Composite fabric with antibacterial function and preparation method thereof
Through the combination of modified polyester fiber and antibacterial and antioxidant additives, the problem of insufficient antibacterial and antioxidant properties of polyester fabrics is solved, and a composite fabric with excellent antibacterial and antioxidant properties is prepared, which extends the service life of the fabric and improves comfort. feel and breathability.
Patent Information
- Application Number
- CN202410975799.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Ordinary polyester fabrics have poor antibacterial and antioxidant properties, which makes the fabrics easily contaminated with microorganisms during use, resulting in odors, stains or stains, which may cause skin infections and allergies, and have insufficient durability.
Composite fabrics are prepared from modified polyester fibers through a weaving process, and bacteriostatic agents and inorganic modified additives are added. The pendant amino silicone oil and kaempferol in the bacteriostatic agents provide antibacterial properties, and porous vermiculite and quercetin improve breathability and antioxidant properties. performance, forming chemical bond connections to stabilize performance.
The prepared composite fabric has good antibacterial and antioxidant properties, avoids odor and stain problems caused by microbial reproduction, extends the service life of the fabric, and improves comfort and breathability.
Smart Images

Figure CN118773797A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fabrics, and in particular to a composite fabric with antibacterial functionality and a preparation method thereof. Background Art
[0002] In recent years, with the development of social economy and the improvement of people's living standards, the demand for fabrics has increased dramatically and is widely used in clothing, home furnishings, medical care, automobiles and other industries. Among the many fabric materials, polyester has the advantages of good wrinkle resistance, high strength, good elasticity and not easy to deform. It is deeply loved by the market and consumers and occupies an important position in the fabric field.
[0003] Polyester fiber is a synthetic fiber made of polyester chips and plays an important role in the preparation of polyester fabrics. With the development of modern industry, functional fabrics have begun to be favored by consumers, but ordinary polyester fabrics have the disadvantages of poor antibacterial and antioxidant properties, which has limited the application of the fabrics. Polyester fabrics may be contaminated with organic matter such as dandruff, grease, and sweat during use. Under suitable temperature and humidity conditions, these organic matter create favorable conditions for the growth and reproduction of microorganisms. If the antibacterial properties of polyester fabrics are poor, microorganisms will multiply and spread in large numbers, destroying their physical and chemical properties, causing problems such as odor, stains or spots on the fabrics, and may also cause skin infections, allergies and other problems, posing a threat to human health. In addition, antioxidant treatment of polyester fabrics can protect the color and gloss of the fabrics, reduce fading and yellowing caused by oxidation, thereby improving the durability of polyester fabrics and extending their service life.
[0004] The patent with publication number CN109384910B discloses a method for preparing a breathable antibacterial fabric. The invention uses terephthalic acid, bisabolol derivatives and ethylene glycol for esterification copolymerization to obtain modified polyester polyester, which is then made into polyester high-strength yarn. After dyeing and weaving, the breathable antibacterial fabric is obtained. By destroying the regularity and symmetry of the original polyethylene terephthalate chain, the crystallization ability is reduced, and water molecules can easily penetrate into the fiber. In addition, the active antibacterial unit bisabolol is introduced, so that the prepared polyester fabric has good antibacterial and breathable properties. However, the invention has not made improvements in anti-oxidation, and the application field of the fabric is limited to a certain extent. Based on this, it is of great significance for the present invention to develop a polyester fabric with excellent antibacterial and antioxidant properties. Summary of the invention
[0005] The purpose of the present invention is to provide a composite fabric with antibacterial functionality and a preparation method thereof, which solves the following technical problems:
[0006] (1) Solved the problem of poor antibacterial performance of ordinary polyester fabrics;
[0007] (2) Solved the problem of poor antioxidant performance of ordinary polyester fabrics.
