Melt iron-rich phase modification treatment method and regenerated aluminum alloy preparation method
By eliminating the nucleation sites of the iron-rich phase in the aluminum alloy melt and adding modifiers to form spherical intermetallic compounds, the problem of iron-rich phase morphology in recycled aluminum alloys is solved, the strength and toughness of the material are significantly improved, and the High-performance preparation of recycled aluminum alloys.
Patent Information
- Application Number
- CN202411258868.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-10-15
AI Technical Summary
Existing technologies cannot effectively improve the morphology of the iron-rich phase in recycled aluminum alloys, resulting in a decrease in the mechanical properties of the material, and existing modification methods are only applicable to alloys with specific compositions or are not applicable to recycled aluminum alloys.
By heating the aluminum alloy melt to 700-1200°C, the nucleation sites of the iron-rich phase are eliminated, and 0.1-5.0% modifier is added to form spherical intermetallic compounds as heterogeneous nucleation sites to change the iron-rich phase. The growth mode forms a spheroidized and diffusely distributed second phase structure.
It significantly improves the strength and fracture toughness of recycled aluminum alloys, avoids stress concentration and crack expansion, improves the mechanical properties of the material, allows recycled aluminum alloys to be used without downgrading, and enhances the added value of scrap aluminum resource utilization.
Smart Images

Figure CN118773469A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy melt processing, and in particular relates to a melt iron-rich phase modification processing method and a recycled aluminum alloy preparation method. Background Art
[0002] The iron-rich phase in recycled aluminum alloys is mostly in the form of needles, laths or networks, which can easily cause stress concentration and seriously deteriorate the mechanical properties of the material.
[0003] When the iron content in the recycled aluminum alloy is high, the iron-rich phase in the alloy transforms into a phase with a higher melting point. Due to the complex composition of scrap aluminum, the types and morphologies of the iron-rich phases in different grades of organization are different. The iron-rich phases with higher melting points, such as β-Fe phase, FeAl3 and Fe2Al5 phase, are mostly in the shape of long needles and laths, which have a great impact on the performance of recycled products after inheritance. Therefore, recycled aluminum alloys can only be downgraded for utilization.
[0004] Chinese patent CN115433859B discloses a method for modifying a deformed aluminum alloy based on a rare earth alloy, which introduces the content of Mn and Fe to transform the iron-rich phase into a Chinese character shape, reduce its cutting effect on the matrix, and improve the hot cracking resistance through arc additive manufacturing. However, the patent introduces Mn and V and limits the elemental composition and content of the aluminum alloy, which cannot achieve the improvement of the alloy performance for a specific grade. Arc additive manufacturing can only improve hot cracking resistance and is not suitable for the production and preparation of recycled aluminum alloys.
[0005] Chinese patent CN113088732B discloses a rare earth metal doped composite modifier and its preparation method, which improves the narrow needle-like structure of Si phase in Al-Si alloy after gravity casting by using the modifier method, transforms eutectic silicon into fine fibers, and solves the problem of Sr easy to absorb air and causes porosity and other casting defects. However, this method is only applicable to Si modification of specific Al-Si alloys, cannot improve the iron-rich phase structure, and is not suitable for the modification of recycled aluminum alloys.
[0006] The existing modification methods only modify the Si phase and refine the grains of alloys with specific components, but cannot improve the morphology of the iron-rich phase in the recycled aluminum alloy.
[0007] In summary, the prior art obviously has inconveniences and defects in practical use, so it is necessary to improve it. Summary of the invention
[0008] In view of the above-mentioned defects, the present invention mainly provides a method for modifying the iron-rich phase in the melt to solve the technical problem that the iron-rich phase in the recycled aluminum alloy melt forms harmful structural morphology and deteriorates the mechanical properties of the material.
[0009] In order to solve the above problems, the present invention provides a method for treating a molten iron-rich phase by modification, comprising the following steps: S1, heating the aluminum alloy melt to 700-1200°C and keeping the temperature for 10-60 min; completely melting the iron-rich phase in the melt and eliminating the nucleation sites in the iron-rich phase; S2, adding 0.1-5.0% by mass of a modifier to the aluminum alloy melt; The modifier and the aluminum element in the melt form a large number of spherical intermetallic compounds with high melting points, which are dispersed in the melt and become heterogeneous nucleation sites for the growth of the iron-rich phase.
