Magnesium alloy template, preparation method of magnesium alloy template and portable house
By setting a transition layer and a protective layer on the magnesium alloy template, and adding Mg-Zr master alloy, the problems of short service life and low safety of prefabricated houses are solved, and higher corrosion resistance and extended service life are achieved. Maintenance costs are reduced.
Patent Information
- Application Number
- CN202410860971.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing prefabricated houses have a short service life, low safety, high maintenance costs, and low recycling rate in complex environments. The thin iron shell of the house is easily rusted and damaged, and the compressive strength and load-bearing capacity are insufficient.
Using a magnesium alloy template, a SiO2-Al2O3-CeO2 composite film layer and a paint layer are provided on the magnesium alloy body to form a transition layer and a protective layer, and Mg-Zr master alloy is added to the magnesium alloy body to improve the overall quality of the magnesium alloy template. Strength and corrosion resistance, used in manufacturing prefab houses.
It extends the service life of the prefab house, improves corrosion resistance, reduces maintenance costs, maintains the lightweight characteristics of the magnesium alloy formwork, and enhances the overall strength and safety of the prefab house.
Smart Images

Figure CN118773496A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of prefabricated house manufacturing, and in particular to a magnesium alloy template, a method for preparing the magnesium alloy template, and a prefabricated house. Background Art
[0002] Traditional prefabricated houses are prefabricated houses that use color steel plates as the frame, sandwich panels as the enclosure material, standard modular series for space combination, and bolted components. They can be assembled and disassembled easily and quickly, achieving universal standardization of temporary buildings, establishing the concept of environmental protection, energy saving, fast and efficient construction, and making temporary houses enter the field of standardized products with serial development, integrated production, supporting supply, inventory and multiple turnover.
[0003] At present, the rock wool sandwich prefabricated houses on the market are mainly composed of channel steel, columns, corrugated boards, floors, rock wool insulation layers, doors and windows. Its advantages are light weight and easy assembly. However, the wall panels of ordinary prefabricated houses are thin iron sheets sandwiched with rock wool layers, which are fixed by welding and channel steel columns. The compressive strength and load-bearing capacity of the shell have certain limitations. If the welding method does not meet the requirements, it is very easy to fall off and produce broken blocks due to shaking during transportation. When used for a long time in complex environments such as construction sites and the wild, the paint peeling of the thin iron sheet of the shell of ordinary prefabricated houses will cause the shell to rust and damage, which will also shorten the service life of ordinary prefabricated houses and increase the cost of long-term maintenance. In summary, the disadvantages of ordinary prefabricated houses are that they are not environmentally friendly, have a short service life, are not safe, have high maintenance costs, and have low recycling rates.
[0004] In view of the above technical defects of ordinary prefabricated houses, it is necessary to propose a new type of prefabricated house to solve the related problems. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the present invention provides a magnesium alloy template, a method for preparing the magnesium alloy template, and a prefabricated house. By providing a transition layer, a protective layer, and a Mg-Zr intermediate alloy, the overall strength and corrosion resistance of the magnesium alloy template can be increased. In the process of making the prefabricated house, the overall service life of the prefabricated house is improved and the overall weight of the magnesium alloy template is maintained. At the same time, the corrosion resistance is improved, thereby avoiding an increase in maintenance costs after the prefabricated house is made.
[0006] The technical solution adopted by the present invention to solve the above technical problems is as follows:
[0007] The present application provides a magnesium alloy template for manufacturing magnesium alloy prefabricated houses. The magnesium alloy template comprises a magnesium alloy body, and the magnesium alloy body comprises the following components:
[0008] Al: 5.5-6.0%, Mn: 0.28-0.35%, Fe: 0.0035-0.0050%, Si: 0.035-0.050%, B: 0.05-0.08%, Ni: 0.0005-0.001%, impurities: 0.001-0.003% and the balance magnesium.
[0009] Optionally, in some embodiments of the present application, the magnesium alloy template includes:
[0010] A transition layer, disposed on the magnesium alloy body;
[0011] The protective layer is arranged on one side of the transition layer relative to the magnesium alloy body.
