acceleration due to gravity, m / s 2 ; μ—dynamic viscosity of molten steel, kg / (m·s); d—equivalent diameter of inclusions, m;

[0017] First, calculate the oxygen and sulfur supply of the alloy raw materials. The calculation formula is as follows:

[0018]

[0019] In the formula, c O / S is the total oxygen and sulfur supply of the alloy raw materials, wt%; c i O / S is the O / S content in the i-th raw material, wt%; C i is the designed content of the i-th raw material in the alloy, wt%;

[0020] Active elements are added after high-temperature refining and the temperature is lowered to near the low-temperature refining temperature. The amount of addition is calculated according to formula (6):

[0021] c H =max(ac O , bc s ) (6)

[0022] In the formula, c H is the amount of active elements added, wt%; c O Total oxygen supply in alloy raw materials, wt%; c S is the total sulfur supply in the alloy raw materials, wt%; a and b are coefficients, which are determined according to the mass ratio of the elements in the stable oxides and sulfides formed by the selected active elements;

[0023] If the alloy design composition contains rare earth elements, the amount of active elements added should be reduced according to the amount of rare earth elements added;

[0024]

[0025] In the formula, c RE is the amount of rare earth element added to the alloy, wt%; e is the empirical coefficient, ranging from 5 to 10;

[0026] Step 2: After the alloy is refined at high temperature, when the melt temperature drops to 10-20°C higher than the low-temperature refining temperature, add small alloy materials in batches, and let the liquid stand for 0.5-5 minutes after the liquid level stabilizes; when the temperature continues to drop to 0-10°C higher than the low-temperature refining point, add active elements;

[0027] Step 3: After the liquid level stabilizes, turn off the vacuum pump group, fill the furnace with high-purity argon to 0.2MPa-0.4MPa, and then turn on the bottom blowing argon system. During the low-temperature refining of the alloy, the molten pool is stirred by blowing argon from the bottom, so that a cycle of the middle molten steel floating up and the molten steel at the edge of the molten pool sinking is formed in the molten steel, thereby increasing the floating rate of inclusions in the molten steel, and adsorbing them on the surface of the crucible when in contact with the crucible, so as to purify the molten steel;

[0028] Step 4: Close the bottom blowing argon system, turn on the vacuum pump group, evacuate the vacuum degree in the furnace to a pressure of less than 50Pa, adjust the temperature to the pouring temperature and then start pouring.

[0029] In the control method for removing inclusions from high-temperature alloys, in formula (6), when the active element Ca is selected, the oxide and sulfide formed are CaO and CaS respectively, and at this time a is 2.5 and b is 1.25.

[0030] In the control method for removing high-temperature alloy inclusions, in the second step, the small alloy material is one or more of the easily oxidizable and burnt elements Al, V, B, Ti, and rare earth elements.

[0031] In the control method for removing inclusions from high-temperature alloys, in the third step, the bottom blowing argon pressure is dynamically adjusted according to the actual state of the liquid level.

[0032] In the control method for removing inclusions from high-temperature alloys, in the third step, the bottom blowing argon flow rate is controlled as follows:

[0033]

[0034] In the formula, τ m is the uniform mixing time of molten steel, s; ε m is the specific stirring energy W / t;

[0035]

[0036] In the formula, Q 0 is the theoretical bottom blowing argon flow rate, m 3 / s; V 0 is the molar volume of gas under standard conditions, which is 22.4×10 -3 m 3 / mol; G is the weight of molten steel, t; R is the universal gas constant, which is 8.314 J / mol·K; T 1 、T 2 are the argon gas and molten steel temperatures, K; P 1 is the sum of the pressure in the crucible and the pressure of the molten steel on the gas plug, Pa; P 2 is the gas pressure in the crucible, Pa;

[0037] P 2 =P 1 +ρgh (10)

[0038] Where ρ is the density of molten steel, kg / m 3 ; h is the height of molten steel, m;

[0039] Q=fQ 0 (11)

[0040] Where, Q is the bottom blowing argon flow rate, m 3 / s; f is the empirical coefficient, ranging from 1 to 2.5;

[0041]

[0042] In the formula, Q Z is the amount of molten steel lifted on the Z horizontal plane, m 3 / s; Z is the depth of the molten steel h minus the thickness of the surface stratosphere, and Z is taken as 0.95h, m;

[0043]

[0044] In the formula, τc is the steel liquid cycle, s; G is the steel liquid weight, t; Q Z is the amount of molten steel lifted on the Z horizontal plane, m 3 / s; ρ is the density of molten steel, kg / m 3 .