[0008] The purpose of the present invention can be achieved through the following technical solutions:
[0009] A method for preparing a composite fabric with antibacterial functionality, wherein the composite fabric is made of modified polyester fiber through a weaving process; the modified polyester fiber comprises the following raw materials in parts by weight: 30 to 50 parts of polyester chips, 7 to 9 parts of antibacterial preparations, 4 to 8 parts of inorganic modified additives, 1 to 3 parts of polyethylene wax, and 1 to 2 parts of polyethylene glycol;
[0010] The preparation method comprises the following steps:
[0011] Step 1: Add polyester chips, antibacterial preparations, inorganic modified additives, polyethylene wax and polyethylene glycol into a high-speed mixer, stir and mix them evenly, and then pour them into a twin-screw extruder for extrusion granulation, wherein the speed of the extruder is 100-150r / min and the temperature is 220-260°C to obtain polyester masterbatch;
[0012] Step 2: melt-spinning the polyester masterbatch obtained in step 1, controlling the spinning temperature to 270-290° C. and the spinning speed to 600-1000 m / min to obtain nascent polyester fibers, stretching and spinning the nascent polyester fibers, and then winding, forming, bundling, stretching and heat setting the fibers to obtain modified polyester fibers;
[0013] Step 3: Spinning the modified polyester fiber into yarn, and weaving the yarn into a composite fabric.
[0014] Furthermore, in step three, the specific process of preparing the composite fabric is: weaving the modified polyester fiber into yarn to obtain modified polyester fiber yarn, using the modified polyester fiber yarn as warp yarn and weft yarn, wherein the yarn count of the warp yarn is 40-45S, the yarn count of the weft yarn is 30-35S, the warp yarn density is 155-162 strands / inch, and the weft yarn density is 72-80 strands / inch, and weaving to obtain the composite fabric.
[0015] Furthermore, the preparation method of the antibacterial preparation comprises the following steps:
[0016] B1: The pendant amino silicone oil, chloroacyl chloride and toluene are stirred and mixed, and stirred at room temperature for 4 to 6 hours under the action of triethylamine. The solvent is removed by rotary evaporation to obtain the modified pendant amino silicone oil;
[0017] B2: Under the action of potassium carbonate aqueous solution, add modified side-amino silicone oil, kaempferol and dimethyl sulfoxide into a nitrogen-protected reactor, stir at 65-75°C for 3-5h, cool and discharge, and the antibacterial preparation can be obtained.
[0018] Furthermore, in step B1, the weight average molecular weight of the pendant amino silicone oil is 1000-2000.
[0019] Furthermore, in step B1, the chloroacyl chloride is any one of 4-chlorobutyryl chloride, 3-chloropropionyl chloride or chloroacetyl chloride.
[0020] Furthermore, in step B2, the mass concentration of the potassium carbonate aqueous solution is 5% to 10%.
[0021] Furthermore, the preparation method of the inorganic modified additive comprises the following steps:
[0022] BB1: treating porous vermiculite with dilute sulfuric acid to obtain pretreated porous vermiculite;
[0023] BB2: Under the action of an esterification catalyst, the pretreated porous vermiculite and 4-bromobutyric acid are placed in an N,N-dimethylformamide solution and stirred at high temperature for 3 to 6 hours to obtain a modified porous vermiculite;
[0024] BB3: Add modified porous vermiculite, quercetin and isopropanol solution into the reactor, perform ultrasound to form a uniform dispersion, add potassium carbonate, stir at a temperature of 60 to 70° C. for 4 to 8 hours, and obtain an inorganic modified additive.
[0025] Furthermore, in step BB2, the esterification catalyst is any one of p-toluenesulfonic acid, aminosulfonic acid, trifluoromethanesulfonic acid or calcium methanesulfonate.
[0026] A composite fabric with antibacterial functionality is prepared by the above-mentioned preparation method.
[0027] Beneficial effects of the present invention:
[0028] (1) The present invention prepares an antibacterial preparation and adds it into a polyester chip base material in the form of an additive. On the one hand, the side amino silicone oil in the antibacterial preparation can give the fabric excellent properties such as softness and smoothness, and can make the fabric have a comfortable fluffy feel, thereby avoiding the discomfort caused by the fabric being too hard or rough. On the other hand, the kaempferol in the antibacterial preparation has good antibacterial properties, so that the prepared composite fabric has good antibacterial properties. In addition, due to the good stability of the antibacterial preparation and the connection method of chemical bonds, the problem of easy migration of small molecule antibacterial agents can be avoided, so that the prepared composite fabric has long-lasting antibacterial properties, avoiding the problems of odor, stains, spots, skin infections, etc. caused by microbial reproduction, and can protect the physical and chemical properties of the fabric and extend its service life.