[0012] Optionally, in some embodiments of the present application, the magnesium alloy body includes a Mg—Zr master alloy, and the content of the Mg—Zr master alloy in the magnesium alloy body is 1.0-1.5 wt %.
[0013] Optionally, in some embodiments of the present application, the transition layer includes SiO 2 -Al 2 O 3 -CeO 2 The composite film layer, the protective layer comprises a paint layer.
[0014] The present application also provides a preparation method for preparing the magnesium alloy template as described above, the preparation method comprising:
[0015] Step 1: Mix and grind aluminum, manganese, iron, silicon, boron, zirconium, nickel and magnesium according to the corresponding proportions to form a mixed raw material;
[0016] Step 2: putting the mixed raw materials into a melting furnace, setting the temperature to 660° C., and filling with nitrogen and sulfur hexafluoride protective gas to melt the mixed raw materials into a magnesium alloy solution;
[0017] Step 3: The magnesium alloy solution is transported into a melting cup of a die-casting machine through an impeller metering pump, and the die-casting machine performs die-casting on the magnesium alloy solution through a vacuum die-casting process to form a magnesium alloy embryo;
[0018] Step 4: The SiO 2 -Al 2 O 3 -CeO 2 The metal layer is die-casted onto the magnesium alloy blank by the die-casting machine to form SiO 2 -Al 2 O 3 -CeO 2 Composite film layer;
[0019] Step 5: In the SiO 2 -Al 2 O 3 -CeO 2 A paint layer is sprayed on the composite film layer to form a magnesium alloy template.
[0020] Optionally, in some embodiments of the present application, during the vacuum die-casting process, the air pressure in the die-casting chamber is 100-150 mbar, and the flow rate of the magnesium alloy solution is controlled to be 0.1-3 m / s.
[0021] Optionally, in some embodiments of the present application, in the vacuum die-casting process, the mold temperature is controlled to be 180-280° C. and the pressure increase ratio is 60-100 MPa.
[0022] An embodiment of the present application also provides a prefabricated house, which is made by the magnesium alloy template as described above, and the prefabricated house includes wall panels, top panels, door panels, bottom panels, connecting frames and hinges, wherein the wall panels, top panels, door panels and bottom panels are all rectangular magnesium alloy templates, the front side is a flat panel, and the surface parallelism is 1 mm.
[0023] The connection frame is an angle steel, which is provided with two connection surfaces. Pin holes are opened on the two connection surfaces, and the processing size of the pin holes corresponds to the size of the wall panel pin holes.
[0024] Compared with the prior art, the beneficial effects of the present invention are:
[0025] 1. In the present application, a transition layer and a protective layer are provided on the magnesium alloy to form a magnesium alloy template, wherein the transition layer is a composite film layer, which can enhance the overall mechanical strength and corrosion resistance of the magnesium alloy template and enhance the overall strength of the magnesium alloy template;
[0026] 2. In the present application, by arranging a Mg-Zr intermediate alloy in the magnesium alloy body, when the magnesium alloy is made into a template, the overall strength of the magnesium alloy template can be further enhanced, and in the process of making it into a portable house, the overall service life of the portable house is increased and the overall weight of the magnesium alloy template is maintained. At the same time, the corrosion resistance is improved, avoiding increased maintenance costs after the portable house is made. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0028] Figure 1A schematic diagram of the overall process of the method for preparing a magnesium alloy template provided in an embodiment of the present application;
[0029] Figure 2 A schematic diagram of the side cross-section structure of a magnesium alloy template provided in an embodiment of the present application;
[0030] Figure 3 A schematic diagram of the overall structure of a prefabricated house provided in an embodiment of the present application;
[0031] Figure 4 for Figure 3 Enlarged structural diagram at A in the middle.
[0032] Description of reference numerals:
[0033] 100, magnesium alloy body; 200, transition layer; 300, protective layer; 400, prefabricated house; 410, wall panel; 420, top panel; 430, door panel; 440, bottom panel; 450, connecting frame; 460, hinge; 470, connecting surface; 480, pin hole. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the protection scope of the present application. It is understood that the drawings are only provided for reference and illustration, and are not used to limit the present application. The connection relationship shown in the drawings is only for the convenience of clear description and does not limit the connection method.