[0010] According to the melt iron-rich phase modification treatment method of the present invention, the modifier is a single substance form of one or more elements of lanthanum La, cerium Ce, praseodymium Pr, neodymium Nd, promethium Pm, samarium Sm, europium Eu, gadolinium Gd, terbium Tb, dysprosium Dy, holmium Ho, erbium Er, thulium Tm, ytterbium Yb, lutetium Lu, yttrium Y, scandium Sc, zirconium Zr, titanium Ti, and boron B.
[0011] According to the melt iron-rich phase modification treatment method of the present invention, the amount of the modifier added is: 0.1-2.0%; the insulation temperature is: 700-900°C, and the insulation time is: 10-30min.
[0012] According to the molten iron-rich phase modification treatment method of the present invention, the modifier is an aluminum-based intermediate alloy with two elements, including: Al-Ti-B, Al-Er-B, Al-B-La, Al-Ti-Y, Al-Sc-Pr, Al-La-Ce, Al-Nd-Y, Al-Er-Ti, Al-Er-Y, Al-La-Ti, Al-Ce-Y, Al-Ce-Tb, Al-Sm-Y and Al-Ce-B.
[0013] According to the melt iron-rich phase modification treatment method of the present invention, the amount of the modifier added is: 2.1-3.4%; the insulation temperature is: 900-1030° C., and the insulation time is: 30-43 minutes.
[0014] According to the melt iron-rich phase modification treatment method of the present invention, the modifier is an intermediate alloy synthesized with aluminum as the base and three elements, including: Al-Y-Zr-Ti, Al-Ce-Tb-Z, Al-La-Ce-B, Al-Ce-Sc-B, Al-Sm-YB, Al-Er-Y-Sc, Al-Er-Nd-Sc and Al-Zr-Ti-B.
[0015] According to the melt iron-rich phase modification treatment method of the present invention, the amount of the modifier added is: 3.5-4.2%; the insulation temperature is: 1040-1110°C, and the insulation time is: 44-51min.
[0016] According to the melt iron-rich phase modification treatment method of the present invention, the modifier is an intermediate alloy synthesized with aluminum as the base and four elements, including: Al-La-Y-Ti-B, Al-Ce-Y-Zr-Ti, Al-Nd-Sc-Zr-B, Al-Ce-Nd-Sc-Ti, Al-Nd-Er-Sc-B, Al-Ho-Er-Sc-B, Al-La-Y-Ti-B, Al-La-Nd-Er-Y and Al-Ce-Er-YB-Ti.
[0017] According to the melt iron-rich phase modification treatment method of the present invention, the amount of the modifier added is: 4.3-5.0%; the insulation temperature is: 1120-1200°C, and the insulation time is: 52-60min.
[0018] A method for preparing a recycled aluminum alloy comprises the following steps: S1, smelting; Melting the raw materials to obtain an aluminum alloy melt; S2, refinement; S3, using the above-mentioned melt iron-rich phase modification method to modify the aluminum alloy melt; S4, casting; The aluminum alloy melt after the modification treatment is poured to obtain a recycled aluminum alloy ingot; the sphericity of the iron-rich phase in the ingot is: 0.70-1.00; S5, processing; Processing of recycled aluminium alloy ingots into plates, profiles, tubes or bars.
[0019] In summary, the iron-rich phase modification treatment method of the melt of the present invention completely melts the original iron-rich phase by heating the melt to a predetermined temperature and keeping it warm, eliminating the nucleation sites in the iron-rich phase, and avoiding the occurrence of iron-rich phase inheritance. After that, a modifier is added to provide a large number of spherical heterogeneous nucleation sites. In the subsequent solidification process, elements such as Fe in the melt grow and eventually form a spheroidized, diffusely distributed second phase structure based on the spherical nucleation sites. The original harmful iron-rich phase morphology is changed into a spherical iron-rich phase, which reduces the stress concentration of the material during the strain process and avoids crack propagation caused by tearing the matrix. The strength and fracture toughness of the recycled aluminum alloy product can be significantly improved. The present invention also provides a method for preparing a recycled aluminum alloy. After the recycled aluminum alloy is modified, it has good mechanical properties and can be used without downgrading. The added value of the resource utilization of waste aluminum is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The metallographic diagram of the inherited nucleation sites of the iron-rich phase of the recycled 7050 aluminum alloy melt at different temperatures of the present invention; Figure 2is a solidification curve diagram of the recycled 7050 aviation aluminum alloy of the present invention; Figure 3 It is the Al-Fe binary alloy phase diagram; Figure 4 is a flow chart of the method for preparing recycled aluminum alloy of the present invention; Figure 1 Middle: (a) and (b) are 650℃ melts; (c) and (d) are 700℃ melts; (e) and (f) are 750℃ regenerated melts; Figure 2 In: L is liquid phase, S is Al2CuMg phase, T is Al2Mg3Zn3 phase or Mg 32 (Al,Cu,Zn) 49 phase, V is the stable AlCuMgZn phase. DETAILED DESCRIPTION
[0021] See also Figure 1 The present invention provides a method for treating a melt iron-rich phase by modification, comprising the following steps: S1, heating the aluminum alloy melt to 700-1200°C and keeping the temperature for 10-60 min; completely melting the iron-rich phase in the melt and eliminating the nucleation sites in the iron-rich phase.
