Aluminum alloy material capable of enhancing connection strength after brazing
By adding specific elements to the aluminum alloy material and forming a large grain structure, the problem of low connection strength after brazing is solved, the fluidity and weld performance of the aluminum alloy material are improved, the service life of the equipment is extended and the light weight requirements are met. quantification and high withstand voltage requirements.
Patent Information
- Application Number
- CN202410811280.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-15
AI Technical Summary
Existing aluminum alloy materials have low connection strength after brazing, resulting in short service life, high maintenance costs and difficulty in aerospace, offshore wind power, battery cold plates, engineering machinery and other fields.
Aluminum alloy materials composed of Si, Mg, Mn, Cu, Fe, Cr, Zn, Ti, V and other elements are used to form a large grain structure through a specific smelting and refining process to improve the fluidity of the liquid solder and the quality of the weld. Air tightness and corrosion resistance.
It significantly enhances the connection strength and air tightness after brazing, extends the working life of the equipment, improves the overall performance of the welding, and meets the requirements of lightweight and high pressure resistance.
Smart Images

Figure CN118773487A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy materials, in particular to an aluminum alloy material capable of enhancing connection strength after brazing. Background Art
[0002] Brazing is a welding method that uses a metal material with a lower melting point than the parent material as a brazing material, uses the liquid brazing material to wet the parent material and fill the gap between the workpiece interface and diffuse it with the parent material. Brazing has small deformation, smooth and beautiful joints, and is suitable for welding precise, complex components composed of different materials, such as heat exchangers, honeycomb structure plates, turbine blades, carbide tools and printed circuit boards. Before brazing, the workpiece must be carefully processed and strictly cleaned to remove oil stains and excessively thick oxide films to ensure the interface assembly gap. During the brazing process, the gap between the parent materials is generally required to be between 0.01 and 0.1 mm. Therefore, in existing aluminum alloy welding operations, due to the poor fluidity of liquid brazing material in narrow gaps, it is difficult to avoid the problem of bubbles at the brazing point. The air tightness, corrosion resistance and connection strength of the connected parts at the weld are low, which leads to a short service life of the parts when used in aerospace, offshore wind power, battery cold plates, engineering machinery, medical equipment and other fields. The above-mentioned fields have the disadvantages of high maintenance cost and high maintenance difficulty. Therefore, there is an urgent need for an aluminum alloy material that can enhance the connection strength after brazing. Summary of the invention
[0003] The technical problem to be solved by the present invention is to overcome the existing defects and provide an aluminum alloy material that can enhance the connection strength after brazing, which can effectively solve the problems in the background technology.
[0004] To achieve the above-mentioned purpose, the present invention provides the following technical solution: an aluminum alloy material capable of enhancing the connection strength after brazing, comprising the following components in weight percentage: Si: 0.2-0.3, Mg≤0.0075, Mn: 1.2-1.3, Cu≤0.05, Fe: 0.1-0.2, Cr≤0.05, Zn≤0.05, Ti≤0.05, V≤0.05, and the rest is Al.
[0005] As a preferred technical solution of the present invention, the aluminum alloy material is composed of the following components in weight percentage: Si: 0.2, Mg: 0.0075, Mn: 1.2, Cu: 0.05, Fe: 0.1, Cr: 0.05, Zn: 0.05, Ti: 0.05, V: 0.05, and the rest is Al.
[0006] As a preferred technical solution of the present invention, the aluminum alloy material is composed of the following components in weight percentage: Si: 0.25, Mg: 0.0075, Mn: 1.25, Cu: 0.05, Fe: 0.15, Cr: 0.05, Zn: 0.05, Ti: 0.05, V: 0.05, and the rest is Al.
[0007] As a preferred technical solution of the present invention, the aluminum alloy material is composed of the following components in weight percentage: Si: 0.3, Mg: 0.0075, Mn: 1.3, Cu: 0.05, Fe: 0.2, Cr: 0.05, Zn: 0.05, Ti: 0.05, V: 0.05, and the rest is Al.
[0008] As a preferred technical solution of the present invention, the preparation method of the aluminum alloy material is:
[0009] Step a, melting temperature is 745°C to 760°C, adding the alloy and stirring for 8 to 10 minutes to allow the alloy elements to be fully dissolved and the alloy to be dissolved uniformly;
[0010] Step b, removing the scum and performing the first refining;
[0011] Step c, refining temperature 740℃~755℃, refining times 4 times, each refining agent is 3kg / ton, refining time is 15 minutes / time. Refining nitrogen purity is 99.999%, nitrogen pressure is 0.1Mpa~0.2Mpa;
[0012] Step d, after refining, the mixture is allowed to stand for 25 to 35 minutes.
