Method for quantifying capacity loss caused by loss of active metal elements
By calculating the loss of active metal elements at different stages of the battery, and using ICP measurement methods and formulas to calculate the proportion of capacity loss, the problem of difficulty in quantifying the loss of active metal elements in the battery is solved, and the accuracy and efficiency of battery performance verification are improved.
Patent Information
- Application Number
- CN202410828119.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-15
AI Technical Summary
Existing technology makes it difficult to accurately and quantitatively calculate the proportion of capacity loss caused by the loss of active metal elements during the battery's decay process, which affects battery performance verification and determination of improvement directions.
By calculating the capacity loss caused by the loss of active metal elements in the positive and negative electrodes, the ICP measurement method is used to measure the percentage content of active metal elements at different stages, and the formula is used to calculate the proportion of capacity loss caused by the loss of active metal elements.
It achieves precise quantification of the loss of active metal elements during the battery capacity decay process, helping product developers more accurately locate the direction of improvement and shortening the long-term battery performance verification cycle.
Smart Images

Figure CN118777908A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of secondary batteries, and in particular to a method for quantifying capacity loss caused by loss of active metal elements. Background Art
[0002] At present, power batteries or energy storage batteries are widely used, and the performance of battery products is constantly developing towards the goals of faster charging speed, less cycle attenuation, longer service time, wider operating temperature range, and lower manufacturing cost. Among them, in actual use, battery capacity attenuation performance is a hot topic that is continuously studied.
[0003] For battery electrical performance, capacity attenuation performance is an important indicator reflecting the battery itself, which directly affects the reliability judgment of the battery and the design of the terminal product. Therefore, it is particularly important to accurately decompose and calibrate the battery loss capacity composition. According to existing public literature and technical solutions, the cell capacity loss is mainly composed of three parts: the loss of positive electrode active materials, the loss of negative electrode active materials and the loss of active metal elements. If the proportion of loss capacity caused by the loss of active metal elements during the battery attenuation process can be accurately quantified and calculated, it can help product developers more accurately locate the direction of improvement and shorten the long-term performance verification cycle of the battery.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a method for quantifying the capacity loss caused by the loss of active metal elements, aiming to accurately quantify and calculate the proportion of lost capacity caused by the loss of active metal elements during the battery attenuation process.
[0006] The present invention is achieved in that:
[0007] In a first aspect, the present invention provides a method for quantifying the capacity loss caused by the loss of active metal elements, comprising: calculating the capacity loss C caused by the loss of the positive active metal elements 正金属 , calculate the capacity loss C caused by the loss of negative electrode active metal elements 负金属 , the capacity loss ratio caused by the loss of active metal elements is calculated as follows:
[0008] P 活性金属 =(C 正金属 +C 负金属 ) / C 总 ×100%;
[0009] Where P 活性金属 It indicates the capacity loss ratio caused by the loss of active metal elements, in %;
[0010] C 正金属It indicates the capacity loss caused by the loss of active metal elements in the positive electrode, in Ah;
[0011] C 负金属 It indicates the capacity loss caused by the loss of active metal elements in the negative electrode, in Ah;
[0012] C 总 Indicates the total capacity loss in Ah.
[0013] In an alternative embodiment, C 总 =BOL stage capacity - EOL stage capacity.
[0014] In an optional embodiment, ICP is used to determine the percentage of active metal elements in the positive electrode after removing the active metal elements in the EOL stage and the BOL stage, and ICP is used to determine the percentage of active metal elements in the negative electrode after removing the active metal elements in the EOL stage and the BOL stage, and a fitting formula is used to calculate the capacity loss due to the loss of active metal elements.
[0015] In an optional embodiment, the capacity loss C caused by the loss of the positive electrode active metal element 正金属 The calculation formula is as follows:
[0016] C 正金属 =(A1×ρ1×Δw1 / M)×a×c;
[0017] In the formula, A1 represents the positive electrode area, in cm 2 ;
[0018] ρ1 represents the surface density of the positive electrode sheet dressing, in g / cm 2 ;
[0019] Δw1 represents the difference in percentage of active metal elements in the positive electrode after the active metal elements are removed measured by ICP at the EOL stage and the BOL stage;
[0020] M represents the molar mass of the active metal element, in g / mol;
[0021] a represents the ion valence state of the active metal element undergoing electrochemical reaction;
[0022] c represents the charge carried by 1 mol.