[0022] If the high-melting-point iron-rich phase is not completely dissolved, it will remain in the melt in the form of clusters or solid phase particles. Since there is a natural solid-liquid interface between these residual solid phases and the melt, which is both a structural fluctuation site and an energy fluctuation site, it can significantly reduce the nucleation energy and promote the heterogeneous nucleation and growth of solute atoms; thus, the corresponding second phase continues to grow on the residual solid phase during solidification, forming harmful genetic phases such as coarse needles. These genetic phases will serve as stress concentration points during material deformation to form crack sources, promote crack propagation, tear the matrix, and seriously affect the strength and toughness of the product.
[0023] The present invention increases the temperature of the melt to completely melt the iron-rich phase and eliminate the nucleation sites in the iron-rich phase. In the subsequent solidification process, the appearance of harmful genetic phases can be effectively avoided, laying a foundation for improving the performance of aluminum alloy products.
[0024] The present invention adaptively sets the temperature and holding time of the aluminum alloy melt according to the type and melting point of the iron-rich phase, so that the nucleation sites in all the iron-rich phases can be effectively eliminated.
[0025] See also Figure 1 The present invention uses 7050 aviation recycled aluminum alloy, heats the melt to different temperatures, and keeps the temperature for a predetermined time. After the melt solidifies, samples are taken and the structure morphology is detected. The specific analysis results are as follows: Combination Figure 1In Figures (a) and (b), after melting and holding at 650°C, the second phase structure in the alloy still has inheritance. These iron-rich phase structures (Al7Cu2Fe) are distributed between grains and in grains in a large fishbone-like morphology. This shows that these second phases were not fully dissolved into the melt during the smelting process, but existed in the form of solid phases, clusters, etc. During solidification, the Fe and Cu elements in the melt heterogeneously nucleated and grew on them, and inherited to form a coarser inclusion phase, which would seriously affect the comprehensive properties of the recycled alloy.
[0026] Combination Figure 1 As shown in Figures (c) and (d), after melting and holding at 700°C, the area of the iron-rich phase structure (Al7Cu2Fe) in the melt is significantly reduced.
[0027] Combination Figure 1 In Figures (e) and (f), after melting and holding at 750°C, the iron-rich phase structure (Al7Cu2Fe) in the melt is evenly distributed along the grain boundaries, and its morphology has changed fundamentally. After the melt is heated to 750°C, the iron-rich phase structure in the aluminum alloy is almost completely dissolved, eliminating the sites for heterogeneous nucleation of the second phase. Therefore, during solidification, the iron-rich phase reprecipitates from the melt and distributes along the grain boundaries.
[0028] It can be seen from this that by increasing the temperature of the aluminum alloy melt and keeping it warm for a sufficient period of time, the iron-rich phase in the melt can be completely melted and the nucleation sites in the iron-rich phase can be eliminated; thereby improving the morphology of the iron-rich phase after recrystallization, and ultimately improving the performance of the recycled aluminum alloy.
[0029] Combination Figure 2 and Figure 3 The melting point of the iron-rich phase in the aluminum alloy will fluctuate with the changes in the type and content of the elements in it. When the iron content in the aluminum alloy is low, the melting point of the iron-rich phase is usually low. Figure 2 The Al7Cu2Fe structure in the sample begins to precipitate at 494.5℃ and transforms into Al at 589.5℃. 13 Fe4 completely dissolves into the melt at 635°C, which is close to the melting point of the alloy.