[0013] As a preferred technical solution of the present invention, the aluminum alloy material is used to prepare a heat exchanger equipped on a wind turbine.
[0014] As a preferred technical solution of the present invention, the aluminum alloy material is used to prepare a heat exchanger equipped on a spacecraft.
[0015] As a preferred technical solution of the present invention, the aluminum alloy material is used to prepare a heat exchanger equipped on a cold plate of a battery of a new energy vehicle.
[0016] As a preferred technical solution of the present invention, the aluminum alloy material is used to prepare a heat exchanger equipped on engineering machinery.
[0017] Compared with the prior art, the beneficial effects of the present invention are as follows: the aluminum alloy material is characterized by having a large grain structure, which can effectively enhance the fluidity of the liquid brazing material in a narrow gap during brazing, so that the liquid brazing material can completely fill the gap of the base material, and the aluminum alloy material with a large grain structure can also increase its contact area with the solder, effectively enhance the air tightness, corrosion resistance and connection strength of the weld of the formed component, and increase the working life of the aluminum alloy after brazing in the fields of aerospace, offshore wind power, new energy vehicle battery cold plate, engineering machinery, medical equipment, etc.
[0018] The aluminum alloy has the following performance characteristics:
[0019] 1. Good forming and processing characteristics, good corrosion resistance, weldability and rust resistance;
[0020] 2. Good surface flatness, good plasticity and high pressure resistance;
[0021] 3. Impact-resistant, not easy to break, not leaking, and will not break during deep drawing and deep drawing;
[0022] 4. Meet the requirements of lightweight vehicles, make the whole vehicle lighter, and improve the endurance of new energy vehicles. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a photo of the pressure alternation experiment in Experimental Example 1;
[0024] Figure 2 It is the pressure alternation curve diagram in Experimental Example 1;
[0025] Figure 3 This is a comparison diagram of the grain structure of aluminum alloy material before and after welding.
[0026] Figure 4 This is a schematic diagram of the failure position and blasting curve of the blasting test results in Experimental Example 3. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The present invention provides a technical solution: an aluminum alloy material capable of enhancing the connection strength after brazing, which is composed of the following components in weight percentage: Si: 0.2-0.3, Mg≤0.0075, Mn: 1.2-1.3, Cu≤0.05, Fe: 0.1-0.2, Cr≤0.05, Zn≤0.05, Ti≤0.05, V≤0.05, and the rest is Al.
[0029] The preparation method of the aluminum alloy material is:
[0030] Step a, melting temperature is 745°C to 760°C, adding the alloy and stirring for 8 to 10 minutes to allow the alloy elements to be fully dissolved and the alloy to be dissolved uniformly;
[0031] Step b, removing the scum and performing the first refining;
[0032] Step c, refining temperature 740℃~755℃, refining times 4 times, each refining agent is 3kg / ton, refining time is 15 minutes / time. Refining nitrogen purity is 99.999%, nitrogen pressure is 0.1Mpa~0.2Mpa;
[0033] Step d, after refining, the mixture is allowed to stand for 25 to 35 minutes.
[0034] The characteristics of this aluminum alloy material are as follows: Figure 3 As shown, it has a large grain structure, which can effectively enhance the fluidity of liquid solder in narrow gaps during brazing, so that the liquid solder can completely fill the gap between the base material. The aluminum alloy material with a large grain structure can also increase its contact area with the solder, and effectively enhance the air tightness, corrosion resistance and connection strength of the weld of the formed component. The heat exchanger made by brazing using this aluminum alloy has a longer working life than existing alloy materials when it is used in aerospace, offshore wind power, new energy vehicle battery cold plate, engineering machinery, medical equipment and other fields.
[0035] Embodiment 1
[0036] The aluminum alloy material consists of the following components in weight percentage: Si: 0.2, Mg: 0.0075, Mn: 1.2, Cu: 0.05, Fe: 0.1, Cr: 0.05, Zn: 0.05, Ti: 0.05, V: 0.05, and the rest is Al.
[0037] Embodiment 2
[0038] The aluminum alloy material consists of the following components in weight percentage: Si: 0.25, Mg: 0.0075, Mn: 1.25, Cu: 0.05, Fe: 0.15, Cr: 0.05, Zn: 0.05, Ti: 0.05, V: 0.05, and the rest is Al.
