NiO nanoparticle modified graphene reinforced aluminum-based composite material and preparation method thereof
Modifying graphene with NiO nanoparticles solves the problem of poor bonding strength between graphene and aluminum-based interfaces, forming a hierarchical interface structure and micro-interface improvement, which significantly improves the mechanical properties and electrical and thermal conductivity of aluminum-based composite materials.
Patent Information
- Application Number
- CN202410808707.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-15
Smart Images

Figure CN118773485A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a graphene-reinforced aluminum-based composite material modified with NiO nanoparticles and a preparation method thereof, belonging to the technical field of metal-based composite materials and preparation methods thereof. Background Art
[0002] Aluminum-based composites are widely used in aerospace, microelectronics, power vehicles and other high-tech fields due to their advantages such as low density, high modulus, corrosion resistance, excellent processing performance and good performance stability. In the traditional sense, there are mainly two types of reinforcements for aluminum-based composites: one is the most widely used discontinuous particle reinforcement phase, such as ZrO2, SiC, Mo, diamond, etc.; the other is the fiber reinforcement phase with relatively harsh preparation conditions, including fabrics, natural fibers, glass fibers, whiskers, etc. These traditional aluminum-based composites, although they have high specific strength and stiffness, usually lead to a mismatch between the strength and plasticity of the composites due to the intrinsic brittleness of the reinforcement phase and its poor interface bonding with the aluminum matrix. And once overloaded during the plastic deformation process, it is easy to cause early cracks, failure or even fracture of the composite material. Therefore, a high-performance nano-reinforcement phase is needed to improve the comprehensive performance of aluminum-based composites.
[0003] Carbon reinforcements represented by graphene are considered to be ideal materials to replace traditional reinforcement phases due to their unique two-dimensional hexagonal honeycomb structure, excellent physical and chemical properties and ultra-high mechanical properties. It has been confirmed that the Young's modulus of a single-layer graphene is about 1TPa, the theoretical tensile strength is as high as 130GPa, and the fracture strain is about 25%. It is expected that a small amount of addition can significantly improve the mechanical properties of composite materials, and the composite material can obtain a plastic deformation capacity similar to that of the aluminum matrix. In addition, due to the ultra-high electrical and thermal conductivity of graphene, adding graphene to the aluminum matrix can improve the electrical and thermal conductivity of aluminum-based composite materials while improving the mechanical properties of the composite material, further expanding the application range of aluminum-based composite materials. However, due to the poor wettability between graphene itself and the aluminum matrix, the low interface bonding strength, and the serious harmful interface reaction with the aluminum matrix under high temperature conditions, the strengthening efficiency of graphene in composite materials has been significantly reduced. Summary of the invention
[0004] Aiming at the problems that the existing interface bonding strength between graphene and aluminum substrate is poor and harmful interface reaction is serious at high temperature, the present invention provides a graphene reinforced aluminum substrate composite material modified with NiO nanoparticles and a preparation method thereof.
[0005] The technical solution of the present invention:
[0006] One of the purposes of the present invention is to provide a method for modifying graphene reinforced aluminum-based composite materials using NiO nanoparticles, the method comprising the following steps:
[0007] (1) GO suspension and Ni(CH3OO)2·4H2O powder were mixed and stirred in a water bath. After the reaction, the product was centrifuged, washed and dried, and then calcined in an inert atmosphere to obtain NiO@rGO reinforced powder;
[0008] (2) The aluminum powder and the NiO@rGO reinforced powder are ball-milled in an inert atmosphere. After the ball-milling, the obtained composite powder is sintered to obtain a NiO@rGO / Al composite material.
[0009] It is further defined that the mass ratio of GO and Ni(CH3OO)2·4H2O in (1) is 1:3.4.
[0010] It is further defined that the stirring reaction process under the water bath condition in (1) is: stirring the reaction at 85° C. for 30 minutes, adding deionized water, and continuing the reaction for 30 minutes.