[0030] When the iron content in aluminum alloy is high, the iron-rich phase in the alloy transforms into a phase with a higher melting point. For example, the melting point of the common α-Fe phase in aluminum alloy is about 860℃, and the melting point of the β-Fe phase is about 870℃. The melting points of FeAl3 phase and Fe2Al5 phase are 1160℃ and 1169℃ respectively.
[0031] Those skilled in the art can conduct quantitative and qualitative analysis on the recycled aluminum material in advance to determine the type and properties of the iron-rich phase it contains, and then formulate corresponding insulation temperature and insulation time so that the iron-rich phase can be completely melted into the melt.
[0032] Preferably, the morphology of the iron-rich phase in the aluminum alloy treated by the present invention is needle-shaped, lath-shaped or mesh-shaped; the components of the iron-rich phase structure include Al8Fe2Si, Al5FeSi, Al9Fe2Si2, Al 15 (Fe,Mn)3Si2、Al 15 (Fe,Mn)4Si2、Al 18 Fe2Mg7Si 10 、Al 13 (Cr,Fe) 2-4 、Al2CuFe、Al 13 Fe4, AlFe3, AlFe, Al2Fe, Al5Fe2, Al3Fe and Al6Fe.
[0033] S2, adding 0.1-5.0% by mass of a modifier to the aluminum alloy melt; The modifier and Al in the melt form a large number of spherical intermetallic compounds with high melting points, which are dispersed in the melt and become heterogeneous nucleation sites for the growth of the iron-rich phase. In the subsequent solidification process, elements such as Fe in the melt take the spherical intermetallic compounds as the substrate and continue to grow on the substrate, eventually forming a spheroidized and dispersed second phase structure.
[0034] The original harmful iron-rich phase morphology is changed into a spherical iron-rich phase, which reduces the stress concentration of the material during the strain process and avoids tearing the matrix to cause crack propagation. At the same time, during the solidification process of the melt, since the atomic radius of the elements in the modifier is larger than the atomic radius of aluminum, it can become a heterogeneous nucleation site when it enters the melt, reducing the interfacial tension between the solid-liquid phase, increasing the nucleation speed and nucleation rate, promoting the nucleation of the second phase and inhibiting its growth; finally, the second phase structure is refined, so that the modified spheroidized iron-rich phase plays a role of dispersion strengthening, which can significantly improve the strength and fracture toughness of the recycled aluminum alloy products.
[0035] As an embodiment, the modifier of the present invention may be one or more of rare earth elements, zirconium (Zr), titanium (Ti) or boron (B); Furthermore, the modifier of the present invention can be a single substance form of one or more elements selected from lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), yttrium (Y), scandium (Sc), zirconium (Zr), titanium (Ti), and boron (B).
[0036] As an embodiment, the modifier of the present invention can also be a master alloy synthesized from multiple elements; Optionally, the modifier is a master alloy based on aluminum and two elements, including: Al-Ti-B, Al-Er-B, Al-B-La, Al-Ti-Y, Al-Sc-Pr, Al-La-Ce, Al-Nd-Y, Al-Er-Ti, Al-Er-Y, Al-La-Ti, Al-Ce-Y, Al-Ce-Tb, Al-Sm-Y and Al-Ce-B; Optionally, the modifier is a master alloy based on aluminum and synthesized with three elements, including: Al-Y-Zr-Ti, Al-Ce-Tb-Z, Al-La-Ce-B, Al-Ce-Sc-B, Al-Sm-YB, Al-Er-Y-Sc, Al-Er-Nd-Sc and Al-Zr-Ti-B; Optionally, the modifier is a master alloy synthesized with aluminum as the base and four elements, including: Al-La-Y-Ti-B, Al-Ce-Y-Zr-Ti, Al-Nd-Sc-Zr-B, Al-Ce-Nd-Sc-Ti, Al-Nd-Er-Sc-B, Al-Ho-Er-Sc-B, Al-La-Y-Ti-B, Al-La-Nd-Er-Y and Al-Ce-Er-YB-Ti; The iron-rich phase modification treatment method of the melt of the present invention completely melts the original iron-rich phase by heating the melt to a predetermined temperature and keeping it warm, thereby eliminating the nucleation sites in the iron-rich phase and avoiding the occurrence of iron-rich phase inheritance. A modifier is then added to provide a large number of spherical heterogeneous nucleation sites. In the subsequent solidification process, elements such as Fe in the melt grow and eventually form a spherical, diffusely distributed second phase structure with the spherical nucleation sites as the substrate. The original harmful iron-rich phase morphology is changed into a spherical iron-rich phase, which reduces the stress concentration of the material during the strain process and avoids tearing the matrix to cause crack propagation. The strength and fracture toughness of the recycled aluminum alloy product can be significantly improved.
