A Re-doped refractory high-entropy alloy material and preparation method thereof
Through the preparation method of Re-doped refractory high-entropy alloy materials, the problem of insufficient high-temperature phase stability and oxidation resistance of traditional high-temperature alloys is solved, and the improvement of high-temperature applications and the feasibility of industrial production is achieved.
Patent Information
- Application Number
- CN202411280943.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-13
AI Technical Summary
Traditional nickel-based and cobalt-based high-temperature alloys cannot meet the modern industry's demand for high-temperature alloys. The phase stability and oxidation resistance of refractory high-entropy alloys at high temperatures are insufficient, which limits their application.
Using the preparation method of Re-doped refractory high-entropy alloy material, the content of Re is controlled to be 0.5% by wrapping Re particles in Al metal blocks and mixing them with Cr, Mo, Ta, Ti and other elements. ~2% to improve high temperature phase stability and antioxidant properties.
It has achieved the high-temperature phase stability and oxidation resistance of Re-doped high-entropy alloys, and has high- and low-temperature creep resistance, tensile strength and gas corrosion resistance. It is suitable for ultra-high temperature environments, and has simple and controllable processes, suitable for industrialization. Production.
Smart Images

Figure CN118773460B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a Re-doped refractory high-entropy alloy material and a preparation method thereof, belonging to the technical field of refractory high-entropy alloys. Background Art
[0002] Traditional nickel-based superalloys and cobalt-based superalloys can no longer meet the needs of modern industry for superalloys. With the development of advanced aircraft engines and gas turbines, advanced high-temperature structural materials have become the key to improving engine service performance and life, reducing energy consumption and costs. High-temperature hot end components must not only withstand high-temperature oxidation, but also resist severe temperature shocks and strong airflow scouring, which leads to an increasingly urgent demand for new high-temperature structural materials with high operating temperature, high high-temperature strength, good high-temperature stability and strong oxidation resistance.
[0003] The high-temperature stability of refractory high-entropy alloys is particularly important for their high-temperature applications. In recent years, researchers have conducted little research on the phase stability of refractory high-entropy alloys at high temperatures. Elements such as Cr, Co and Al are elements with high negative mixing enthalpy like most refractory metals. They easily form strong interactions with refractory elements in the alloy to form second phases such as Laves phase and B2 phase. As a strengthening phase in refractory high-entropy alloys, Laves phase increases the room temperature and high-temperature yield strength of the alloy while also reducing the room temperature plasticity of the alloy. The B2 phase of the ordered intermetallic compound will reduce the room temperature ductility of the alloy. Therefore, it is particularly important to establish the relationship between the heat treatment process and the high-temperature phase stability of refractory high-entropy alloys.
[0004] High temperature oxidation failure is an important issue that restricts the application of refractory high entropy alloys. Refractory high entropy alloys can serve in extremely harsh environments, but their poor oxidation resistance limits their widespread application. Therefore, improving the high temperature oxidation resistance of refractory high entropy alloys is an urgent problem to be solved, which is of great value to their future practical application and development. Summary of the invention
[0005] In view of the above prior art, the first object of the present invention is to provide a high temperature phase stable and oxidation resistant Re ( )-doped refractory high entropy alloy material, the preparation method provided by the present invention is simple and controllable, and is suitable for industrial production.
[0006] The second object of the present invention is to provide a Re-doped refractory high entropy alloy material prepared by the above preparation method. The refractory high entropy alloy material provided by the present invention has excellent high temperature phase stability and oxidation resistance.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] The present invention provides a method for preparing a Re-doped refractory high entropy alloy material, wherein Re ( ) particles and Al particles, and divided them into several portions, taking any portion of Al particles and melting them to obtain aluminum melt, adding any portion of Re particles, and cooling to obtain an Al metal block wrapping the Re particles, repeating the above process to obtain several Al metal blocks wrapping the Re particles, mixing Cr powder, Mo powder, Ta powder, and Ti powder to obtain mixed powder, dividing the mixed powder into N portions, and pressing them into N powder blocks of different sizes, placing several Al metal blocks wrapping the Re particles at the bottom of a smelting furnace, and then placing N powder blocks above the several Al metal blocks wrapping the Re particles, and finally smelting to obtain a Re-doped refractory high entropy alloy material;
[0009] The chemical expression of the Re-doped refractory high entropy alloy material is AlCrMoTaTiRe, wherein the atomic percentage of Re is 0.5% to 2%, preferably 1 to 2%.