[0039] Embodiment 3
[0040] The aluminum alloy material consists of the following components in weight percentage: Si: 0.3, Mg: 0.0075, Mn: 1.3, Cu: 0.05, Fe: 0.2, Cr: 0.05, Zn: 0.05, Ti: 0.05, V: 0.05, and the rest is Al.
[0041] Experimental Example 1
[0042] Test parameters
[0043]
[0044] Test results
[0045]
[0046] in conclusion
[0047] According to the test requirements, a set of CBAT-210 products made of this aluminum alloy material was subjected to pressure alternation. After the product was subjected to 1 million times of alternating pressure, no leakage or deformation occurred, thereby verifying that the product passed the fatigue life test assessment.
[0048] Experimental Example 2
[0049] The temperature alternation test results are as follows:
[0050]
[0051] Experimental Example 3
[0052] The blasting test was carried out on the test piece, and the results are as follows:
[0053]
[0054] from Figure 4 It can be seen that: the 16th channel of XXX-0956 product leaked at 11.19MPa. The design requires the bursting strength to be ≥10.00MPa, and its bursting performance meets the design requirements. Sampling the failure position revealed that the failure position was a normal break in the middle of the oil channel.
[0055] Experimental Example 4
[0056] The mechanical properties test results are as follows:
[0057]
[0058] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An aluminum alloy material capable of enhancing the connection strength after brazing, characterized in that: The following weight percentages of components composition: Si: 0.2~0.3; Mg≤0.0075; Mn: 1.2~1.3; Cu≤0.05; Fe: 0.1~0.2; Cr≤0.05; Zn≤0.05; Ti≤0.05; V≤0.05; The rest is Al.
2. The aluminum alloy material capable of enhancing the connection strength after brazing according to claim 1, characterized in that: The following weight percentages of components composition: Si: 0.2; Mg: 0.0075; Mn: 1.2; Cu: 0.05; Fe: 0.1; Cr:0.05; Zn: 0.05; Ti: 0.05; V:0.05; The rest is Al.
3. The aluminum alloy material capable of enhancing the connection strength after brazing according to claim 1, characterized in that: The following weight percentages of components composition: Si: 0.25; Mg: 0.0075; Mn: 1.25; Cu: 0.05; Fe: 0.15; Cr:0.05; Zn: 0.05; Ti: 0.05; V:0.05; The rest is Al.
4. The aluminum alloy material capable of enhancing the connection strength after brazing according to claim 1, characterized in that: The following weight percentages of components composition: Si: 0.3; Mg: 0.0075; Mn: 1.3; Cu: 0.05; Fe: 0.2; Cr:0.05; Zn: 0.05; Ti: 0.05; V:0.05; The rest is Al.
5. The aluminum alloy material capable of enhancing the connection strength after brazing according to any one of claims 1, 2, 3 or 4, characterized in that: The preparation method of the aluminum alloy is: Step a, melting temperature is 745°C to 760°C, adding the alloy and stirring for 8 to 10 minutes to allow the alloy elements to be fully dissolved and the alloy to be dissolved uniformly; Step b, removing the scum and performing the first refining; Step c, refining temperature 740℃~755℃, refining times 4 times, each refining agent is 3kg / ton, refining time is 15 minutes / time. Refining nitrogen purity is 99.999%, nitrogen pressure is 0.1Mpa~0.2Mpa; Step d, after refining, the mixture is allowed to stand for 25 to 35 minutes.
6. The use of the aluminum alloy material capable of enhancing the connection strength after brazing according to any one of claims 1, 2, 3, 4 or 5, characterized in that: Used to prepare heat exchangers equipped on wind turbines.
7. The use of the aluminum alloy material capable of enhancing the connection strength after brazing according to any one of claims 1, 2, 3, 4 or 5, characterized in that: Used to prepare heat exchangers equipped on spacecraft.
8. The use of the aluminum alloy material capable of enhancing the connection strength after brazing according to any one of claims 1, 2, 3, 4 or 5, characterized in that: Used to prepare heat exchangers installed on cold plates of new energy vehicle batteries.
9. The use of the aluminum alloy material capable of enhancing the connection strength after brazing according to any one of claims 1, 2, 3, 4 or 5, characterized in that: Used to prepare heat exchangers equipped on construction machinery.
Citation Information
Patent Citations
Aluminum alloy fin material for heat exchangers having excellent strength, conductivity, corrosion resistance and brazability, and heat exchanger
CN111630196A
New energy battery aluminum shell material suitable for continuous die stamping and manufacturing method of new energy battery aluminum shell material
CN115386702A
Method for producing almn strips or sheets
CN1505692A
use of aluminum alloy
DE2037804A1