[0023] In an optional embodiment, the capacity loss C caused by the loss of the negative electrode active metal element 负金属 The calculation formula is as follows:
[0024] C 负金属 =(A2×ρ2×Δw2 / M)×a×c;
[0025] Where A2 represents the negative electrode area, in cm 2 ;
[0026] ρ2 represents the surface density of the negative electrode dressing, in g / cm 2 ;
[0027] Δw2 represents the difference in the percentage of active metal elements in the negative electrode after the active metal elements are removed by ICP at the EOL stage and the BOL stage;
[0028] M represents the molar mass of the active metal element, in g / mol;
[0029] a represents the ion valence state of the active metal element undergoing electrochemical reaction;
[0030] c represents the charge carried by 1 mol.
[0031] In an alternative embodiment, c = 1 mol of charge / 1 Ah of charge = 96500 / 3600 = 26.8 Ah.
[0032] In an optional embodiment, when the active metal element is Li, the value of a is 1;
[0033] And / or, when the active metal element is Na, the value of a is 1.
[0034] In an optional embodiment, when the active metal element is K, the value of a is 1;
[0035] And / or, when the active metal element is Al, the value of a is 3.
[0036] In an optional embodiment, when the active metal element is Zn, the value of a is 2.
[0037] In an optional implementation, the BOL stage refers to an initial stage of a battery life cycle, and the EOL stage refers to any stage other than the BOL stage.
[0038] The present invention has the following beneficial effects: the capacity loss C caused by the loss of the positive electrode active metal element is calculated respectively. 正金属 , capacity loss caused by loss of negative electrode active metal elements C 负金属 , test the total capacity loss, and fit the formula to calculate the capacity loss ratio caused by the loss of active metal elements. This method is suitable for situations where there are many EOL cells and good parallelism. It can simply, quickly and accurately quantify the loss capacity ratio caused by the loss of active metal elements during the battery attenuation process, helping product developers to more accurately identify the direction of improvement and shorten the battery long-term performance verification cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0040] Figure 1 This is a diagram of the charging and discharging process of a lithium-ion battery. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0042] When the metal element ion battery is charged, the positive electrode releases the metal element ions, and the negative electrode embeds the metal element ions, while the opposite is true when it is discharged. Based on this, the inventors summarize and unify the calculation methods of the total amount of active metal elements in the BOL stage, the total amount of active metal elements in the EOL stage, the dead metal content of the positive electrode, the dead metal content of the negative electrode, and the active metal loss of the metal element ion battery, which can be calculated by Figure 1 The full charging and discharging process of lithium-ion batteries helps to understand.
[0043] Total amount of active metal elements in BOL stage = BOL full discharge positive electrode + BOL full discharge negative electrode;
[0044] Total amount of active metal elements at EOL stage = EOL full discharge positive electrode + EOL full discharge negative electrode;
[0045] Positive dead metal = EOL fully charged positive electrode - BOL fully charged positive electrode;
[0046] Negative dead metal = EOL full discharge negative electrode - BOL full discharge negative electrode;
[0047] Active metal loss = positive electrode dead metal + negative electrode dead metal = (EOL fully charged positive electrode - BOL fully charged positive electrode) + (EOL fully discharged negative electrode - BOL fully discharged negative electrode).
[0048] from Figure 1 It can be seen that in the BOL stage, after the positive electrode lithium is extracted in the fully charged state, it is embedded in the negative electrode; in the fully discharged state, the active Li of the negative electrode returns to the positive electrode. In the EOL stage, the oxygen and metal of the positive electrode are lost, and the amount of dead Li increases, and dead Li exists on the positive electrode, negative electrode and SEI film.
[0049] Therefore, to accurately quantify the capacity loss caused by the loss of active metal elements, it is necessary to consider the capacity loss caused by the loss of active metal elements in the positive electrode and the capacity loss caused by the loss of active metal elements in the negative electrode respectively, and calculate the sum of the two as the total capacity loss caused by the loss of active metal elements. By calculating the capacity of the battery in the EOL stage and the BOL stage, the total capacity loss of the battery is calculated, and then the proportion of the capacity loss caused by the loss of active metal elements to the total capacity loss is calculated.