[0010] The Re-doped refractory high-entropy alloy material provided by the present invention has Re element enriched on the dendrites, which can protect the matrix structure and improve the high-temperature phase stability of the matrix. The Re element will be enriched in the oxide film position in the form of filling, inhibiting the inward diffusion of oxygen and nitrogen, reducing internal oxidation, thereby improving the oxidation resistance of the refractory high-entropy alloy, so that the refractory high-entropy alloy material provided by the present invention has excellent high-temperature phase stability and oxidation resistance. The Re element will promote the precipitation of the Cr-rich phase, increase the Cr2Ta phase in the alloy, and although it will increase the hardness of the alloy, it will also deteriorate the plasticity of the alloy. Therefore, the content of the doped Re element needs to be controlled within the scope of the present invention.
[0011] Re and its alloys have excellent properties such as good high and low temperature creep resistance, high high temperature tensile strength and creep rupture strength, no brittle critical transition temperature, not easy to form compounds with carbon, good gas corrosion resistance, etc., and are suitable for ultra-high temperature and strong thermal shock working environments. However, the melting point of Re element is as high as 3186 ℃, which is very different from the melting point of elements in AlCrMoTaTi refractory high entropy alloy. The setting of current parameters and the control of time during smelting need to be very precise, and high melting point particles are prone to splashing and will take away part of the melted metal, making the smelted alloy deviate greatly from the designed composition.
[0012] The present invention firstly reduces the loss of Al and Re by wrapping Re particles into molten Al, and prepares a plurality of metal blocks wrapping Re particles at the same time. This is because dividing the required mass of Re into a plurality of small blocks can make Re melt faster, reduce the mass loss caused by splashing, improve the smelting efficiency, and also make the Re particles more evenly distributed. In addition, other metal elements are added by mixing powder and pressing powder into blocks to promote full mixing between metals, so that the composition of the smelted alloy is more uniform and the deviation between the smelted alloy and the designed composition is avoided.
[0013] In a preferred solution, the particle sizes of the Al particles and the Re particles are both 1-2 mm. The inventors have found that the particle sizes of the Al particles and the Re particles are controlled within the above range, and the final smelting effect is optimal. If the particle size is too large, uneven metal mixing, uneven heating, and severe smoke and volatilization will occur; if the particle size is too small, splashing will occur, causing loss, resulting in deviation of the composition of the sample after smelting from the designed ratio.
[0014] The preferred solution is to match Re according to the design ratio ( ) particles and Al particles, and divided them into 3 to 6 portions. The inventors found that Re ( ) particles and Al particles are divided into the above-mentioned number, and the final smelting effect is optimal.
[0015] In the actual operation process, Al particles and Re particles need to first use an electric grinder to remove impurities and oxide scale on the metal surface, and then put the Al and Re particles into alcohol for ultrasonic cleaning for 5 minutes, and then put them into clean water for ultrasonic cleaning for 5 minutes. After cleaning, they are placed in a drying oven at a constant temperature of 70 ℃ for 2 hours for use.
[0016] A preferred solution is to melt any Al particles at 720-750°C to obtain an aluminum melt, keep the temperature for 10-15 minutes, add any Re particles, stir evenly, keep the temperature for 5-8 minutes, and cool to obtain an Al metal block encapsulating the Re particles.
[0017] The inventors found that after adding Re particles, stirring evenly and then keeping warm for 5-8 minutes can allow the gas to be discharged and reduce the holes in the smelting process.
[0018] In a preferred embodiment, the particle size of the Cr powder, Mo powder, Ta powder and Ti powder is less than 300 mesh.
[0019] In the present invention, the purity of the metal raw materials used is ≥ 99.9%.
[0020] In a preferred embodiment, Cr powder, Mo powder, Ta powder and Ti powder are mixed in a mixer for 8-10 hours to obtain a mixed powder.
[0021] In a preferred embodiment, the mixed powder is divided into three portions and pressed into three powder blocks with diameters of φ1-1.5 mm, φ2-2.5 mm, and φ3-3.5 mm, respectively.