[0029] (2) The present invention forms an inorganic protective layer in the matrix by adding an inorganic modified additive during the preparation of the composite fabric. The porous vermiculite in the inorganic modified additive has good interface properties with the polyester chip matrix after being organically modified, which helps the inorganic modified additive to be evenly dispersed in the matrix and avoids the phase separation phenomenon between the two phases due to interface problems. The porous vermiculite has a rich pore structure and good air permeability, which can give the composite fabric good air permeability and improve the comfort of the composite fabric. In addition, the quercetin in the inorganic modified additive has good antioxidant properties. Introducing it into the composite fabric can improve the antioxidant properties of the composite fabric, avoid fading and yellowing of the fabric due to oxidation, improve the durability of the composite fabric, and further extend its service life.
[0030] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0032] Figure 1 It is the infrared spectrum test diagram of the modified side-amino silicone oil and the antibacterial preparation of the present invention.
[0033] Figure 2 This is an infrared spectrum test chart of the inorganic modified additive of the present invention. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The preparation methods of the antibacterial preparations and inorganic modified additives in the following examples and comparative examples of the present invention are as follows:
[0036] 1. Preparation of antibacterial preparations
[0037] B1: 5 g of a lateral amino silicone oil with a weight average molecular weight of 1000 was stirred and mixed with toluene, 1.6 g of chloroacetyl chloride was added and mixed, nitrogen was introduced for protection, 0.1 g of triethylamine was added dropwise, and after the addition was completed, the mixture was stirred at room temperature for 5 h, and the solvent was removed by rotary evaporation to obtain a modified lateral amino silicone oil;
[0038] B2: Add 5g of modified side-amino silicone oil and dimethyl sulfoxide to a nitrogen-protected reactor, stir mechanically, then add 1.4g of kaempferol and 0.1g of a 5% potassium carbonate aqueous solution, turn on the heating until the temperature in the reactor reaches 70°C, keep stirring for 4h, cool and discharge the material to obtain an antibacterial preparation.
[0039] The infrared spectroscopy analysis of the modified side-amino silicone oil and antibacterial preparation was performed using the Nicolet 6700 intelligent Fourier transform infrared spectrometer produced by Thermo Corporation of the United States. Figure 1 As shown by Figure 1 It can be seen that in the infrared spectrum of the modified side amino silicone oil, 3435cm -1 The absorption peak of NH in amide appears at 1685 cm -1 The absorption peak of C=O in amide appears at 1365cm -1 The absorption peak of CN appears at 1265cm -1 The absorption peak of CS i appears at 1046 cm -1 The absorption peak of Si-O appears at 721cm -1 The absorption peak of CCl appears at 3430cm -1 The absorption peak of NH in amide appears at 1680 cm -1 The absorption peak of C=O in amide appears at 3059cm -1 The absorption peak of CH in the benzene ring appears at 1401cm -1 The absorption peak of CN appears at 1260cm -1 The absorption peak of CS i appears at 1022 cm -1 The absorption peak of Si-O appears at 1054 cm -1 The absorption peak of ether bond COC appears at 1766 cm -1 The absorption peak of the carbonyl group C=O appears, and the absorption peak of C-Cl disappears.
[0040] It can be inferred that the principle of the above scheme is: the amino silicone oil structure contains active amino groups, and the chloroacetyl chloride structure contains highly active acyl chloride groups. Under the action of triethylamine, an amidation condensation reaction can occur, thereby introducing a halogen group into the structure of the amino silicone oil to obtain a modified amino silicone oil. Then, under the action of an aqueous potassium carbonate solution, the halogen group in the modified amino silicone oil structure undergoes a substitution reaction with the hydroxyl group in the kaempferol structure, thereby grafting kaempferol into the structure of the amino silicone oil to obtain an antibacterial preparation.