[0050] An embodiment of the present invention provides a method for quantifying capacity loss caused by loss of active metal elements, comprising the following steps:
[0051] S1. Calculate the capacity loss C caused by the loss of positive electrode active metal elements 正金属
[0052] ICP was used to determine the percentage of active metal elements in the positive electrode after removing the active metal elements in the EOL and BOL stages, and the capacity loss caused by the loss of active metal elements was calculated using a fitting formula.
[0053] Specifically, ICP is tested using an emission spectrometer, and the test steps are as follows: (1) First, scrape the positive and negative electrode powder and weigh 0.11g of sample into a clean sample jar, add 9.00mL of hydrochloric acid and 3ml of nitric acid for wet digestion. After complete digestion, cool to room temperature, filter with filter paper and adjust the volume to 50mL to ensure that the concentration of the element ion to be tested in the sample solution is within the standard curve. The same method is used to make a sample blank; (2) Test process: After the sample is loaded into the instrument, operate the software to ignite the ICP-OES plasma, establish LabBooks, set the test parameters, measure, and process the data according to the test results after the test conditions are met. The test parameters are shown in Table 1:
[0054] Table 1 Element determination parameters
[0055]
[0056]
[0057] Specifically, the BOL stage refers to the initial stage of the battery life cycle, that is, the fresh battery stage; the EOL stage refers to any stage other than the BOL stage, which can refer to the end of the battery life cycle or other stages where capacity decay occurs.
[0058] Capacity loss caused by loss of positive electrode active metal elements C 正金属 The calculation formula is as follows:
[0059] C 正金属 =Δn1×a×c=(ΔW1 / M)×a×c=(A1×ρ1×Δw1 / M)×a×c;
[0060] In the formula, Δn1 represents the difference in the molar amount of active metal elements in the positive electrode after the active metal elements are removed from the positive electrode plate in the EOL stage and the BOL stage, that is, Δn = the molar amount of active metal elements after the active metal elements are removed from the positive electrode in the EOL stage - the molar amount of active metal elements after the active metal elements are removed from the positive electrode in the BOL stage, in mol.
[0061] a represents the ion valence state of the active metal element undergoing electrochemical reaction, and different active metal elements have different corresponding valence states. Specifically, when the active metal element is Li, the value of a is 1; when the active metal element is Na, the value of a is 1; when the active metal element is K, the value of a is 1; when the active metal element is Al, the value of a is 3; when the active metal element is Zn, the value of a is 2.
[0062] c represents the charge carried by 1 mol, c = charge of 1 mol / charge of 1 Ah = 96500 / 3600 = 26.8 Ah. That is, the value of c is 26.8 Ah.
[0063] ΔW1 represents the difference in mass of the active metal elements in the positive electrode after the active metal elements are removed at the EOL stage and the BOL stage, in g. Specifically, ΔW1 = the mass of the active metal elements in the positive electrode after the active metal elements are removed at the EOL stage - the mass of the active metal elements in the positive electrode after the active metal elements are removed at the BOL stage.
[0064] M represents the molar mass of the active metal element, and its unit is g / mol. If the active metal element is lithium, then M=6.941 g / mol.
[0065] A1 represents the positive electrode area, in cm 2 , that is, the area of the positive electrode sheet coated with the positive electrode active layer.
[0066] ρ1 represents the surface density of the positive electrode sheet dressing, in g / cm 2 , that is, the mass of the positive electrode active layer per unit area on the positive electrode sheet, A1×ρ1 represents the mass of the positive electrode active layer.
[0067] Δw1 represents the difference in the percentage of active metal elements in the positive electrode plate after the active metal elements are removed in the EOL stage and the BOL stage as measured by ICP, that is, the percentage of active metal elements in the positive electrode plate after the active metal elements are removed in the EOL stage as measured by ICP - the percentage of active metal elements in the positive electrode plate after the active metal elements are removed in the BOL stage as measured by ICP.