[0037] See also Figure 4 The present invention also provides a method for preparing a recycled aluminum alloy, comprising the following steps: S1, smelting; Melting the raw materials to obtain an aluminum alloy melt; S2, refinement; S3, using the above-mentioned melt iron-rich phase modification method to modify the aluminum alloy melt; S4, casting; After pouring the aluminum alloy melt, a recycled aluminum alloy ingot is obtained; the sphericity of the iron-rich phase in the ingot is 0.70-1.00.
[0038] Furthermore, the method further comprises a processing step of processing the recycled aluminum alloy ingot into a desired shape; Preferably, the recycled aluminum alloy ingot can be processed into plates, profiles, tubes or bars; After being modified, the recycled aluminum alloy of the present invention has good mechanical properties and can be used without being downgraded, thereby increasing the added value of waste aluminum resource utilization.
[0039] The inventors selected waste aluminum as raw material, selected different holding temperatures, holding times, modifier components and other factors, prepared recycled aluminum alloys, and sampled the ingots to test the sphericity of the iron-rich phase. The specific example results are shown in the table below.
[0040] The modifier is a single substance, and the amount of the modifier added is: 0.1-2.0%; the insulation temperature is: 700-900°C, and the insulation time is: 10-30min; the sphericity of the iron-rich phase is: 0.70-0.81. The specific results of each embodiment are shown in Table 1.
[0041] Table 1: Examples of single-substance modifiers Example No. Insulation temperature ℃ Insulation time min Modifier ingredients Modifying agent addition amount% Sphericity 1 700 10 La 0.1 0.70 2 710 11 Ce 0.2 0.71 3 720 12 Pr 0.3 0.71 4 730 13 Nd 0.4 0.72 5 740 14 Pm 0.5 0.72 6 750 15 Sm 0.6 0.73 7 760 16 Eu 0.7 0.74 8 770 17 G 0.8 0.74 9 780 18 Tb 0.9 0.75 10 790 19 Dy 1.0 0.75 11 800 20 Ho 1.1 0.76 12 810 21 Er 1.2 0.77 13 820 22 Tm 1.3 0.77 14 830 23 Yb 1.4 0.78 15 840 24 Lu 1.5 0.78 16 850 25 Y 1.6 0.79 17 860 26 Sc 1.7 0.8 18 870 27 Zr 1.8 0.8 19 880 28 Ti 1.9 0.81 20 890 29 B 2.0 0.81 Modifiers are master alloys based on aluminum and two elements, including: Al-Ti-B, Al-Er-B, Al-B-La, Al-Ti-Y, Al-Sc-Pr, Al-La-Ce, Al-Nd-Y, Al-Er-Ti, Al-Er-Y, Al-La-Ti, Al-Ce-Y, Al-Ce-Tb, Al-Sm-Y and Al-Ce-B; The amount of the modifier added is: 2.1-3.4%; the holding temperature is: 900-1030°C, the holding time is: 30-43min; the sphericity of the iron-rich phase is: 0.82-0.90. The specific results of each embodiment are shown in Table 2.
[0042] Table 2: Examples of modifiers for three elements Example No. Insulation temperature ℃ Insulation time min Modifier ingredients Modifying agent addition amount% Sphericity 21 900 30 Al-Ti-B 2.1 0.82 22 910 31 Al-Er-B 2.2 0.83 23 920 32 Al-B-La 2.3 0.83 24 930 33 Al-Ti-Y 2.4 0.84 25 940 34 Al-Sc-Pr 2.5 0.84 26 950 35 Al-La-Ce 2.6 0.85 27 960 36 Al-Nd-Y 2.7 0.86 28 970 37 Al-Er-Ti 2.8 0.86 29 980 38 Al-Er-Y 2.9 0.87 30 990 39 Al-La-Ti 3.0 0.87 31 1000 40 Al-Ce-Y 3.1 0.88 32 1010 41 Al-Ce-Tb 3.2 0.89 33 1020 42 Al-Sm-Y 3.3 0.89 34 1030 43 Al-Ce-B 3.4 0.90 The modifier is a master alloy based on aluminum and synthesized with three elements, including: Al-Y-Zr-Ti, Al-Ce-Tb-Z, Al-La-Ce-B, Al-Ce-Sc-B, Al-Sm-YB, Al-Er-Y-Sc, Al-Er-Nd-Sc and Al-Zr-Ti-B; The amount of the modifier added is 3.5-4.2%; the holding temperature is 1040-1110°C, the holding time is 44-51 minutes; the sphericity of the iron-rich phase is 0.82-0.95. The specific results of each embodiment are shown in Table 3.