[0045] The control method for removing high-temperature alloy inclusions, when determining the bottom blowing argon flow rate, first selects the uniform mixing time τ of the molten steel according to the complexity of the high-temperature alloy composition. m , between 90s and 200s; then, the bottom blowing argon flow rate Q is calculated according to equations (8)-(11); finally, the steel liquid cycle period τ is calculated according to equations (12)-(13) c , if τ is satisfied m ≥3τ c , then the uniform mixing time of molten steel is τ m The selected value and the calculated value of bottom blowing argon flow rate are valid, otherwise re-select the uniform mixing time value of the molten steel and repeat the above steps.

[0046] In the control method for removing inclusions from high-temperature alloys, in the third step, the bottom blowing argon pressure is controlled, and the bottom blowing argon pressure satisfies the following relationship:

[0047] P≥P 1 +ΔP (14)

[0048] Where, P is the bottom blowing argon pressure, Pa, ΔP is the total pressure drop from the pressure gauge to the bottom of the crucible, which is 20000Pa~70000Pa.

[0049] In the control method for removing high-temperature alloy inclusions, in actual production, the bottom blowing argon pressure is flexibly adjusted according to equation (14) and the state of bubbles above the molten pool to ensure that the steel liquid level does not fluctuate violently.

[0050] In the control method for removing inclusions from high-temperature alloys, in the third step, the bottom argon blowing time is controlled, and the bottom argon blowing time satisfies the following relationship:

[0051] t = jτ m (15)

[0052] Where, t is the bottom blowing time, s; j is the coefficient, ranging from 1 to 10; τ m is the uniform mixing time of molten steel, s.

[0053] According to the control method for removing inclusions from high-temperature alloys, during the production process, active elements are added after high-temperature refining and adding small materials, and then the temperature is lowered to near the low-temperature refining point. After the liquid level is stabilized, the vacuum pump group is turned off, and high-purity argon gas is filled into the furnace to 0.2MPa-0.4MPa, and then the bottom blowing argon system is turned on; thereafter, the bottom blowing argon system is turned off, the vacuum pump group is turned on, the vacuum degree in the furnace is evacuated to a pressure of less than 50Pa, and the temperature is adjusted to the pouring temperature before pouring.

[0054] The design concept of the present invention is:

[0055] The present invention includes the addition amount of purification elements and the addition process and the design of bottom argon blowing process parameters. The design addition amount of purification elements such as active elements Ca is calculated by empirical formula and alloy composition, and added in appropriate production process steps. At the same time, reasonable bottom argon blowing process parameters are calculated according to empirical formula and smelting related parameters. Through the reasonable addition amount of active elements, while ensuring that the residual amount of active elements meets the standard requirements of the master alloy, the tiny inclusions in the molten steel can be modified to form large-sized low-density inclusions, thereby accelerating the floating speed of the inclusions. At the same time, in conjunction with the bottom argon blowing process, the inclusions in the molten steel can float faster and contact with the crucible to achieve the purpose of separation from the molten steel, which can effectively reduce the percentage of secondary remelting slag of the master alloy, improve the purity of the alloy, and help improve the subsequent casting qualification rate.

[0056] The present invention selects active elements such as Ca as inclusion modifiers. The chemical properties of the active elements are more active than Al. Therefore, the introduction of active elements can partially reduce the Al element. At the same time, the density of the formed oxide inclusions is low, which is more conducive to floating. On the one hand, the formed oxide inclusions in the molten steel react with Al 2 O 3 The inclusions collide and react to form xCaO·yAl 2 O 3 For composite inclusions, the inclusion size increases, the density decreases, and the floating rate further increases. On the other hand, active elements such as Ca have different degrees of desulfurization ability, which is very helpful for the removal of S elements in high-temperature alloys.