[0041] 2. Preparation of Inorganic Modified Additives
[0042] BB1: Add 6 g of porous vermiculite to dilute sulfuric acid, raise the temperature to 40°C, keep stirring at this temperature for 30 min, filter the material, collect the solid sample, wash it, and vacuum dry it to obtain the pretreated porous vermiculite;
[0043] BB2: Under nitrogen protection, 6 g of pretreated porous vermiculite was placed in N, N-dimethylformamide solution, ultrasonically dispersed for 20 min, 2 g of 4-bromobutyric acid and 0.08 g of p-toluenesulfonic acid were added, the system temperature was raised to 105 ° C, stirred for 5 h, the nitrogen was removed, the solid material was filtered out, washed and dried to obtain modified porous vermiculite;
[0044] BB3: Add 6 g of modified porous vermiculite and isopropanol solution into the reactor, perform ultrasound to form a uniform dispersion, pass nitrogen, exhaust the air, add 2.4 g of quercetin and 0.1 g of potassium carbonate into the dispersion, stir for 6 h at 65 °C, separate the solid material by centrifugation, wash with water, and dry to obtain the inorganic modified additive.
[0045] The infrared spectrum analysis of inorganic modified additives was performed using the Nicolet 6700 intelligent Fourier transform infrared spectrometer produced by Thermo Corporation of the United States. Figure 2 As shown by Figure 2 It can be seen that in the infrared spectrum of inorganic modified additives, 3295cm -1 The absorption peak of hydroxyl group OH appears at 1761cm -1 The absorption peak of the ester group C=O appears at 1732 cm -1 The absorption peak of carbonyl group C=O appears at 1020cm -1 The absorption peak of ether bond COC appears at 3051cm -1 The characteristic absorption peak of CH in the benzene ring appears at .
[0046] It can be inferred that the principle of the above scheme is: after the porous vermiculite is treated with sulfuric acid solution, the hydroxyl active groups on its surface are exposed, and under the action of p-toluenesulfonic acid, they can react with the carboxyl groups in the structure of 4-bromobutyric acid, thereby grafting 4-bromobutyric acid to the surface of the porous vermiculite to obtain modified porous vermiculite, and then under the action of potassium carbonate, the halogen groups on the surface of the modified porous vermiculite react with the hydroxyl groups in the structure of quercetin, thereby grafting quercetin to the surface of the porous vermiculite to obtain an inorganic modified additive.
[0047] Example 1
[0048] Preparation of composite fabrics
[0049] Step 1: Add 30g polyester chips, 7g antibacterial preparation, 4g inorganic modified additive, 1g polyethylene wax and 1g polyethylene glycol into a high-speed mixer, stir and mix evenly, and then pour into a twin-screw extruder for extrusion granulation, wherein the speed of the extruder is 100r / min and the temperature is 220°C to obtain polyester masterbatch;
[0050] Step 2: melt-spinning the polyester masterbatch obtained in step 1, controlling the spinning temperature to 270° C. and the spinning speed to 600 m / min to obtain nascent polyester fibers, stretching and spinning the nascent polyester fibers, and then winding, forming, bundling, stretching and heat setting processes to obtain modified polyester fibers;
[0051] Step 3: Weaving the modified polyester fiber into yarn to obtain modified polyester fiber yarn, using the modified polyester fiber yarn as warp yarn and weft yarn, wherein the warp yarn count is 40S, the weft yarn count is 30S, the warp yarn density is 155 yarns / inch, and the weft yarn density is 72 yarns / inch, and weaving to obtain a composite fabric.
[0052] Example 2
[0053] Preparation of composite fabrics
[0054] Step 1: Add 40g polyester chips, 8g antibacterial preparation, 6g inorganic modified additive, 2g polyethylene wax and 1.5g polyethylene glycol into a high-speed mixer, stir and mix evenly, and then pour into a twin-screw extruder for extrusion granulation, wherein the speed of the extruder is 120r / min and the temperature is 240°C to obtain polyester masterbatch;
[0055] Step 2: melt-spinning the polyester masterbatch obtained in step 1, controlling the spinning temperature to 280° C. and the spinning speed to 800 m / min to obtain nascent polyester fibers, stretching and spinning the nascent polyester fibers, and then performing winding, forming, bundling, stretching and heat setting processes to obtain modified polyester fibers;
[0056] Step 3: Weaving the modified polyester fiber into yarn to obtain modified polyester fiber yarn, using the modified polyester fiber yarn as warp yarn and weft yarn, wherein the yarn count of the warp yarn is 42S, the yarn count of the weft yarn is 32S, the warp yarn density is 158 yarns / inch, and the weft yarn density is 76 yarns / inch, and weaving to obtain a composite fabric.