[0022] The inventors have found that the use of briquettes of the above sizes can achieve the best smelting effect and the performance of the refractory high-entropy alloy material finally obtained is the best.
[0023] Further preferably, a pressure of 200-250 MPa is used for pressing a φ1-1.5 mm powder block, and the pressing time is 2-3 min; a pressure of 300-350 MPa is used for pressing a φ2-2.5 mm powder block, and the pressing time is 2-3 min; a pressure of 400-450 MPa is used for pressing a φ3-3.5 mm powder block, and the pressing time is 2-3 min.
[0024] Greater pressure and time can make the powder pressed more compactly. The above-mentioned powder blocks of different sizes use the above-mentioned different pressures to obtain corresponding compactness, and the final smelting effect is optimal.
[0025] The preferred solution is to place φ3-3.5 mm, φ2-2.5 mm, and φ1-1.5 mm powder blocks on top of several Al metal blocks wrapped with Re particles from bottom to top. The inventors found that by placing the large-sized blocks at the bottom and the small-sized blocks at the top, the small-sized blocks can fill some gaps between the large-sized blocks, so that the blocks are in close contact with each other, increasing the contact area, and thus making the smelting more uniform.
[0026] If only a single block is used to obtain the granular raw material and directly smelt it, the smelting time will be increased, and pores and cracks will be easily generated, which will reduce the smelting efficiency and cause the loss of components.
[0027] Preferably, the smelting method is vacuum arc melting.
[0028] In a preferred embodiment, the smelting process is as follows: gradually increasing the current to 470-500 A at a rate not exceeding 5 A / s to obtain a melt, turning the melt over after 3-5 minutes of smelting, turning the resulting alloy block over after a single smelting, and repeating the above smelting operation, smelting repeatedly for 15-17 times, and cooling to room temperature for 15-20 minutes to obtain the melt. In the smelting process of the present invention, the current speed needs to be effectively controlled. Too fast an increase in the current speed will lead to uneven smelting and stress concentration, thereby causing holes and cracks in the alloy.
[0029] During the design and operation process, the furnace is first vacuumed, and high-purity argon gas with a purity of 99.99% is introduced into the furnace until the surface pressure in the furnace reaches -0.05 MPa. Then the current is gradually increased for smelting.
[0030] Preferably, after obtaining the melt, electromagnetic stirring is applied. By applying electromagnetic stirring, the composition of the smelted alloy can be made more uniform.
[0031] In a preferred embodiment, the Re-doped refractory high entropy alloy material has the following composition, calculated by atomic percentage: Al 19.6% to 19.9%, Cr 19.6% to 19.9%, Ti 19.6% to 19.9%, Ta 19.6% to 19.9%, Mo 19.6% to 19.9%, and Re 0.5% to 2%.
[0032] The present invention also provides a Re-doped refractory high-entropy alloy material prepared by the above preparation method.
[0033] In a preferred embodiment, the Re-doped refractory high entropy alloy material has a dendritic structure, the dendrites are composed of a BCC phase, and the interdendritic region is composed of a B2-type solid solution phase and a precipitation phase Cr2Ta phase.
[0034] The Re-doped refractory high-entropy alloy material provided by the present invention has the Re element enriched on the dendrites, which can protect the matrix structure and improve the high-temperature phase stability of the matrix. The Re element is enriched in the oxide film position in the form of filling, inhibiting the inward diffusion of oxygen and nitrogen, reducing internal oxidation, and thus improving the oxidation resistance of the refractory high-entropy alloy.
[0035] Compared with the existing technology, the present invention has the following beneficial effects:
[0036] 1. The present invention provides a method for preparing a Re-doped refractory high-entropy alloy material. Conventional arc melting will cause a large amount of Al metal loss due to the large difference in melting points between alloys, resulting in the alloy composition not meeting the designed ratio. By wrapping Re particles into molten Al, the loss of Al and Re can be reduced at the same time. The method of mixing powder and powder briquetting can make the metals fully mixed, and the alloy composition of the smelted alloy is more uniform. The method provided by the present invention has simple process, easy operation, low loss, less pollution, and is suitable for large-scale industrial production.