[0057] The advantages and positive effects of the present invention are:

[0058] 1. Compared with the original production process, it can significantly reduce the content of O, N, and S in the alloy, significantly reduce the percentage of slag in the secondary remelting process of the alloy ingot, and improve the purity of the alloy. This method is suitable for most high-temperature alloy smelting production, and can adjust relevant process parameters in real time according to actual production conditions, with strong practicality.

[0059] 2. Introducing active elements into molten steel according to the method of the present invention, in conjunction with a bottom argon blowing system, can purify the alloy, ensuring that the O content in the alloy is less than 8ppm, the N content is less than 5ppm, the S content is less than 5ppm, and the active element content is less than 10ppm, thereby significantly reducing the slag percentage during the secondary remelting of the alloy. DETAILED DESCRIPTION

[0060] In a specific implementation process, the present invention proposes a control method for removing inclusions from high-temperature alloys, which specifically includes the following steps:

[0061] The first step is to design the amount of active elements to be added according to equations (1) to (7), and wrap them with Ni foil or Al foil for later use;

[0062] For fine non-metallic inclusions in molten steel, the relationship between the drag coefficient of the inclusions and the Reynolds number can be divided into the Stokes law region, transition region, Newton's law region, etc. according to the size of the Reynolds number. The limit floating rate of non-metallic inclusions in different regions meets the requirements of formulas (1)-(3):

[0063] (1) Stokes' law region, Reynolds number Re<1

[0064]

[0065] (2) Transition zone, 1<Re<500

[0066]

[0067] (3) Newton’s law area, 500<Re<2×10 5

[0068]

[0069] Reynolds number formula:

[0070] Where, v is the limit floating velocity of inclusions, m / s; ρ f —Steel liquid density, kg / m 3 ρ k —Inclusion density, kg / m 3 ; g—acceleration due to gravity, m / s 2 ; μ—dynamic viscosity of molten steel, kg / (m·s); d—equivalent diameter of inclusion, m.

[0071] From the above formula, we can know that the limit floating speed of inclusions in molten steel is positively correlated with the size of inclusions and the density difference between molten steel and inclusions. Since the density of inclusions in molten steel is generally lower than that of molten steel, they are removed by floating during the smelting process, so their limit floating speed is negatively correlated with the density of inclusions.

[0072] First, the oxygen and sulfur supply of the alloy raw materials need to be calculated. The calculation formula is as follows:

[0073]

[0074] In the formula, c O / S is the total oxygen and sulfur supply of the alloy raw materials, wt%; c i O / S is the O / S content in the i-th raw material, wt%; C i is the designed content of the ith raw material in the alloy, wt%.

[0075] In order to purify the molten steel, active elements are added after high-temperature refining and the temperature is lowered to near the low-temperature refining temperature. The amount of addition is calculated according to formula (6):

[0076] c H =max(ac O , bc s ) (6)

[0077] In the formula, c H is the amount of active elements added, wt%; c O Total oxygen supply in alloy raw materials, wt%; c S is the total sulfur supply in the alloy raw materials, wt%; a and b are coefficients, which can be determined according to the element mass ratio of the stable oxides and sulfides formed by the selected active elements. When the active element Ca is selected, the oxides and sulfides formed are CaO and CaS respectively, at this time a is 2.5 and b is 1.25.

[0078] If the alloy design composition contains rare earth elements, the amount of active elements added can be reduced according to the amount of rare earth elements added.

[0079]

[0080] In the formula, c RE is the amount of rare earth element added to the alloy, wt%; e is the empirical coefficient, generally 5 to 10.