[0057] Example 3
[0058] Preparation of composite fabrics
[0059] Step 1: Add 50g polyester chips, 9g antibacterial preparation, 8g inorganic modified additive, 3g polyethylene wax and 2g polyethylene glycol into a high-speed mixer, stir and mix evenly, and then pour into a twin-screw extruder for extrusion granulation, wherein the speed of the extruder is 150r / min and the temperature is 260°C to obtain polyester masterbatch;
[0060] Step 2: melt-spinning the polyester masterbatch obtained in step 1, controlling the spinning temperature to 290° C. and the spinning speed to 1000 m / min to obtain nascent polyester fibers, stretching and spinning the nascent polyester fibers, and then winding, forming, bundling, stretching and heat setting processes to obtain modified polyester fibers;
[0061] Step 3: Weaving the modified polyester fiber into yarn to obtain modified polyester fiber yarn, using the modified polyester fiber yarn as warp yarn and weft yarn, wherein the warp yarn count is 45S, the weft yarn count is 35S, the warp yarn density is 162 strands / inch, and the weft yarn density is 80 strands / inch, and weaving to obtain a composite fabric.
[0062] Comparative Example 1
[0063] Preparation of composite fabrics
[0064] Step 1: Add 40g polyester chips, 8g antibacterial preparation, 2g polyethylene wax and 1.5g polyethylene glycol into a high-speed mixer, stir and mix evenly, and then pour into a twin-screw extruder for extrusion granulation, wherein the speed of the extruder is 120r / min and the temperature is 240°C to obtain polyester masterbatch;
[0065] Step 2: melt-spinning the polyester masterbatch obtained in step 1, controlling the spinning temperature to 280° C. and the spinning speed to 800 m / min to obtain nascent polyester fibers, stretching and spinning the nascent polyester fibers, and then performing winding, forming, bundling, stretching and heat setting processes to obtain modified polyester fibers;
[0066] Step 3: Weaving the modified polyester fiber into yarn to obtain modified polyester fiber yarn, using the modified polyester fiber yarn as warp yarn and weft yarn, wherein the yarn count of the warp yarn is 42S, the yarn count of the weft yarn is 32S, the warp yarn density is 158 yarns / inch, and the weft yarn density is 76 yarns / inch, and weaving to obtain a composite fabric.
[0067] Comparative Example 2
[0068] Preparation of composite fabrics
[0069] Step 1: Add 40g polyester chips, 6g inorganic modified additives, 2g polyethylene wax and 1.5g polyethylene glycol into a high-speed mixer, stir and mix evenly, and then pour into a twin-screw extruder for extrusion granulation, wherein the speed of the extruder is 120r / min and the temperature is 240°C to obtain polyester masterbatch;
[0070] Step 2: melt-spinning the polyester masterbatch obtained in step 1, controlling the spinning temperature to 280° C. and the spinning speed to 800 m / min to obtain nascent polyester fibers, stretching and spinning the nascent polyester fibers, and then performing winding, forming, bundling, stretching and heat setting processes to obtain modified polyester fibers;
[0071] Step 3: Weaving the modified polyester fiber into yarn to obtain modified polyester fiber yarn, using the modified polyester fiber yarn as warp yarn and weft yarn, wherein the yarn count of the warp yarn is 42S, the yarn count of the weft yarn is 32S, the warp yarn density is 158 yarns / inch, and the weft yarn density is 76 yarns / inch, and weaving to obtain a composite fabric.