[0068] S2. Calculate the capacity loss C caused by the loss of negative electrode active metal elements 负金属
[0069] ICP was used to determine the percentage of active metal elements in the negative electrode sheets after removing the active metal elements in the EOL and BOL stages, and the capacity loss caused by the loss of active metal elements was calculated using a fitting formula.
[0070] Specifically, ICP is tested using an emission spectrometer, and the test steps and test parameters refer to the introduction of S1.
[0071] Capacity loss caused by loss of negative electrode active metal elements C 负金属 The calculation formula is as follows:
[0072] C 负金属 =Δn2×a×c=(ΔW2 / M)×a×c=(A2×ρ2×Δw2 / M)×a×c;
[0073] In the formula, Δn2 represents the difference in the molar amount of active metal elements in the negative electrode in the EOL stage and the BOL stage, that is, Δn2 = the molar amount of active metal elements after the active metal elements are removed from the negative electrode in the EOL stage - the molar amount of active metal elements after the active metal elements are removed from the negative electrode in the BOL stage, in mol.
[0074] a represents the ion valence state of the active metal element undergoing electrochemical reaction. Different active metal elements have different corresponding valence states. For specific values, see S1.
[0075] c represents the charge carried by 1 mol, c = charge of 1 mol / charge of 1 Ah = 96500 / 3600 = 26.8 Ah. That is, the value of c is 26.8 Ah.
[0076] ΔW2 represents the mass difference between the active metal elements at the EOL stage and the BOL stage after the active metal elements are removed from the negative electrode, in g. Specifically, ΔW2 = the mass of the active metal elements at the EOL stage after the active metal elements are removed from the negative electrode - the mass of the active metal elements at the BOL stage after the active metal elements are removed from the negative electrode.
[0077] M represents the molar mass of the active metal element, and its unit is g / mol. If the active metal element is lithium, then M=6.941 g / mol.
[0078] A2 represents the negative electrode area, in cm 2 , that is, the area of the negative electrode plate coated with the negative electrode active layer.
[0079] ρ2 represents the surface density of the negative electrode sheet dressing, in g / cm 2 , that is, the mass of the negative electrode active layer per unit area on the negative electrode sheet, A2×ρ2 represents the mass of the negative electrode active layer.
[0080] Δw2 represents the difference between the percentage of active metal elements in the negative electrode plate after the active metal elements are removed by ICP in the EOL stage and the BOL stage; that is, the percentage of active metal elements in the EOL stage after the active metal elements are removed by ICP - the percentage of active metal elements in the BOL stage after the active metal elements are removed by ICP.
[0081] S3. Calculate the capacity loss ratio caused by loss of active metal elements
[0082] The percentage of capacity loss caused by loss of active metal elements is calculated as follows:
[0083] P 活性金属 =(C 正金属 +C 负金属 ) / C 总 ×100%;
[0084] Where P 活性金属 It indicates the capacity loss ratio caused by the loss of active metal elements, in %;
[0085] C 正金属 It indicates the capacity loss caused by the loss of active metal elements in the positive electrode, in Ah;
[0086] C 负金属 It indicates the capacity loss caused by the loss of active metal elements in the negative electrode, in Ah;
[0087] C 总 Indicates the total capacity loss in Ah.
[0088] It should be noted that both the positive and negative electrodes will experience loss of active metal elements, which will lead to capacity loss. C is calculated based on S1 and S2 respectively. 正金属 and C 负金属 .
[0089] Furthermore, C 总 =BOL stage capacity - EOL stage capacity, C 总 It represents the total capacity change of the battery, which can be calculated by testing the battery capacity at the EOL stage and the BOL stage using conventional methods.
[0090] It should be noted that the method provided in the embodiment of the present invention is applicable to different attenuation stages of the entire life cycle of metal element ion batteries. The proportion of loss capacity caused by the loss of active metal elements can be quantitatively calculated through the model formula at different stages, which is applicable to situations where there are many EOL cells and good parallelism. The method provided in the embodiment of the present invention is applicable to different types of metal element ion batteries, such as lithium ion batteries, sodium ion batteries, potassium ion batteries, aluminum ion batteries, zinc ion batteries, etc.; the method provided in the embodiment of the present invention can also be extended to the use of batteries with different system materials of the same metal element ion, such as Li material can be LiFePO4, ternary lithium, LiCoO2; Na material can be sodium ferrous sulfate, sodium ferrous pyrophosphate, sodium nickel iron manganese oxide, etc.