[0037] 2. The present invention further optimizes the composition ratio of a Re-doped refractory high-entropy alloy material, so that the high-entropy alloy has good high-temperature phase stability and oxidation resistance. When the Re content is 2%, the high-entropy alloy material can stabilize the matrix BCC phase well below 1200°C and inhibit the growth of the B2 ordered phase; when the Re content is 1%, the high-entropy alloy material still has the effect of stabilizing the matrix phase and inhibiting the B2 phase below 1200°C, and the unit area mass gain after oxidation at 1000°C for 12 h does not exceed 0.54 mg / cm 2The optimization of Re addition can make AlCrMoTaTiRe refractory high entropy alloy material have good high temperature phase stability and oxidation resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.
[0039] Figure 1 X-ray diffraction spectra of the refractory high entropy alloys prepared in Example 1, Example 2 and Comparative Example 1.
[0040] Figure 2 The microstructures of the refractory high entropy alloys prepared in Example 1, Example 2 and Comparative Example 1 before and after high temperature heat treatment are shown in Figure 1; wherein: (a) is the AlCrMoTaTi alloy as-cast prepared in Comparative Example 1; (b) is the AlCrMoTaTi alloy prepared in Comparative Example 1 annealed at 1000 °C; (c) is the AlCrMoTaTi alloy prepared in Comparative Example 1 annealed at 1200 °C; (d) is the AlCrMoTaTiRe prepared in Example 1 0.05 Alloy cast; (e) AlCrMoTaTiRe prepared in Example 1 0.05 Alloy annealing 1000 ℃; (f) is AlCrMoTaTiRe prepared in Example 1 0.05 Alloy annealing 1200 ℃; (g) is AlCrMoTaTiRe prepared in Example 2 0.1 Alloy cast; (h) AlCrMoTaTiRe prepared in Example 2 0.1 Alloy annealing 1000 ℃; (i) AlCrMoTaTiRe prepared in Example 2 0.1 Alloy annealing at 1200 °C.
[0041] Figure 3 Surface states of the samples of the refractory high entropy alloys prepared in Example 1 and Comparative Example 1 after being oxidized at 1000°C for 12 hours.
[0042] Figure 4 X-ray diffraction spectra of the refractory high entropy alloys prepared in Example 1 and Comparative Example 1 after being oxidized at 1000°C for 12 hours.
[0043] Figure 5 Continuous weight gain curves of the refractory high entropy alloys prepared in Example 1 and Comparative Example 1 after oxidation at 1000°C for 12 hours.
[0044] Figure 6 Surface microstructure of the refractory high entropy alloys prepared in Example 1 and Comparative Example 1 after oxidation at 1000°C for 12 hours.
[0045] Figure 7 The microstructure and element distribution of the oxide layer cross section of the refractory high entropy alloy prepared in Comparative Example 1 after oxidation at 1000°C for 12 hours.
[0046] Figure 8 The microstructure and element distribution of the oxide layer cross section of the refractory high entropy alloy prepared in Example 1 after being oxidized at 1000°C for 12 hours. DETAILED DESCRIPTION
[0047] The present invention is described in detail below with reference to the accompanying drawings and embodiments.
[0048] Example 1
[0049] This embodiment provides an AlCrMoTaTiRe 0.05 The preparation process of refractory high entropy alloy material includes the following steps:
[0050] (1) Ingredients: Al particles, Re particles, Cr metal powder, Ti metal powder, Ta metal powder, and Mo metal powder with a purity of ≥ 99.9% are selected. The particle size of Al particles and Re particles is 1-2 mm, and the particle size of Cr metal powder, Ti metal powder, Ta metal powder, and Mo metal powder is less than 300 mesh. The mass of a single smelted button ingot is 50 g. According to the atomic ratio of Al:Cr:Mo:Ta:Ti:Re=19.8%:19.8%:19.8%:19.8%:19.8%:19.8%, it is converted to a mass ratio of Al:Cr:Mo:Ta:Ti:Re=6.53%:12.59%:23.22%:43.8%:11.59%:2.28%. The required masses are: Al -3.265g; Cr -6.293g; Mo -11.611g; Ta -21.899g; Ti -5.795g; Re -1.138g.