[0043] Table 3: Examples of modifiers for four elements Example No. Insulation temperature ℃ Insulation time min Modifier ingredients Modifying agent addition amount% Sphericity 35 1040 44 Al-Y-Zr-Ti 3.5 0.90 36 1050 45 Al-Ce-Tb-Z 3.6 0.91 37 1060 46 Al-La-Ce-B 3.7 0.92 38 1070 47 Al-Ce-Sc-B 3.8 0.92 39 1080 48 Al-Sm-YB 3.9 0.93 40 1090 49 Al-Er-Y-Sc 4.0 0.93 41 1100 50 Al-Er-Nd-Sc 4.1 0.94 42 1110 51 Al-Zr-Ti-B 4.2 0.95 The modifier is a master alloy synthesized with aluminum as the base and four elements, including: Al-La-Y-Ti-B, Al-Ce-Y-Zr-Ti, Al-Nd-Sc-Zr-B, Al-Ce-Nd-Sc-Ti, Al-Nd-Er-Sc-B, Al-Ho-Er-Sc-B, Al-La-Y-Ti-B, Al-La-Nd-Er-Y and Al-Ce-Er-YB-Ti; The amount of the modifier added is: 4.3-5.0%; the holding temperature is: 1120-1200°C, the holding time is: 52-60min; the sphericity of the iron-rich phase is: 0.95-1.0. The specific results of each embodiment are shown in Table 3.
[0044] Table 4: Examples of modifiers for five elements Example No. Insulation temperature ℃ Insulation time min Modifier ingredients Modifying agent addition amount% Sphericity 43 1120 52 Al-La-Y-Ti-B 4.3 0.95 44 1130 53 Al-Ce-Y-Zr-Ti 4.4 0.96 45 1140 54 Al-Nd-Sc-Zr-B 4.5 0.96 46 1150 55 Al-Ce-Nd-Sc-Ti 4.6 0.97 47 1160 56 Al-Nd-Er-Sc-B 4.7 0.98 48 1170 57 Al-Ho-Er-Sc-B 4.8 0.98 49 1180 58 Al-La-Y-Ti-B 4.9 0.99 50 1190 59 Al-La-Nd-Er-Y 5.0 1.0 51 1200 60 Al-Ce-Er-YB-Ti 5.0 1.0 The body is heated to a predetermined temperature and kept warm, so that the original iron-rich phase is completely melted, the nucleation sites in the iron-rich phase are eliminated, and the iron-rich phase inheritance is avoided. A modifier is then added to provide a large number of spherical heterogeneous nucleation sites. In the subsequent solidification process, elements such as Fe in the melt grow and eventually form a spheroidized, diffusely distributed second phase structure based on the spherical nucleation sites. The original harmful iron-rich phase morphology is changed into a spherical iron-rich phase, which reduces the stress concentration of the material during the strain process and avoids tearing the matrix to cause crack propagation. The strength and fracture toughness of the recycled aluminum alloy product can be significantly improved. The present invention also provides a method for preparing a recycled aluminum alloy. After the recycled aluminum alloy is subjected to a modification treatment, it has good mechanical properties and can be used without being downgraded. The added value of the resource utilization of waste aluminum is improved.
[0045] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art may make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for treating a melt by modifying an iron-rich phase, characterized in that: The steps include: S1, heating the aluminum alloy melt to 700-1200°C and keeping the temperature for 10-60 min; completely melting the iron-rich phase in the melt and eliminating the nucleation sites in the iron-rich phase; S2, adding 0.1-5.0% by mass of a modifier to the aluminum alloy melt; The modifier and the aluminum element in the melt form a large number of spherical intermetallic compounds with high melting points, which are dispersed in the melt and become heterogeneous nucleation sites for the growth of the iron-rich phase.