[0011] It is further defined that the calcination temperature in (1) is 250°C and the calcination time is 1 h.
[0012] It is further defined that the mass ratio of aluminum powder to NiO@rGO reinforcing powder in (2) is 200:1.
[0013] It is further defined that in (2), the ball milling speed is 300 r / min, the intermittent ball milling time is 1 h, and the ball-to-material ratio is 10:1.
[0014] Furthermore, the ball milling process was allowed to pause for 10 minutes after every 5 minutes of operation.
[0015] Further, the sintering conditions in (2) are: pressure of 40 MPa and vacuum of 1×10 -2 Pa, temperature is 600℃, time is 1h.
[0016] A second object of the present invention is to provide an aluminum-based composite material prepared by the above method.
[0017] It is further defined that the yield strength of the aluminum-based material is 92.6±3.3MPa and the ultimate tensile strength is as high as 130.7±1.8MPa.
[0018] Beneficial effects:
[0019] The present invention firstly adopts NiO nanoparticles to modify the surface of graphene oxide, introduces NiO nanoparticles at the graphene / aluminum interface, utilizes the aluminothermic reaction of NiO and aluminum matrix, forms a hierarchical interface structure in the composite material, improves the interface bonding strength between the reinforcement and the aluminum matrix, and then improves the mechanical properties of the composite material. At the same time, the Al2O3 phase and Al3Ni intermetallic compound generated by the aluminothermic reaction of NiO nanoparticles and aluminum matrix can greatly improve the microscopic interface structure of graphene / aluminum, wherein the Al2O3 phase distributed along the grain boundary can be used as a transition layer between graphene and aluminum matrix, forming a unique microscopic interface configuration of graphene / Al2O3 / Al, converting the weak physical bonding of the graphene / aluminum interface into chemical bonding, improving the interface bonding strength, and then improving the load transfer efficiency of the composite material. The Al3Ni intermetallic compound can diffuse from the grain boundary to the crystal by the thermal effect generated by the aluminothermic reaction, and can be used as a second phase nanoparticle to hinder the dislocation movement in the crystal, relieve the stress concentration at the grain boundary, and give full play to the strengthening effect of the reinforcement. The test results show that the yield strength of the prepared NiO@rGO / Al composite material is 92.6±3.3MPa, and the ultimate tensile strength is as high as 130.7±1.8MPa, which are increased by 85.6% and 60% respectively compared with the aluminum matrix. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 TEM image of NiO@rGO reinforced powder prepared in Example 1;
[0021] Figure 2 XRD spectrum of NiO@rGO reinforced powder prepared in Example 1;
[0022] Figure 3 This is the SEM image of the NiO@rGO / Al composite powder prepared in Example 1;
[0023] Figure 4 TEM image of the interface structure of the NiO@rGO / Al composite material prepared in Example 1;
[0024] Figure 5 This is the intracrystalline TEM image of the NiO@rGO / Al composite material prepared in Example 1;
[0025] Figure 6 TEM image of the interface structure of the rGO / Al composite material prepared in Comparative Example 1;
[0026] Figure 7 The graph is a comparison curve of the mechanical properties of the composite materials prepared in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0028] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0029] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0030] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art, and the purity of the solid and liquid reagents used is analytically pure.
[0031] Example 1
[0032] The method for preparing the NiO@rGO / Al composite material in this embodiment is carried out according to the following steps:
[0033] Step 1: Preparation of NiO@rGO reinforced powder
[0034] First, 0.1g GO was added to 50mL isopropanol and ultrasonically dispersed for 30min. Then, the uniformly dispersed suspension and 0.34g Ni(CH3OO)2·4H2O powder were poured into a round-bottom flask equipped with a condensation reflux device, heated to 85°C in a water bath, stirred vigorously for 30min, and then 5mL deionized water was added, and the reaction continued for another 30min. The product was then centrifuged, washed, and dried at 60°C. Finally, the precipitate was calcined at 250°C for 1h in an argon atmosphere in a tubular furnace to obtain NiO@rGO reinforced powder.