[0072] Comparative Example 3
[0073] Preparation of composite fabrics
[0074] Step 1: Add 40g polyester chips, 8g antibacterial preparation, 4g porous vermiculite, 2g quercetin, 2g polyethylene wax and 1.5g polyethylene glycol into a high-speed mixer, stir and mix evenly, and then pour into a twin-screw extruder for extrusion granulation, wherein the speed of the extruder is 120r / min and the temperature is 240°C to obtain polyester masterbatch;
[0075] Step 2: melt-spinning the polyester masterbatch obtained in step 1, controlling the spinning temperature to 280° C. and the spinning speed to 800 m / min to obtain nascent polyester fibers, stretching and spinning the nascent polyester fibers, and then performing winding, forming, bundling, stretching and heat setting processes to obtain modified polyester fibers;
[0076] Step 3: Weaving the modified polyester fiber into yarn to obtain modified polyester fiber yarn, using the modified polyester fiber yarn as warp yarn and weft yarn, wherein the yarn count of the warp yarn is 42S, the yarn count of the weft yarn is 32S, the warp yarn density is 158 yarns / inch, and the weft yarn density is 76 yarns / inch, and weaving to obtain a composite fabric.
[0077] Comparative Example 4
[0078] Preparation of composite fabrics
[0079] Step 1: Add 40g polyester chips, 2g polyethylene wax and 1.5g polyethylene glycol into a high-speed mixer, stir and mix them evenly, and then pour them into a twin-screw extruder for extrusion granulation, wherein the speed of the extruder is 120r / min and the temperature is 240°C to obtain polyester masterbatch;
[0080] Step 2: melt-spinning the polyester masterbatch obtained in step 1, controlling the spinning temperature to 280° C. and the spinning speed to 800 m / min to obtain nascent polyester fibers, stretching and spinning the nascent polyester fibers, and then performing winding, forming, bundling, stretching and heat setting processes to obtain modified polyester fibers;
[0081] Step 3: Weaving the modified polyester fiber into yarn to obtain modified polyester fiber yarn, using the modified polyester fiber yarn as warp yarn and weft yarn, wherein the yarn count of the warp yarn is 42S, the yarn count of the weft yarn is 32S, the warp yarn density is 158 yarns / inch, and the weft yarn density is 76 yarns / inch, and weaving to obtain a composite fabric.
[0082] Performance testing:
[0083] The composite fabrics prepared in Examples 1 to 3 and Comparative Examples 1 to 4 of the present invention were made into samples that met the test specifications. The antibacterial performance of the samples and the samples after washing 50 times were tested according to GB / T 20944.2-2007 "Evaluation of Antibacterial Properties of Textiles Part 2: Absorption Method", the test bacteria were Escherichia coli, the washing method was carried out on a washing fastness tester, and the washing conditions were: washing powder 4g / L, bath ratio (mass ratio of fabric to washing liquid was 1:30), temperature 35°C, and time 10min for one washing; the air permeability of the samples was tested according to GB / T5453-1997 "Determination of Air Permeability of Textile Fabrics"; the radial elongation under constant force was tested according to FZ / T 70006-2022 "Test Method for Tensile Elastic Recovery of Knitted Fabrics", and the specific test results are shown in the following table:
[0084]
[0085] From the test results in the above table, it can be seen that the samples prepared in Examples 1 to 3 all have excellent antibacterial properties, antioxidant properties and air permeability, and after washing 50 times, the antibacterial effect of the samples has not changed significantly, so they have long-lasting antibacterial properties; in the samples prepared in Comparative Example 1, no inorganic modified additives were added, so the samples were at a relatively poor level in terms of antioxidant properties and air permeability, but antibacterial preparations were added thereto, so the antibacterial properties of the samples were better; in the samples prepared in Comparative Example 2, no antibacterial preparations were added, so the antibacterial properties were not as good as those in the examples, but inorganic modified additives were added thereto. Comparative Example 4 prepared the sample, neither antibacterial preparation nor inorganic modified additive was added, so the performance of each sample was the worst.