[0091] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0092] Example 1
[0093] This embodiment provides a method for quantifying the capacity loss caused by the loss of active metal elements. C is calculated according to the calculation formula given in the embodiment of the invention. 正金属 and C 负金属 , calculate C based on the capacity test results of the BOL and EOL stages 总 , and further calculate the proportion of capacity loss caused by the loss of active metal elements.
[0094] The battery cell provided in this embodiment is a 314Ah lithium-ion battery product of LFP-graphite iron phosphate metal element system, and the test conditions are: 25±2°C, 0.5C constant current and constant voltage charging to 3.65V (0.05C current cutoff), standing for 30 minutes, 0.5C constant current discharge to 2.5V, and constant capacity test.
[0095] After testing: the capacity of the BOL stage is 325.73Ah, and the capacity of the EOL stage is 268.923Ah. The parameters of the negative electrode and the positive electrode are shown in Table 2:
[0096] Table 2 Parameters of negative electrode sheet and positive electrode sheet of Example 1
[0097]
[0098]
[0099] The Li content of the positive and negative electrodes refers to the lithium content of the positive and negative electrodes after delithiation. Due to the generation of dead lithium, the lithium content in the EOL stage is higher.
[0100] C 正金属 =(A1×ρ1×Δw1 / M)×a×c=(410.59*0.1735*(0.63-0.49) / 6.941)
[0101] *1*26.8=38.5077
[0102] C 负金属 =(A2×ρ2×Δw2 / M)×a×c=(397.65*0.3768*(0.2163-0.2064) / 6.941)
[0103] *1*26.8=5.7274
[0104] From Table 2, we can see that the capacity loss caused by the loss of active Li in the negative electrode of the battery cell after cycling is 38.508Ah, accounting for 67.787% of the total capacity loss; the capacity loss caused by the loss of active Li in the positive electrode is 5.727Ah, accounting for 10.082% of the total capacity loss. The proportion of capacity attenuation caused by active Li loss (P active Li) is 77.869%.
[0105] Example 2
[0106] This embodiment provides a method for quantifying the capacity loss caused by the loss of active metal elements. C is calculated according to the calculation formula given in the embodiment of the invention. 正金属 and C 负金属 , calculate C based on the capacity test results of the BOL and EOL stages 总 , and further calculate the proportion of capacity loss caused by the loss of active metal elements.
[0107] The battery cell provided in this embodiment is a ternary graphite system 150Ah lithium-ion battery whose battery cell is NCM523-graphite. The test conditions are: 25±2°C, 0.5C constant current and constant voltage charging to 4.4V (0.05C current cutoff), standing for 30 minutes, 0.5C constant current discharge to 2.8V, and constant capacity test.
[0108] After testing: the capacity of the BOL stage is 162.47Ah, and the capacity of the EOL stage is 134.897Ah. The parameters of the negative electrode and the positive electrode are shown in Table 3:
[0109] Table 3 Parameters of negative electrode sheet and positive electrode sheet of Example 2
[0110]
[0111] It can be seen from Table 3 that the capacity loss caused by the loss of active Li at the positive electrode of the battery cell after cycling is 19.047Ah, accounting for 69.078% of the total capacity loss; the capacity loss caused by the loss of active Li at the negative electrode is 5.182Ah, accounting for 18.794% of the total capacity loss. The proportion of capacity attenuation caused by active Li loss (P active Li) is 87.872%.
[0112] Example 3
[0113] This embodiment provides a method for quantifying the capacity loss caused by the loss of active metal elements. C is calculated according to the calculation formula given in the embodiment of the invention. 正金属 and C 负金属 , calculate C based on the capacity test results of the BOL and EOL stages 总 , and further calculate the proportion of capacity loss caused by the loss of active metal elements.
[0114] The battery cell provided in this embodiment is a 140Ah sodium ion battery of a sodium iron pyrophosphate hard carbon system. The test conditions are: 25±2°C, 0.5C constant current and constant voltage charging to 3.3V (0.05C current cutoff), standing for 30 minutes, 0.5C constant current discharge to 2V, and constant capacity test.