[0081] Step 2: After the alloy is refined at high temperature, when the melt temperature drops to 10-20°C higher than the low-temperature refining temperature, add small alloy materials (small alloy materials are easily oxidized and burned elements, such as Al, V, B, Ti, rare earth elements, etc.) in batches, and let it stand for 0.5-5 minutes after the liquid level stabilizes; when the temperature continues to drop to 0-10°C higher than the low-temperature refining point, add active elements;

[0082] Step 3: After the liquid level stabilizes, turn off the vacuum pump group, fill the furnace with high-purity argon (volume purity ≥ 99.999%) to 0.2MPa-0.4MPa, then start the bottom blowing argon system and execute the process parameters determined by equations (8)-(15). During the process, the bottom blowing argon pressure can be dynamically adjusted according to the actual state of the liquid level;

[0083] During the low-temperature refining of alloys, the molten pool is stirred by blowing argon from the bottom, forming a cycle in which the middle molten steel floats and the molten steel at the edge of the molten pool sinks, thereby increasing the floating rate of inclusions in the molten steel and adsorbing them on the surface of the crucible when in contact with the crucible, thereby achieving the purpose of purifying the molten steel. The bottom blowing argon process parameters can be calculated according to the following formula:

[0084] 1) Bottom blowing argon flow control

[0085]

[0086] In the formula, τ m is the uniform mixing time of molten steel, s; ε m It is the specific stirring energy W / t.

[0087]

[0088] In the formula, Q 0 is the theoretical bottom blowing argon flow rate, m 3 / s; V 0 is the molar volume of gas under standard conditions, which is 22.4×10- 3 m 3 / mol; G is the weight of molten steel, t; R is the universal gas constant, which is 8.314 J / mol·K; T 1 、T 2 are the argon gas and molten steel temperatures, K; P 1 is the sum of the pressure in the crucible and the pressure of the molten steel on the gas plug, Pa; P 2 is the gas pressure in the crucible, Pa.

[0089] P 2 =P 1 +ρgh (10)

[0090] Where ρ is the density of molten steel, kg / m 3 ; h is the height of molten steel, m.

[0091] Q=fQ 0 (11)

[0092] Where, Q is the bottom blowing argon flow rate, m 3 / s; f is the empirical coefficient, generally ranging from 1 to 2.5.

[0093]

[0094] In the formula, Q Z is the amount of molten steel lifted on the Z horizontal plane, m 3 / s; Z is the depth of molten steel h minus the thickness of the surface stratosphere, generally Z = 0.95h, m.

[0095]

[0096] In the formula, τ c is the steel liquid cycle, s; G is the steel liquid weight, t; Q Z is the amount of molten steel lifted on the Z horizontal plane, m 3 / s; ρ is the density of molten steel, kg / m 3 .

[0097] When determining the bottom blowing argon flow rate, it is necessary to first select the uniform mixing time τ of the molten steel according to the complexity of the high-temperature alloy composition. m , generally between 90s and 200s. If the high-temperature alloy contains a large amount of segregation elements, the uniform mixing time of the molten steel can be appropriately increased. Then, the bottom blowing argon flow rate Q is calculated according to equations (8)-(11). Finally, the molten steel cycle period τ is calculated according to equations (12)-(13): c , if τ is satisfied m ≥3τ c , then the uniform mixing time of molten steel is τ m The selected value and the calculated value of bottom blowing argon flow rate are valid, otherwise re-select the uniform mixing time value of the molten steel and repeat the above steps.

[0098] 2) Bottom blowing argon pressure control

[0099] The bottom blowing argon pressure should satisfy the following relationship:

[0100] P≥P 1 +ΔP (14)

[0101] Where P is the bottom blowing argon pressure, Pa, and ΔP is the total pressure drop from the pressure gauge to the bottom of the crucible, which is generally 20000Pa~70000Pa.

[0102] In the actual production process, the bottom blowing argon pressure can be flexibly adjusted according to formula (14) and the state of bubbles above the molten pool to ensure that the steel liquid level does not fluctuate violently.

[0103] 3) Bottom blowing argon time control

[0104] The bottom blowing time should satisfy the following relationship:

[0105] t = jτ m (15)

[0106] Where, t is the bottom blowing time, s; j is the coefficient, generally 1 to 10; τm is the uniform mixing time of molten steel, s.