[0035] The obtained NiO@rGO enhanced powder was characterized and the results are as follows:
[0036] (1) TEM images of NiO@rGO reinforced powders Figure 1 As shown by Figure 1It can be seen that a large number of uniform NiO nanoparticles are loaded on the surface of the graphene sheets, and the loading of a large number of uniform NiO nanoparticles can act as a layer of interlayer between graphene and graphene sheets during the dispersion of graphene, thereby effectively avoiding the problem of graphene agglomeration caused by a large specific surface area; secondly, aluminothermic reaction and redox reaction can occur during the high-temperature forming process of the composite material to generate intermetallic compounds (Al3Ni, Al2O3), thereby improving the problem of non-wetting between aluminum and carbon, improving the interface bonding strength, and ensuring the reinforcement efficiency of the reinforcement phase; finally, the loading of NiO nanoparticles also effectively avoids direct contact between aluminum and carbon, thereby reducing the chemical reaction between aluminum and carbon during the high-temperature forming process and reducing the generation of the brittle phase Al4C3.
[0037] (2) XRD spectrum of NiO@rGO enhanced powder Figure 2 As shown by Figure 2 It can be seen that the 2θ values of all characteristic peaks of the composite powder after sintering at 250℃ for 1h are consistent with NiO with Bunsenite structure (PDF#04-0835). Among them, the three most obvious characteristic peaks at 36.9°, 42.9°, and 62.6° correspond to the (111), (200), and (220) crystal planes of NiO, respectively. In addition, the graphene characteristic peaks are very weak, which can be attributed to the effective prevention of restacking of graphene sheets by the attachment of NiO nanoparticles.
[0038] Step 2: Preparation of NiO@rGO / Al composite material
[0039] Spherical Al powder and synthesized NiO@rGO reinforcement (0.5wt.%) were milled in an argon atmosphere with a ball-to-material ratio of 10:1 and a ball milling speed of 300r / min for 1h (5min run and 10min pause). The composite powder was then loaded into a graphite mold with a diameter of 50mm and a pressure of 40MPa and a vacuum of 1×10 -2 The NiO@rGO / Al composite material was obtained by vacuum hot pressing and sintering at 600℃ for 1h under the condition of Pa.
[0040] The microscopic morphology of the composite powder obtained after ball milling was characterized, and the SEM images were as follows: Figure 3 As shown by Figure 3 It can be seen that the Al powder undergoes slight plastic deformation after ball milling, and is squeezed from a spherical shape into an irregular block, and no serious cold welding occurs. This can be attributed to the fact that intermittent ball milling reduces the continuous high-energy ball milling time, avoids excessive shear stress on the Al powder during the ball milling process, and inhibits the occurrence of cold welding. In addition, it can be observed in the figure that small transparent NiO@rGO flakes are evenly dispersed on the surface of the Al powder, which indicates that the reinforcement is evenly dispersed, which helps to improve the mechanical properties of the composite material.
[0041] The interface structure of the NiO@rGO / Al composite material was further characterized. The TEM images are shown in Figure 2. Figure 4 As shown by Figure 4 It can be seen that there is an obvious Al2O3 interlayer at the graphene / aluminum interface, with a thickness of about 10nm, which constitutes the microscopic interface structure of graphene / Al2O3 / aluminum. This Al2O3 transition layer can form a strong metallurgical bond at the graphene / Al interface, effectively improving the load transfer efficiency of the composite material and inhibiting the formation of the Al4C3 brittle phase.
[0042] Further, the intracrystalline TEM images of NiO@rGO / Al composite materials were obtained. Figure 5 As shown by Figure 5 It can be observed that the lattice fringes with a spacing of 0.228 nm correspond to the (102) crystal plane of the Al3Ni intermetallic compound. It is not difficult to find that Al3Ni does not gather at the grain boundary but diffuses into the interior of the aluminum grains, which is attributed to the large amount of thermal effect generated by the aluminum-thermal interface reaction, which promotes the long-distance diffusion of Ni atoms. The Al3Ni nanoparticles diffused into the interior of the aluminum grains can act as a second phase, which hinders the movement of grain dislocations during plastic deformation, relieves the stress concentration at the grain boundary, and is beneficial to the improvement of the mechanical properties of the NiO@rGO / Al composite material.