[0086] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a composite fabric with antibacterial functionality, characterized in that: The composite fabric is made of modified polyester fiber through a weaving process; the modified polyester fiber includes the following raw materials in parts by weight: 30 to 50 parts of polyester chips, 7 to 9 parts of antibacterial preparations, 4 to 8 parts of inorganic modified additives, 1 to 3 parts of polyethylene wax, and 1 to 2 parts of polyethylene glycol; The preparation method comprises the following steps: Step 1: Add polyester chips, antibacterial preparations, inorganic modified additives, polyethylene wax and polyethylene glycol into a high-speed mixer, stir and mix them evenly, and then pour them into a twin-screw extruder for extrusion granulation, wherein the speed of the extruder is 100-150r / min and the temperature is 220-260°C to obtain polyester masterbatch; Step 2: melt-spinning the polyester masterbatch obtained in step 1, controlling the spinning temperature to 270-290° C. and the spinning speed to 600-1000 m / min to obtain nascent polyester fibers, stretching and spinning the nascent polyester fibers, and then winding, forming, bundling, stretching and heat setting the fibers to obtain modified polyester fibers; Step 3: Spinning the modified polyester fiber into yarn, and weaving the yarn into a composite fabric.
2. The method for preparing a composite fabric with antibacterial functionality according to claim 1, characterized in that: In step three, the specific process of preparing the composite fabric is: weaving the modified polyester fiber into yarn to obtain modified polyester fiber yarn, using the modified polyester fiber yarn as warp yarn and weft yarn, wherein the yarn count of the warp yarn is 40-45S, the yarn count of the weft yarn is 30-35S, the warp yarn density is 155-162 strands / inch, and the weft yarn density is 72-80 strands / inch, weaving to obtain the composite fabric.
3. The method for preparing a composite fabric with antibacterial functionality according to claim 1, characterized in that: The preparation method of the antibacterial preparation comprises the following steps: B1: The pendant amino silicone oil, chloroacyl chloride and toluene are stirred and mixed, and stirred at room temperature for 4 to 6 hours under the action of triethylamine. The solvent is removed by rotary evaporation to obtain the modified pendant amino silicone oil; B2: Under the action of potassium carbonate aqueous solution, add modified side-amino silicone oil, kaempferol and dimethyl sulfoxide into a nitrogen-protected reactor, stir at 65-75°C for 3-5h, cool and discharge, and the antibacterial preparation can be obtained.
4. The method for preparing a composite fabric with antibacterial functionality according to claim 3, characterized in that: In step B1, the weight average molecular weight of the pendant amino silicone oil is 1000-2000.
5. The method for preparing a composite fabric with antibacterial functionality according to claim 3, characterized in that: In step B1, the chloroacyl chloride is any one of 4-chlorobutyryl chloride, 3-chloropropionyl chloride or chloroacetyl chloride.
6. The method for preparing a composite fabric with antibacterial functionality according to claim 3, characterized in that: In step B2, the mass concentration of the potassium carbonate aqueous solution is 5% to 10%.
7. The method for preparing a composite fabric with antibacterial functionality according to claim 1, characterized in that: The preparation method of the inorganic modified additive comprises the following steps: BB1: treating porous vermiculite with dilute sulfuric acid to obtain pretreated porous vermiculite; BB2: Under the action of an esterification catalyst, the pretreated porous vermiculite and 4-bromobutyric acid are placed in an N,N-dimethylformamide solution and stirred at high temperature for 3 to 6 hours to obtain a modified porous vermiculite; BB3: Add modified porous vermiculite, quercetin and isopropanol solution into the reactor, perform ultrasound to form a uniform dispersion, add potassium carbonate, stir at a temperature of 60 to 70° C. for 4 to 8 hours, and obtain an inorganic modified additive.
8. The method for preparing a composite fabric with antibacterial functionality according to claim 7, characterized in that: In step BB2, the esterification catalyst is any one of p-toluenesulfonic acid, aminosulfonic acid, trifluoromethanesulfonic acid or calcium methanesulfonate.
9. A composite fabric with antibacterial function, characterized in that: The method is as claimed in claim 1.
Citation Information
Patent Citations
A method for preparing a breathable and antibacterial fabric
CN109384910B
Cited By
Functional plant fiber jacquard fabric and manufacturing process thereof
CN119194706A
Functional plant fiber jacquard fabric and manufacturing process thereof
CN119194706B