[0107] During the production process, active elements can be added after high-temperature refining and adding small materials, and when the temperature drops to near the low-temperature refining point, the vacuum pump group is turned off after the liquid level stabilizes, and high-purity argon gas is filled into the furnace to 0.2MPa~0.4MPa, and then the bottom blowing argon system is turned on, and the process parameters determined by equations (8)-(15) are executed. After that, the bottom blowing argon system is turned off, the vacuum pump group is turned on, the vacuum degree in the furnace is evacuated to a pressure of less than 50Pa, and the temperature is adjusted to the pouring temperature before pouring.

[0108] Step 4: Close the bottom blowing argon system, turn on the vacuum pump group, evacuate the vacuum degree in the furnace to a pressure of less than 50Pa, adjust the temperature to the pouring temperature and then start pouring.

[0109] Below, the present invention is further described in detail by examples.

[0110] Example 1

[0111] DZ417G is a nickel-based precipitation hardening directionally solidified columnar high-temperature alloy. Its composition range, by weight percentage, is: C 0.13~0.22, Cr 8.50~9.50, Co 9.0~11.0, Mo 2.50~3.50, Al 4.80~5.70, Ti4.10~4.70, V 0.60~0.90, B 0.012~0.024, and Ni balance.

[0112] In this embodiment, the master alloy grade DZ417G is smelted, and its specific composition by weight percentage is: C 0.16, Cr8.7, Co 10.2, Mo 2.8, Al 5.3, Ti 4.5, V 0.71, B 0.014, Ni balance. The smelting mass is 400kg, and a 500kg vacuum smelting furnace is used for smelting, and active element Ca is selected for inclusion modification and removal.

[0113] The calculation shows that the O content of the raw materials in the master alloy is about 114 ppm and the S content is about 37 ppm. According to equations (5) and (6), the Ca addition amount is 285 ppm, i.e. 0.0285 wt.%. The added amount is 114 g, which is wrapped in nickel foil for later use.

[0114] Alloy smelting process:

[0115] (1) Alloy raw materials except Al, V, B, Ti and other elements are loaded into the furnace, and when the vacuum degree is reduced to a pressure of 30 Pa, the electrified materials are fed;

[0116] (2) After the charge is cleaned, high temperature refining is carried out at 1500°C for 10 minutes;

[0117] (3) When the melt temperature drops to 1410°C, add elements such as Al, V, B, and Ti, and let it stand for 1 minute after the liquid level stabilizes;

[0118] (4) When the melt temperature drops to around 1400°C (i.e., the low-temperature refining point), add the Ca element;

[0119] (5) After the liquid level stabilizes, turn off the vacuum pump group and fill the furnace with high-purity argon to 0.3 MPa. Then, turn on the bottom blowing argon system and perform low-temperature refining. The bottom blowing argon flow rate is 3.33×10 -4 m 3 / s, that is 0.02m 3 / min. The initial pressure of bottom blowing argon is 400000Pa, i.e. 0.4MPa, which can be adjusted dynamically according to the liquid level state. The bottom blowing argon time is 10min.

[0120] (6) After the bottom blowing argon time meets the requirements, turn off the bottom blowing argon system, turn on the vacuum pump group, evacuate the vacuum degree in the furnace to a pressure of 20Pa, and adjust the temperature to the pouring temperature of 1430℃ for pouring.