[0043] Comparative Example 1
[0044] The method for preparing the rGO / Al composite material in this comparative example is carried out according to the following steps:
[0045] 0.1g GO was calcined at 250℃ for 1h in a tube furnace under argon atmosphere to obtain rGO reinforced powder. Then, spherical Al powder and synthesized rGO reinforced powder (0.5wt.%) were milled at a ball-to-material ratio of 10:1 and a ball milling speed of 300r / min for 1h (running for 5min and pausing for 10min) under argon atmosphere. The composite powder was then loaded into a graphite mold with a diameter of 50mm and calcined at a pressure of 40MPa and a vacuum of 1×10 -2 The rGO / Al composite material was obtained by vacuum hot pressing and sintering at 600 °C for 1 h under the condition of Pa.
[0046] The TEM image of the interface structure of rGO / Al composite material is shown in Figure 6 As shown by Figure 6 It can be observed that lattice fringes with a spacing of 0.28nm are observed at the graphene / aluminum interface, corresponding to the (012) crystal plane of the Al4C3 phase. This is mainly due to the direct contact between graphene and Al during the hot pressing sintering process, and the interface reaction occurs at high temperature. These Al4C3 phases will significantly reduce the mechanical properties of the composite material.
[0047] The mechanical properties of the composite materials obtained in Example 1 and Comparative Example 1 were characterized. Figure 7 As shown in the figure, curve 1 is the stress-strain curve of the NiO@rGO / Al composite material, and curve 2 is the stress-strain curve of the rGO / Al composite material. It can be seen from the figure that the tensile strength of the NiO@rGO / Al composite material is as high as 130.7±1.8MPa, which is about 51% higher than the tensile strength of the rGO / Al composite material without adding NiO.
[0048] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for using NiO nanoparticles to modify graphene to enhance aluminum-based composite materials, characterized in that: include: (1) GO suspension and Ni(CH3OO)2·4H2O powder were mixed and stirred in a water bath. After the reaction, the product was centrifuged, washed and dried, and then calcined in an inert atmosphere to obtain NiO@rGO reinforced powder; (2) The aluminum powder and the NiO@rGO reinforced powder are ball-milled in an inert atmosphere. After the ball-milling, the obtained composite powder is sintered to obtain a NiO@rGO / Al composite material.
2. The method according to claim 1, characterized in that (1) The mass ratio of GO and Ni(CH3OO)2·4H2O is 1:3.
4.
3. The method according to claim 1, characterized in that: (1) The stirring reaction process under water bath conditions is as follows: after stirring the reaction at 85°C for 30 minutes, deionized water is added and the reaction is continued for 30 minutes.
4. The method according to claim 1, characterized in that: (1) The calcination temperature is 250°C and the time is 1 h.
5. The method according to claim 1, characterized in that (2) The mass ratio of aluminum powder and NiO@rGO reinforced powder is 200:
1.
6. The method according to claim 1, characterized in that (2) The ball milling speed is 300 r / min, the intermittent ball milling time is 1 h, and the ball-to-material ratio is 10:
1.
7. The method according to claim 6, characterized in that During the ball milling process, the milling was paused for 10 min after running for 5 min.
8. The method according to claim 1, characterized in that (2) The sintering conditions are: pressure of 40 MPa and vacuum of 1×10 -2 Pa, temperature is 600℃, time is 1h.
9. An aluminum-based composite material, characterized in that: The method is prepared by any one of claims 1 to 8.
10. The aluminum-based composite material according to claim 1, characterized in that: The yield strength is 92.6±3.3MPa and the ultimate tensile strength is 130.7±1.8MPa.