[0051] (2) Al-molten coating: Use an electric grinder to remove impurities and oxide scale on the metal surface of Al and Re particles. Place Al and Re particles in alcohol for ultrasonic cleaning for 5 min, then place them in clean water for ultrasonic cleaning for 5 min. After cleaning, place them in a drying oven at a constant temperature of 70 °C for 2 h. Melt Al particles at 750 °C, keep them in a molten state for 10 min, add Re particles, stir them thoroughly, keep them in a molten state for 8 min, and wait for them to cool to obtain an Al metal block that wraps Re particles. Use the same method to make 5 Al metal blocks that wrap Re particles.
[0052] (3) Powder briquetting: Mix the Cr, Mo, Ta, and Ti metal powders in a mixer for 8 h, then put them into a hydraulic press and press them at a pressure of 200 MPa for 3 min to form powder blocks with a diameter of 1 mm. Press them at a pressure of 300 MPa for 3 min to form powder blocks with a diameter of 2 mm. Press them at a pressure of 400 MPa for 3 min to form powder blocks with a diameter of 3 mm.
[0053] (4) Arc melting: Place the Al metal block wrapped with Re particles at the bottom of a water-cooled copper mold in a vacuum arc melting furnace. Then, place pressed powder blocks of φ3 mm, φ2 mm, and φ1 mm in order from bottom to top on one side of the Al metal block wrapped with Re particles. Evacuate the furnace. Pass high-purity argon gas with a purity of 99.99% into the furnace until the pressure inside the furnace reaches -0.05 MPa. Gradually increase the current to 470 A at a rate of 4.8 A / s to melt the block to obtain a melt. Turn on the electromagnetic stirring for stirring. After a single melting lasts for 3 minutes, turn it over. Continue melting and flipping for 17 times. After the melting is completed, cool it to room temperature and wait for 20 minutes to obtain AlCrMoTaTiRe with high temperature phase stability and oxidation resistance. 0.05 Refractory high entropy alloys.
[0054] Example 2
[0055] This embodiment provides an AlCrMoTaTiRe 0.1 The preparation process of the refractory high entropy alloy material is the same as that of Example 1, except that the ratios of the alloy elements are different. The mass of a single smelted button ingot is 50 g. According to the atomic ratio of Al:Cr:Mo:Ta:Ti:Re=19.6%:19.6%:19.6%:19.6%:19.6%:2%, the mass ratio is changed to Al:Cr:Mo:Ta:Ti:Re=6.38%:12.3%:22.69%:42.8%:11.33%:4.49%, and the required masses are: Al-3.191g; Cr-6.15g; Mo-11.347g; Ta-21.401g; Ti-5.663g; Re-2.247g.
[0056] Comparative Example 1
[0057] An AlCrMoTaTi refractory high entropy alloy material, the preparation process of which is consistent with that of Example 1, except that the Re element is not added and the ratio of the alloy elements is also different. The mass of a single smelted button ingot is 50 g, and the atomic ratio is Al:Cr:Mo:Ta:Ti=20%:20%:20%:20%:20%, which is converted to a mass ratio of 6.68%:12.88%:23.76%:44.82%:11.86%, and the required masses are: Al-3.341g; Cr-6.439g; Mo-11.881g; Ta-22.409g; Ti-5.929g.
[0058] Comparative Example 2
[0059] The other conditions are the same as those in Example 1, except that powder briquetting is not used. Al particles wrapped with Re particles are directly placed at the bottom of a water-cooled copper mold, and then Ti, Cr, Mo, and Ta particles are placed in order from low to high melting points. The smelted alloy block has uneven composition distribution and many cracks and pores.
[0060] Comparative Example 3
[0061] The other conditions were the same as those in Example 1, except that the alloy block was not wrapped with molten Al. Instead, the Al particles were placed directly at the bottom of the water-cooled copper mold, the powder compact was placed above the Al particles, and then the Re particles with the highest melting point were placed on the top for smelting. It was found that the particles splashed severely and the smelting failed.
[0062] Comparative Example 4
[0063] The other conditions were the same as those in Example 1. Instead of using the method of powder briquetting and molten Al to wrap the alloy block, Al, Ti, Cr, Mo, Ta, and Re were directly added in order from low to high melting points. It was found that smoke and volatilization occurred during the smelting process, and particles splashed, indicating that the smelting failed.