[0121] The residual Ca content of the DZ417G alloy ingot obtained by this embodiment is ≤0.0005wt%, which meets the standard requirements. The O, N, S content and the secondary remelting slag area (slag detection according to HB 5406) ​​are compared with those of the traditional process as follows:

[0122] O / ppm N / ppm S / ppm Secondary remelting slag area The present invention 4 4 2 0.5% Traditional crafts 12 10 7 1.68%

[0123] The implementation results show that the present invention proposes a simple and efficient process for removing inclusions in high-temperature alloys. The present invention introduces active elements into the molten steel, and cooperates with the bottom blowing argon system to purify the alloy, ensuring that the O content in the alloy is less than 8ppm, the N content is less than 5ppm, the S content is less than 5ppm, and the active element content is less than 10ppm. The present invention is suitable for the smelting production of most high-temperature alloys, and is suitable for the removal of inclusions in the vacuum induction melting process. It can improve the purity of the alloy, reduce the percentage of alloy remelting slag, and greatly improve the quality of the master alloy product. The economic benefits are significant, and it is of great significance to improve the purity of the master alloy of high-temperature alloys, and has broad application prospects.

Claims

1. A control method for removing inclusions from high temperature alloys, It is characterized in that The specific steps include: The first step is to design the amount of active elements to be added according to equations (1) to (7), and wrap them with Ni foil or Al foil for later use; For fine non-metallic inclusions in molten steel, the relationship between the drag coefficient of the inclusions and the Reynolds number is divided into the Stokes law region, the transition region, and the Newton law region according to the size of the Reynolds number. In different regions, the limit floating rate of non-metallic inclusions meets the requirements of equations (1)-(3): (1) Stokes' law region, Reynolds number Re<1 (2) Transition zone, 1<Re<500 (3) Newton’s law area, 500<Re<2×10 5 Reynolds number formula: Where, v is the limit floating velocity of inclusions, m / s; ρ f —Steel liquid density, kg / m 3 ; ρ k —Inclusion density, kg / m 3 ; g—acceleration due to gravity, m / s 2 ; μ—dynamic viscosity of molten steel, kg / (m·s); d—equivalent diameter of inclusions, m; First, calculate the oxygen and sulfur supply of the alloy raw materials. The calculation formula is as follows: In the formula, c O / S is the total oxygen and sulfur supply of the alloy raw materials, wt%; c i O / S is the O / S content in the i-th raw material, wt%; C i is the designed content of the i-th raw material in the alloy, wt%; Active elements are added after high-temperature refining and the temperature is lowered to near the low-temperature refining temperature. The amount of addition is calculated according to formula (6): c H =max(ac O ,bc s ) (6) In the formula, c H is the amount of active elements added, wt%; c O Total oxygen supply in alloy raw materials, wt%; c S is the total sulfur supply in the alloy raw materials, wt%; a and b are coefficients, which are determined according to the element mass ratio in the stable oxides and sulfides formed by the selected active elements; If the alloy design composition contains rare earth elements, the amount of active elements added should be reduced according to the amount of rare earth elements added; In the formula, c RE is the amount of rare earth element added to the alloy, wt%; e is the empirical coefficient, ranging from 5 to 10; Step 2: After the alloy is refined at high temperature, when the melt temperature drops to 10-20°C higher than the low-temperature refining temperature, add small alloy materials in batches, and let the liquid stand for 0.5-5 minutes after the liquid level stabilizes; when the temperature continues to drop to 0-10°C higher than the low-temperature refining point, add active elements; Step 3: After the liquid level stabilizes, turn off the vacuum pump group, fill the furnace with high-purity argon to 0.2MPa-0.4MPa, and then turn on the bottom blowing argon system. During the low-temperature refining of the alloy, the molten pool is stirred by blowing argon from the bottom, so that a cycle of the middle molten steel floating up and the molten steel at the edge of the molten pool sinking is formed in the molten steel, thereby increasing the floating rate of inclusions in the molten steel, and adsorbing them on the surface of the crucible when in contact with the crucible, so as to purify the molten steel; Step 4: Close the bottom blowing argon system, turn on the vacuum pump group, evacuate the vacuum degree in the furnace to a pressure of less than 50Pa, adjust the temperature to the pouring temperature and then start pouring.

2. The control method for removing high temperature alloy inclusions according to claim 1, It is characterized in that In formula (6), when the active element Ca is selected, the oxide and sulfide formed are CaO and CaS respectively. At this time, a is 2.5 and b is 1.

25.