[0035] Specifically, Figure 1 As shown, a magnesium alloy template and a preparation method are provided in an embodiment of the present application, wherein the magnesium alloy template is used to construct a movable house 400. The construction of the movable house 400 requires optimization of the material and physical properties of the magnesium alloy template so as to reduce the construction cost of the movable house 400.
[0036] Among them, in the process of preparing the magnesium alloy template, the preparation is carried out in the following manner in the embodiment of the present application:
[0037] Step 1: Mix and grind aluminum, manganese, iron, silicon, boron, zirconium, nickel and magnesium to form a mixed raw material;
[0038] Step 2: Put the mixed raw materials into the melting furnace, set the temperature to 660℃, and fill with N 2 Nitrogen and sulfur hexafluoride (SF 6 ) protective gas to melt the mixed raw materials into a magnesium alloy solution;
[0039] Step 3: The magnesium alloy solution is transported to the melting cup of the die-casting machine through an impeller metering pump, and the die-casting machine performs a vacuum die-casting process on the magnesium alloy solution to form a magnesium alloy embryo;
[0040] Step 4: SiO 2 -Al 2 O 3 -CeO 2 The metal layer is die-casted onto the magnesium alloy blank by a die-casting machine to form SiO 2 -Al 2 O 3 -CeO 2 Composite film layer;
[0041] Step 5: In SiO 2 -Al 2 O 3 -CeO 2 A paint layer is sprayed on the composite film layer to form a magnesium alloy template.
[0042] Specifically, in step one, it is necessary to control the proportions of aluminum, manganese, iron, silicon, boron, zirconium, nickel and magnesium for mixed crushing. To maintain the physical strength and corrosion resistance of the magnesium alloy, it is necessary to control the mass percentages of each component in the mixed raw material to be: aluminum (Al): 5.5-6.0%, manganese (Mn): 0.28-0.35%, iron (Fe): 0.0035-0.0050%, silicon (Si): 0.035-0.050%, boron (B): 0.05-0.08%, nickel (Ni): 0.0005-0.001%, impurities: 0.001-0.003% and the remaining magnesium metal content.
[0043] In one of the embodiments of the present application, the magnesium alloy is set to be an AM60B magnesium alloy, in which the content of each component is preferably selected as: aluminum (Al): 5.7-5.9%, manganese (Mn): 0.30-0.33%, iron (Fe): 0.0040-0.0047%, silicon (Si): 0.041-0.049%, boron (B): 0.06-0.075%, nickel (Ni): 0.0007-0.0009%.
[0044] Further, preferably, in another embodiment of the present application, the content of each component can be set to: aluminum (Al): 5.85%, manganese (Mn): 0.32%, iron (Fe): 0.0043%, silicon (Si): 0.045%, boron (B): 0.067%, nickel (Ni): 0.0008%.
[0045] The overall physical properties and corrosion resistance of the magnesium alloy template can be improved by the proportion of each component in each embodiment of the present application.
[0046] In the preferred range of the above embodiments, controlling the impurity content to be below 0.0025% can maintain the overall strength and corrosion resistance of the magnesium alloy template.
[0047] Among them, in the above, the impurity components in the magnesium alloy template material are mainly carbon components.
[0048] In step 2, the mixed raw materials of each component ratio need to be put into a melting furnace for melting. In order to melt all the metals, the melting temperature is controlled to be 660°C. In the embodiment of the present application, the temperature can also be set between 700-800°C. Under the temperature environment, the magnesium and other metals in the melting range need to be protected. In the embodiment of the present application, nitrogen (N 2 ) and sulfur hexafluoride (SF 6 ) is used as a protective gas to isolate the oxygen in the air from reacting with the magnesium metal, making it easier to melt the mixed raw materials into a pure magnesium alloy solution.
[0049] In step 2, zirconium metal is added to the magnesium alloy solution during the preparation of the mixed raw materials. The zirconium metal is melted with the magnesium metal at a temperature of 660° C. to form a Mg-Zr intermediate alloy, which accounts for 1.0-1.5wt% by mass in the magnesium alloy solution.
[0050] In the magnesium alloy solution, the Mg—Zr master alloy can improve the mechanical properties and corrosion resistance of the magnesium alloy, and enhance the overall strength and durability of the prefabricated house 400 during the construction process of the prefabricated house 400 .