[0064] Performance Testing
[0065] (1) Heat treatment: The alloys melted in Example 1, Example 2 and Comparative Example 1 were cut into 5.2*5.2*3.2 mm pieces by wire electric discharge cutting. 3cube; polish the sample with SiC sandpaper in the order of #400, #800, #1000, #1500, and #2000 until a mirror surface appears on the sample surface; then polish with SiO2 polishing liquid until no obvious scratches can be seen under an optical microscope; ultrasonically clean the sample in acetone for 5 min, and then continue to ultrasonically clean the sample with clean water for 5 min; dry it in a drying oven at a constant temperature of 70°C for 2 h; put the dried sample in an Al2O3 crucible and place it in a tubular furnace for heat treatment. High-purity argon gas with a purity of 99.99% is introduced into the tubular furnace to prevent the sample from being oxidized. The tubular furnace is set to heat up to 1000°C and 1200°C at a heating rate of 5°C / min, respectively, and kept warm for 20 h, and then cooled to room temperature with the furnace and taken out.
[0066] The X-ray diffraction spectra of the refractory high entropy alloy materials prepared in Example 1, Example 2 and Comparative Example 1 are as follows: Figure 1 All three alloys are composed of three phases: BCC type plus B2 type solid solution phase and precipitation phase Cr2Ta phase. It can be seen that the addition of Re element does not change the phase composition of the original AlCrMoTaTi system.
[0067] The microstructures of the refractory high entropy alloy materials obtained in Example 1, Example 2 and Comparative Example 1 before and after high temperature heat treatment are as follows: Figure 2 shown. Figure 2 (a) is the cast structure of the AlCrMoTaTi alloy prepared in Comparative Example 1, which is mainly composed of the dendritic BCC phase in the light-colored part and the interdendritic B2 phase in the dark-colored part. Figure 2 (b) is the microstructure of the AlCrMoTaTi alloy prepared in Comparative Example 1 after annealing at 1000 °C. After annealing at 1000 °C, the dendritic crystal structure becomes coarse and the distribution of the dark B2 phase becomes dispersed. Figure 2 (c) is the microstructure of the AlCrMoTaTi alloy annealed at 1200 °C prepared in Comparative Example 1. It can be seen that the dendrite structure becomes further coarsened, the BCC phase growth area is smaller, and the interdendritic area is further expanded, that is, the volume fraction of the B2 phase increases, and there are many precipitates in the interdendritic area, that is, the formation of the Cr2Ta phase. Figure 2 (d) AlCrMoTaTiRe prepared in Example 1 0.05 The as-cast structure of the alloy is the same as that of the alloy prepared in Comparative Example 1, both of which are dendritic crystal structures, the light-colored part is the BCC phase, and the dark-colored part is the B2 phase. Figure 2 (e) AlCrMoTaTiRe prepared in Example 1 0.05 The alloy was annealed at 1000 ℃. It can be seen that the dendritic crystal structure of the alloy with the addition of Re element grows more regularly and is more concentrated. Figure 2 (f) is AlCrMoTaTiRe prepared in Example 1 0.05The alloy was annealed at 1200 °C. The alloy had an obvious dendritic structure and a relatively fine structure. The BCC phase grew more densely. The volume of the B2 phase was smaller than that of the alloy prepared in Comparative Example 1. The Cr2Ta phase also precipitated in the interdendritic region. Figure 2 (g) is AlCrMoTaTiRe prepared in Example 2 0.1 The cast structure of the alloy also has a dendritic crystal structure, and the dendrites grow relatively regularly. Figure 2 (h) is AlCrMoTaTiRe prepared in Example 2 0.1 The alloy was annealed at 1000 ℃ and the dendrite structure was complete and regular, with concentrated distribution of BCC phase and B2 phase. Figure 2 (i) AlCrMoTaTiRe prepared in Example 2 0.1 The alloy was annealed at 1200 ℃. Compared with the alloy of comparative example 1 without adding Re element, the dendrite structure distribution is relatively denser, the volume fraction of BCC phase is significantly increased, the volume fraction of B2 phase is significantly reduced, and the Cr2Ta phase is also distributed in the interdendritic region.