3. The control method for removing high temperature alloy inclusions according to claim 1, It is characterized in that In the second step, the alloy material is one or more of the easily oxidizable and burnt elements Al, V, B, Ti, and rare earth elements.

4. The control method for removing high temperature alloy inclusions according to claim 1, It is characterized in that In the third step, the bottom blowing argon pressure is dynamically adjusted according to the actual state of the liquid level.

5. The control method for removing high temperature alloy inclusions according to claim 1, It is characterized in that In the third step, the bottom blowing argon flow rate is controlled as follows: In the formula, τ m is the uniform mixing time of molten steel, s; ε m is the specific stirring energy W / t; In the formula, Q 0 is the theoretical bottom blowing argon flow rate, m 3 / s; V 0 is the molar volume of gas under standard conditions, which is 22.4×10 -3 m 3 / mol; G is the weight of molten steel, t; R is the universal gas constant, which is 8.314 J / mol·K; T 1 , T 2 are the argon gas and molten steel temperatures, K; P 1 is the sum of the pressure in the crucible and the pressure of the molten steel on the gas plug, Pa; P 2 is the gas pressure in the crucible, Pa; P 2 =P 1 +ρgh (10) Where ρ is the density of molten steel, kg / m 3 ; h is the height of molten steel, m; Q=fQ 0 (II) Where, Q is the bottom blowing argon flow rate, m 3 / s; f is the empirical coefficient, ranging from 1 to 2.5; In the formula, Q Z is the amount of molten steel lifted on the Z horizontal plane, m 3 / s; Z is the depth of the molten steel h minus the thickness of the surface stratosphere, and Z is taken as 0.95h, m; In the formula, τ c is the steel liquid cycle, s; G is the steel liquid weight, t; Q Z is the amount of molten steel lifted on the Z horizontal plane, m 3 / s; ρ is the density of molten steel, kg / m 3 .

6. The control method for removing high temperature alloy inclusions according to claim 5, It is characterized in that When determining the bottom blowing argon flow rate, first select the uniform mixing time τ of the molten steel according to the complexity of the high-temperature alloy composition. m , between 90s and 200s; then, the bottom blowing argon flow rate Q is calculated according to equations (8)-(11); finally, the steel liquid cycle period τ is calculated according to equations (12)-(13) c , if τ is satisfied m ≥3τ c , then the uniform mixing time of molten steel is τ m The selected value and the calculated value of bottom blowing argon flow rate are valid, otherwise re-select the uniform mixing time value of the molten steel and repeat the above steps.

7. The control method for removing high temperature alloy inclusions according to claim 1, It is characterized in that In the third step, the bottom blowing argon pressure is controlled, and the bottom blowing argon pressure satisfies the following relationship: P≥P l +ΔP (14) Where, P is the bottom blowing argon pressure, Pa, ΔP is the total pressure drop from the pressure gauge to the bottom of the crucible, which is 20000Pa~70000Pa.

8. The control method for removing high temperature alloy inclusions according to claim 7, It is characterized in that In the actual production process, the bottom blowing argon pressure is flexibly adjusted according to formula (14) and the bubble state above the molten pool to ensure that the steel liquid level does not fluctuate violently.

9. The control method for removing high temperature alloy inclusions according to claim 1, It is characterized in that In the third step, the bottom argon blowing time is controlled, and the bottom argon blowing time satisfies the following relationship: t=jτ m (15) Where, t is the bottom blowing time, s; j is the coefficient, ranging from 1 to 10; τ m is the uniform mixing time of molten steel, s.

10. The control method for removing high temperature alloy inclusions according to claim 9, It is characterized in that During the production process, after high-temperature refining and adding small materials, the active elements are added when the temperature drops to near the low-temperature refining point. After the liquid level stabilizes, the vacuum pump group is turned off, and high-purity argon gas is filled into the furnace to 0.2MPa~0.4MPa, and then the bottom blowing argon system is turned on; then the bottom blowing argon system is turned off, the vacuum pump group is turned on, the vacuum degree in the furnace is evacuated to a pressure of less than 50Pa, and the temperature is adjusted to the pouring temperature before pouring.