[0051] After the mixed raw materials are melted into a magnesium alloy solution, the magnesium alloy solution is die-casted to complete step three.
[0052] Among them, in step three, an impeller metering pump and a die-casting machine are provided, wherein the impeller metering pump can transport the magnesium solution to the die-casting machine, and during transportation, the magnesium solution can be transported by an inert gas, specifically:
[0053] During transportation, the magnesium alloy solution is stored in a chamber, and the impeller metering pump is controlled by a program. When transportation is required, the program controls the release of inert gas, and the inert gas pushes the magnesium alloy solution for transportation, so that the magnesium alloy solution is transported to the die-casting machine.
[0054] Among them, in the embodiment of the present application, the transportation of the magnesium alloy solution can be carried out by an inert gas quantitative component, and the specific transportation process is:
[0055] A pump chamber is provided, a cavity is provided in the pump chamber, a first pair of interfaces, a second pair of interfaces and a third pair of interfaces are provided on the pump chamber, the first pair of interfaces connects the cavity and the casting furnace, the second pair of interfaces connects the cavity and the nitrogen control device, the nitrogen control device controls the nitrogen to pressurize the pump chamber, the third pair of interfaces connects the pump chamber and the material cylinder, and the material cylinder is connected to the die-casting machine. When the magnesium alloy solution is transported, the nitrogen can be transported through the nitrogen control device, and the transportation of nitrogen causes the cavity in the pump chamber to generate negative pressure and positive pressure. Under the negative pressure condition, the magnesium alloy solution enters the cavity through the first pair of interfaces. When the magnesium alloy solution fills the cavity, the driving nitrogen generates positive pressure on the pump chamber, and the nitrogen can push the magnesium alloy solution through the third pair of interfaces into the material cylinder, thereby realizing the quantitative transportation of the magnesium alloy solution.
[0056] After the magnesium alloy solution is transported, the magnesium alloy solution is put into a die-casting machine for die-casting. In the embodiment of the present application, the die-casting conditions of the die-casting machine are:
[0057] The air pressure in the die casting cavity is 100-150 mbar, and the flow rate of the magnesium alloy solution is controlled to be 0.1-3 m / s. In the die casting process, the air pressure can be set to 110-130 mbar, and the flow rate of the magnesium alloy is 0.5-2 m / s. Preferably, in the embodiment of the present application, the air rolling is set to 125 mbar, and the flow rate of the magnesium alloy is 1.75 m / s.
[0058] During the die-casting process, the mold temperature is controlled at 180-280°C and the pressure increase ratio is 60-100MPa.
[0059] In the embodiment of the present application, preferably, the mold temperature is controlled to be 220-250°C, and the pressure ratio is 65-80MPa. Further preferably, the mold temperature is controlled to be 230-245°C, and the pressure ratio is 70-75MPa.
[0060] In the above preferred embodiment, the conditions within this range can improve the overall strength of the magnesium alloy during the magnesium alloy die-casting process, so as to facilitate the formation of the magnesium alloy embryo.
[0061] After completing the above steps, the magnesium alloy is subjected to step 4 operation, in which SiO 2 -Al 2 O 3 -CeO 2 The metal layer is die-casted onto the magnesium alloy blank by the die-casting machine to form SiO 2 -Al 2 O 3 -CeO 2 Composite film, such as Figure 2As shown, the composite film layer is a transition layer 200, and the composite film layer is used to enhance the bonding strength and corrosion resistance of the magnesium alloy template.
[0062] In the embodiment of the present application, the SiO 2 -Al 2 O 3 -CeO 2 The thickness of the composite film layer is controlled between 1.5-2mm.
[0063] After the composite film layer is pressed onto the magnesium metal blank, step five is performed, which is to spray paint on the composite film layer to present a paint layer and form a protective layer 300, which prevents the magnesium alloy template from rusting and corroding.
[0064] In the embodiment of the present application, on the one hand, the magnesium alloy template can be surface-treated by the transition layer 200 and the protective layer 300 mentioned above, and on the other hand, the magnesium alloy body 100 can be directly bonded with a stainless steel plate by a connector, thereby eliminating a series of surface treatment processes and enhancing the overall strength of the magnesium alloy.