[0068] (2) Oxidation test: The alloys melted in Example 1 and Comparative Example 1 were cut into 5.2*5.2*10.2 mm pieces by wire electric discharge cutting. 3 cube; polish the sample with SiC sandpaper in the order of #400, #800, #1000, #1500, and #2000 until a mirror surface appears on the sample surface; then polish with SiO2 polishing liquid until no obvious scratches can be seen under an optical microscope; ultrasonically clean the sample in acetone for 5 min, and then continue to ultrasonically clean the sample with clean water for 5 min; dry it in a drying oven at a constant temperature of 70 ℃ for 2 h; weigh the net weight of the dried sample with an electronic balance with an accuracy of 0.00001, place the sample in an Al2O3 crucible, and weigh the total weight of the sample and the crucible; place the crucible in a tubular furnace at 1000 ℃ for 12 h of oxidation test, take out the sample every two hours, cool it to room temperature, and then weigh it.
[0069] The refractory high entropy alloy materials prepared in Example 1 and Comparative Example 1 were oxidized at 1000°C for 12 hours. The surface conditions of the samples before and after oxidation were as follows: Figure 3 It can be seen that the samples of the two alloys remain intact after oxidation, with no obvious oxide shedding on the surface, and have good oxidation resistance.
[0070] The X-ray diffraction spectra of the refractory high entropy alloy materials obtained in Example 1 and Comparative Example 1 after oxidation at 1000°C for 12 hours are as follows: Figure 4 As shown in Figure 2, both alloys produced four oxidation products: Al2O3, TiO2, Cr2O3, and CrTaO4.
[0071] The continuous weight gain curves of the refractory high entropy alloy materials obtained in Example 1 and Comparative Example 1 after oxidation at 1000 °C for 12 h are as follows: Figure 5 The AlCrMoTaTi alloy prepared in Comparative Example 1 has an oxidation weight gain of 0.710708001 mg / cm after 12 hours of continuous oxidation. 2 , the oxidation rate is 0.05922566675 mg / cm 2 h, according to the oxidation resistance rating standard for steel and alloys provided in GB / T13303-1991 as shown in Table 1, the high entropy alloy belongs to the oxidation resistance level; AlCrMoTaTiRe prepared in Example 1 0.05 After 12 hours of continuous oxidation, the weight gain of the alloy was only 0.530567595 mg / cm 2 , the oxidation rate is 0.04421396625 mg / cm 2 h. According to the oxidation resistance rating standard for steel and alloys provided in GB / T13303-1991 as shown in Table 1, the high entropy alloy belongs to the oxidation resistance level. Compared with comparative example 1, the oxidation weight gain of example 1 is reduced by 0.180140406 mg / cm 2 The oxidation rate decreased by 0.0150117005 mg / cm 2 ·h.
[0072] It can be seen that the appropriate addition of Re element can reduce oxidation weight gain, improve the high-temperature oxidation resistance of AlCrMoTaTi alloy, and extend the high-temperature service life of the alloy.
[0073]
[0074] The surface microstructures of the refractory high entropy alloy materials obtained in Example 1 and Comparative Example 1 after oxidation at 1000 °C for 12 h are as follows: Figure 6 The microstructure and element distribution of the cross section are shown in Figure 7 , 8 shown. Figure 6 (a) is the surface microstructure of the AlCrMoTaTi alloy prepared in Comparative Example 1 after oxidation. It can be seen that there are many lumpy protruding oxides in the interdendritic region, and the surface of the oxide layer is not very flat and uniform. Figure 7 The microstructure and element distribution of the oxidized cross section of Comparative Example 1 show that there are many pores in the Al2O3 and Cr2O3 layers, which accelerates the diffusion of oxygen and nitrogen into the interior and leads to severe internal oxidation. Figure 6 (b) AlCrMoTaTiRe prepared in Example 1 0.05 The surface microstructure of the alloy after oxidation shows that compared with Comparative Example 1, the oxidized surface has fewer protruding oxides and the oxide layer is smoother and more uniform. Figure 8 The microstructure and element distribution of the oxidized cross section of Example 1. The Re element diffuses into the oxide layer in the form of filling, supplementing part of the voids in the CrTaO4 layer, which is beneficial to inhibiting the inward diffusion of oxygen and nitrogen, protecting the base alloy from oxidation, and greatly reducing the internal oxidation phenomenon.