2. The method for treating the molten iron-rich phase according to claim 1, characterized in that: The modifier is a single substance form of one or more elements selected from lanthanum La, cerium Ce, praseodymium Pr, neodymium Nd, promethium Pm, samarium Sm, europium Eu, gadolinium Gd, terbium Tb, dysprosium Dy, holmium Ho, erbium Er, thulium Tm, ytterbium Yb, lutetium Lu, yttrium Y, scandium Sc, zirconium Zr, titanium Ti, and boron B.
3. The method for treating the molten iron-rich phase according to claim 2, characterized in that: The amount of the modifier added is: 0.1-2.0%; the insulation temperature is: 700-900°C, and the insulation time is: 10-30min.
4. The method for treating the molten iron-rich phase according to claim 1, characterized in that: The modifier is an intermediate alloy based on aluminum and two elements, including: Al-Ti-B, Al-Er-B, Al-B-La, Al-Ti-Y, Al-Sc-Pr, Al-La-Ce, Al-Nd-Y, Al-Er-Ti, Al-Er-Y, Al-La-Ti, Al-Ce-Y, Al-Ce-Tb, Al-Sm-Y and Al-Ce-B.
5. The method for treating the molten iron-rich phase according to claim 4, characterized in that: The amount of the modifier added is: 2.1-3.4%; the insulation temperature is: 900-1030°C, and the insulation time is: 30-43min.
6. The method for treating the molten iron-rich phase according to claim 1, characterized in that: The modifier is an intermediate alloy synthesized with aluminum as the base and three elements, including: Al-Y-Zr-Ti, Al-Ce-Tb-Z, Al-La-Ce-B, Al-Ce-Sc-B, Al-Sm-YB, Al-Er-Y-Sc, Al-Er-Nd-Sc and Al-Zr-Ti-B.
7. The method for treating the molten iron-rich phase according to claim 6, characterized in that: The amount of the modifier added is: 3.5-4.2%; the insulation temperature is: 1040-1110°C, and the insulation time is: 44-51min.
8. The method for treating the molten iron-rich phase according to claim 1, characterized in that: The modifier is an intermediate alloy synthesized with aluminum as the base and four elements, including: Al-La-Y-Ti-B, Al-Ce-Y-Zr-Ti, Al-Nd-Sc-Zr-B, Al-Ce-Nd-Sc-Ti, Al-Nd-Er-Sc-B, Al-Ho-Er-Sc-B, Al-La-Y-Ti-B, Al-La-Nd-Er-Y and Al-Ce-Er-YB-Ti.
9. The method for treating the molten iron-rich phase according to claim 8, characterized in that: The amount of the modifier added is: 4.3-5.0%; the insulation temperature is: 1120-1200°C, and the insulation time is: 52-60min.
10. A method for preparing a recycled aluminum alloy, characterized in that: The steps include: S1, smelting; Melting the raw materials to obtain an aluminum alloy melt; S2, refinement; S3, performing a modification treatment on the aluminum alloy melt using the melt iron-rich phase modification treatment method as described in any one of claims 1 to 9; S4, casting; The aluminum alloy melt after the modification treatment is poured to obtain a recycled aluminum alloy ingot; the sphericity of the iron-rich phase in the ingot is: 0.70-1.00; S5, processing; Processing of recycled aluminium alloy ingots into plates, profiles, tubes or bars.
Citation Information
Patent Citations
A rare earth metal-doped composite modifier and its preparation method, and a method for preparing Al-Si cast aluminum alloys.
CN113088732B
A modification method for wrought aluminum alloys based on rare earth alloys
CN115433859B
Method for renewable aluminum alloy iron-rich phase metamorphism
CN107385257A
Iron-rich phase modifier as well as preparation method and modification method thereof
CN108998687A
Composite treatment method for recycled wrought aluminum alloy melt
WO2021184827A1
Cited By
Method for regulating and controlling structure and performance of high-Fe-content 6016 secondary aluminum alloy
CN120442971A
Aluminum alloy comprehensive alterant and preparation method thereof
CN121294928A
Aluminum alloy comprehensive modifier and preparation method thereof
CN121294928B
Regulation and control method for morphology of iron-rich phase in secondary aluminum alloy
CN121380645A
Method for refining iron-containing compound of high-Fe-content 3104 aluminum alloy
CN121428324A