[0065] The present application also provides a mobile house 400, such as Figure 3 and Figure 4 As shown, the movable house 400 is mainly assembled by the magnesium alloy template prepared as above, and includes a wall panel 410, a top panel 420, a door panel 430, a bottom panel 440, a connecting frame 450 and a hinge 460, wherein the wall panel 410, the top panel 420, the door panel 430 and the bottom panel 440 are all rectangular magnesium alloy templates, the front side is a flat panel, and the surface parallelism is 1mm, the connecting frame 450 is an angle steel, and the angle steel is provided with two connecting surfaces 470, and pin holes 480 are opened on the two connecting surfaces 470, and the processing size of the pin hole 480 corresponds to the size of the pin hole 480 of the wall panel 410, and the hinge 460 is connected with the door panel 430 and the wall panel 410, so as to facilitate the opening and closing of the movable house 400.
[0066] The above embodiments are only used to illustrate the technical method of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical method of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical method of the present invention.
Claims
1. A magnesium alloy template for manufacturing magnesium alloy mobile houses, the magnesium alloy template comprising a magnesium alloy body, characterized in that: The magnesium alloy body comprises the following components: Al: 5.5-6.0%, Mn: 0.28-0.35%, Fe: 0.0035-0.0050%, Si: 0.035-0.050%, B: 0.05-0.08%, Ni: 0.0005-0.001%, impurities: 0.001-0.003% and the balance magnesium.
2. The magnesium alloy template according to claim 1, characterized in that: The magnesium alloy template comprises: A transition layer, disposed on the magnesium alloy body; The protective layer is arranged on one side of the transition layer relative to the magnesium alloy body.
3. The magnesium alloy template according to claim 2, characterized in that: The magnesium alloy body includes a Mg-Zr master alloy, and the content of the Mg-Zr master alloy in the magnesium alloy body is 1.0-1.5wt%.
4. The magnesium alloy template according to claim 2, characterized in that: The transition layer comprises a SiO2-Al2O3-CeO2 composite film layer, and the protective layer comprises a paint layer.
5. A preparation method for preparing the magnesium alloy template according to any one of claims 1 to 4, characterized in that: The preparation method comprises: Step 1: Mix and grind aluminum, manganese, iron, silicon, boron, zirconium, nickel and magnesium according to the corresponding proportions to form a mixed raw material; Step 2: putting the mixed raw materials into a melting furnace, setting the temperature to 660° C., charging nitrogen and sulfur hexafluoride as protective gases, and melting the mixed raw materials into a magnesium alloy solution; Step 3: The magnesium alloy solution is transported into a melting cup of a die-casting machine through an impeller metering pump, and the die-casting machine performs die-casting on the magnesium alloy solution through a vacuum die-casting process to form a magnesium alloy embryo; Step 4: The SiO2-Al2O3-CeO2 metal layer is die-casted onto the magnesium alloy embryo by the die-casting machine to form a SiO2-Al2O3-CeO2 composite film layer; Step five: spraying a paint layer on the SiO2-Al2O3-CeO2 composite film layer to form a magnesium alloy template.
6. The preparation method according to claim 5, characterized in that: During the vacuum die-casting process, the air pressure in the die-casting cavity is 100-150 mbar, and the flow rate of the magnesium alloy solution is controlled to be 0.1-3 m / s.
7. The preparation method according to claim 5, characterized in that: In the vacuum die-casting process, the mold temperature is controlled to be 180-280° C. and the pressure increase ratio is 60-100 MPa.
8. A prefabricated house, made by the magnesium alloy formwork according to any one of claims 1 to 4, characterized in that: The movable board house comprises wall panels, a top panel, a door panel, a bottom panel, a connecting frame and a hinge, wherein the wall panels, the top panel, the door panel and the bottom panel are all rectangular magnesium alloy templates, the front side is a flat panel, and the surface parallelism is 1 mm. The connection frame is an angle steel, which is provided with two connection surfaces. Pin holes are opened on the two connection surfaces, and the processing size of the pin holes corresponds to the size of the wall panel pin holes.