[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a Re-doped refractory high entropy alloy material, characterized in that: Re particles and Al particles are prepared according to the designed ratio and divided into several portions, any portion of Al particles is melted to obtain aluminum melt, any portion of Re particles is added, and an Al metal block wrapping the Re particles is obtained after cooling, and the above process is repeated to obtain several Al metal blocks wrapping the Re particles, Cr powder, Mo powder, Ta powder, and Ti powder are mixed to obtain mixed powder, and the mixed powder is divided into 3 portions, and pressed into 3 powder blocks with diameters of φ1-1.5 mm, φ2-2.5 mm, and φ3-3.5 mm, respectively; several Al metal blocks wrapping the Re particles are placed at the bottom of a smelting furnace, and then powder blocks of φ3-3.5 mm, φ2-2.5 mm, and φ1-1.5 mm are placed in sequence from bottom to top above the several Al metal blocks wrapping the Re particles, and finally smelting is performed to obtain Re-doped refractory high entropy alloy materials; The chemical expression of the Re-doped refractory high entropy alloy material is AlCrMoTaTiRe, wherein the atomic percentage of Re is 0.5% to 2%.
2. The method for preparing a Re-doped refractory high entropy alloy material according to claim 1, characterized in that: The particle sizes of the Al particles and the Re particles are both 1-2 mm; Prepare Re particles and Al particles according to the designed ratio and divide them into 3 to 6 portions; Take any Al particles and melt them at 720-750°C to obtain aluminum melt. After keeping the temperature for 10-15 minutes, add any Re particles and stir evenly. After keeping the temperature for 5-8 minutes, cool the mixture to obtain an Al metal block encapsulating the Re particles.
3. The method for preparing a Re-doped refractory high entropy alloy material according to claim 1 or 2, characterized in that: The particle size of the Cr powder, Mo powder, Ta powder and Ti powder is less than 300 mesh; Mix Cr powder, Mo powder, Ta powder and Ti powder in a mixer for 8-10 h to obtain mixed powder.
4. The method for preparing a Re-doped refractory high entropy alloy material according to claim 3, characterized in that: The φ1-1.5 mm powder block is pressed at a pressure of 200-250 MPa for 2-3 min; the φ2-2.5 mm powder block is pressed at a pressure of 300-350 MPa for 2-3 min; the φ3-3.5 mm powder block is pressed at a pressure of 400-450 MPa for 2-3 min.
5. The method for preparing a Re-doped refractory high entropy alloy material according to claim 1 or 2, characterized in that: The smelting method is vacuum arc melting; The smelting process is as follows: gradually increasing the temperature to 470-500 A at a speed not exceeding 5A / s to obtain a melt, turning over after smelting for 3-5 minutes, turning over the obtained alloy block after a single smelting is completed, and repeating the above smelting operation, repeatedly smelting for 15-17 times, and cooling to room temperature for 15-20 minutes to obtain the alloy block.
6. The method for preparing a Re-doped refractory high entropy alloy material according to claim 5, characterized in that: After the melt is obtained, electromagnetic stirring is applied.
7. The method for preparing a Re-doped refractory high entropy alloy material according to claim 1 or 2, characterized in that: The Re-doped refractory high entropy alloy material has the following composition, calculated by atomic percentage: Al 19.6% to 19.9%, Cr 19.6% to 19.9%, Ti 19.6% to 19.9%, Ta 19.6% to 19.9%, Mo 19.6% to 19.9%, and Re 0.5% to 2%.
8. A Re-doped refractory high-entropy alloy material prepared by the preparation method according to any one of claims 1 to 7.
9. The Re-doped refractory high entropy alloy material according to claim 8, characterized in that: The Re-doped refractory high-entropy alloy material has a dendrite structure, the dendrites are composed of a BCC phase, and the interdendritic region is composed of a B2-type solid solution phase and a precipitation phase Cr2Ta phase.
Citation Information
Patent Citations
High-plasticity and high-strength hexabasic refractory high-entropy alloy and verification method thereof
CN107619982A
Preparation method of refractory high-entropy alloy powder
CN112893852A
Method for improving high-temperature oxidation resistance of AlCrMoTaTi refractory high-entropy alloy through microalloying
CN115838890A
HIGH-ENTROPY AlCrTiV ALLOYS
US20180119255A1
BCC dual phase refractory superalloy with high phase stability and manufacturing method therefore
US20210301375A1