[0115] After testing: the capacity of the BOL stage is 153.74Ah, and the capacity of the EOL stage is 132.984Ah. The parameters of the negative electrode and the positive electrode are shown in Table 4:
[0116] Table 4 Parameters of negative electrode sheet and positive electrode sheet of Example 3
[0117]
[0118] From Table 4, we can see that the capacity loss caused by the loss of active Na in the positive electrode of the battery cell after cycling is 12.672Ah, accounting for 61.052% of the total capacity loss; the capacity loss caused by the loss of active Na in the negative electrode is 4.556Ah, accounting for 21.95% of the total capacity loss. The proportion of capacity attenuation caused by active Na loss (Pactive Na) is 83.002%.
[0119] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method to quantify capacity loss due to loss of active metal elements, It is characterized in that include: Calculate the capacity loss C caused by the loss of positive electrode active metal elements 正金属 , calculate the capacity loss C caused by the loss of negative electrode active metal elements 负金属 , the capacity loss ratio caused by the loss of active metal elements is calculated as follows: P 活性金属 =(C 正金属 +C 负金属 ) / C 总 ×100%; Where P 活性金属 It indicates the capacity loss ratio caused by the loss of active metal elements, in %; C 正金属 It indicates the capacity loss caused by the loss of active metal elements in the positive electrode, in Ah; C 负金属 It indicates the capacity loss caused by the loss of active metal elements in the negative electrode, in Ah; C 总 Indicates the total capacity loss in Ah.
2. The method according to claim 1, It is characterized in that C 总 =BOL stage capacity - EOL stage capacity.
3. The method according to claim 1, It is characterized in that ICP was used to determine the percentage of active metal elements in the positive electrode after removing the active metal elements in the EOL and BOL stages. ICP was used to determine the percentage of active metal elements in the negative electrode after removing the active metal elements in the EOL and BOL stages, and the capacity loss caused by the loss of active metal elements was calculated using a fitting formula.
4. The method according to claim 3, It is characterized in that Capacity loss caused by loss of positive electrode active metal elements C 正金属 The calculation formula is as follows: C 正金属 =(A 1 ×ρ 1 ×Δw 1 / M)×a×c; In the formula, A 1 Indicates the area of the positive electrode, in cm 2 ; ρ 1 Indicates the surface density of the positive electrode sheet dressing, in g / cm 2 ; Δw 1 It indicates the difference in percentage of active metal elements in the positive electrode after removing active metal elements measured by ICP at the EOL stage and the BOL stage; M represents the molar mass of the active metal element, in g / mol; a represents the ion valence state of the active metal element undergoing electrochemical reaction; c represents the charge carried by 1 mol.
5. The method according to claim 3, It is characterized in that Capacity loss caused by loss of negative electrode active metal elements C 负金属 The calculation formula is as follows: C 负金属 =(A 2 ×ρ 2 ×Δw 2 / M)×a×c; In the formula, A 2 Indicates the area of the negative electrode, in cm 2 ; ρ 2 Indicates the surface density of the negative electrode sheet dressing, in g / cm 2 ; Δw 2 It indicates the difference in the percentage of active metal elements in the negative electrode after the active metal elements are removed by ICP at the EOL stage and the BOL stage; M represents the molar mass of the active metal element, in g / mol; a represents the ion valence state of the active metal element undergoing electrochemical reaction; c represents the charge carried by 1 mol.
6. The method according to claim 4 or 5, It is characterized in that c = charge amount of 1 mol / charge amount of 1 Ah = 96500 / 3600 = 26.8 Ah.
7. The method according to claim 4 or 5, It is characterized in that When the active metal element is Li, the value of a is 1; And / or, when the active metal element is Na, the value of a is 1.
8. The method according to claim 4 or 5, It is characterized in that When the active metal element is K, the value of a is 1; And / or, when the active metal element is Al, the value of a is 3.
9. The method according to claim 4 or 5, It is characterized in that When the active metal element is Zn, the value of a is 2.
10. The method according to claim 4 or 5, It is characterized in that The BOL stage refers to the initial stage of the battery life cycle, and the EOL stage refers to any stage other than the BOL stage.