Anti-adhesion coating for structural materials
By applying an anti-adhesion outer coating composition containing a high Tg polymer on the surface of the structural component, the problem of structural component adhesion is solved, a fast, cheap and low solid waste solution is achieved, and the storage and transportation process is simplified.
Patent Information
- Application Number
- CN202380024093.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-21
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-21
AI Technical Summary
Structural components are prone to sticking during storage and transportation. Existing methods such as extending curing time, using anti-blocking additives or thin lining paper have high cost and solid waste problems. There is a lack of fast, cheap and low solid waste solutions.
An anti-adhesion outer coating composition containing a solvent, a binder and a high Tg polymer is applied on the surface of the structural component by spraying or other methods, and cured under appropriate conditions to form an outer coating that is not prone to adhesion. The composition Aqueous compositions are included to reduce volatile organic compounds and solid waste.
Without increasing costs and solid waste, it effectively prevents adhesion of structural components, simplifies storage and transportation processes, reduces curing time and costs, and avoids the use of anti-adhesion additives and thin lining paper.
Smart Images

Figure BDA0005014581400000131 
Figure BDA0005014581400000141 
Figure BDA0005014581400000142
Abstract
Description
Technical Field
[0001] The present application relates to the field of coatings for structural components. Background Art
[0002] Structural components include a wide variety of solid objects such as beams, laths, sheets, membranes, tubes, and other shaped articles, such as door components, window components, fence and deck components, furniture components, and housings for mechanical equipment. Structural components are made of a variety of structural materials, depending on the intended use; examples of structural materials include wood, metal, plastic, concrete, fiberglass, and glass.
[0003] The outer surface of a structural component is often coated with one or more coating materials to improve appearance, protect it from environmental influences, improve safety in use and / or provide other desired properties. Examples of such coatings include various paints, varnishes, shellacs, sealants and curable powder coatings.
[0004] "Blocking" is a common problem with coated structural components. Many coating compositions dry quickly to the touch, but take longer to fully cure, possibly even days. Other coating compositions are intentionally soft even after being fully cured. Individual structural components can be stacked or bundled after they leave the production line so that their weight presses their surfaces together. Or a sheet or film can be rolled into a roll after it leaves the production line so that the surface of one layer from the roll is pressed on the surface of another layer from the same roll. Time and pressure make the still soft coating adhere to the two surfaces between which it is squeezed, with the result that the coating bonds the two surfaces together, thereby forming a solid block by the structural component or layer intended to be separated. Separating these surfaces can damage the surface or the coating or both.
[0005] For the sake of clarity, it should be noted that "curing" of a coating composition can occur by two separate mechanisms: physical drying and chemical curing. See, e.g., Muller et al., Coatings Formulation, 2nd Edition , Vincentz Network GmbH & Co. (2011) Chapter 1.1.1 (Solidification of Paints). In physical drying, the surface is cured by evaporating the solvent, so that the surface feels dry and adheres to the surface to which it is applied. In chemical curing, chemical reactions between molecules in the coating and molecules on the surface further solidify the cohesion of the coating and its adhesion to the surface. The curing of the coating composition may involve one or both of these mechanisms. For many coatings, physical drying occurs faster than chemical curing, so that the structural components feel dry and are stacked or bundled or rolled before the chemical curing is complete; this situation provides a common condition for adhesion formation.
[0006] Blocking and methods to avoid it are discussed in coating industry references such as: “Blocking Resistance in Coatings: Composition Factors to Consider,” https: / / www.lubrizol.com / Coatings / Blog / 2019 / 11 / Blocking-Resistance; “Fluoroadditives: Antiblock Characteristics in Architectural Paint Systems,” Paint and Coatings Industry Magazine, https: / / www.pcimag.com / articles / 83026-fluoroadditives-antiblock-characteristics-in-architectural-paint-systems and “EBook A Guide to Applying Powder Coatings,” www.ifscoatings.com.
[0007] Sometimes, adhesion can be reduced by performing longer curing cycles on the structural components to more fully cure the coating composition, but the curing time is longer; more capital investment is required for additional facilities and equipment to keep each structural component separate from other components until the coating composition is fully cured. Alternatively, anti-adhesion additives can be added to the coating composition, but anti-adhesion additives increase costs and may interfere with the adhesion of the coating to the surface to which it is applied. Alternatively, thin linings or spacers can be placed between the surfaces of different structural components to keep the surfaces separate until they are fully cured, such as is common in boxes for assembling furniture for customers. However, thin linings and spacers increase costs and generate additional solid waste.
[0008] It is desirable to find a fast, inexpensive and low solid waste method to reduce the adhesion of structural components. Summary of the invention
[0009] One aspect of the present invention is a method for preventing adhesion of a structural component, the method comprising the steps of:
[0010] 1) providing a structural component, the structural component comprising at least one surface ("adhesion-forming surface") coated with a primary coating composition that facilitates adhesion;
[0011] 2) applying an anti-adhesion outer coating composition to the adhesion-forming surface, the anti-adhesion outer coating composition comprising
[0012] a) solvent;
[0013] b) a binder, and
[0014] c) a film-forming high Tg polymer having a glass transition temperature greater than 80°C; and
[0015] 3) curing the anti-adhesion top coating composition under conditions suitable for forming an anti-adhesion top coating that is not prone to adhesion,
[0016] "Readily blocks" with respect to a composition herein means that the composition will adhere to a surface other than the block-forming surface which is pressed against the block-forming surface at a temperature of up to 50°C for at least one hour.
[0017] A second aspect of the present invention is an aqueous composition which can be used as an anti-adhesion topcoat composition and comprises the following solid components dissolved or suspended in an aqueous solvent:
[0018] a) a binder in an amount sufficient to form a stable coating;
[0019] b) 1 to 20 wt% of a film-forming, high Tg polymer having a glass transition temperature of at least 80°C;
[0020] c) 1 to 25 wt % of a hydrophobic additive; and
[0021] d) optionally up to 70% by weight of fillers,
[0022] wherein (1) the solids content of the composition is at least 5% by weight; (2) the weight percentages listed for each of components (a)-(d) are based on the total weight of the aqueous composition including the solvent;
[0023] and (3) the pH of the aqueous composition is between 2 and 6. The terms "solid and solids" in this specification refer to components that are solid or waxy solid at 25° C. when suspended in a solvent. Components (a) to (d) are solids.
[0024] A third aspect of the present invention is a structural member comprising at least one surface coated with:
[0025] a. at least one layer of a primary coating composition; and
[0026] b. at least one layer of an anti-blocking top coating on top of the primary coating composition, the anti-blocking top coating comprising:
[0027] i. a binder in an amount sufficient to form a stable coating;
[0028] ii. 1 to 20 wt% of a film-forming high Tg polymer having a glass transition temperature of at least 80°C;
[0029] iii. 1 wt % to 25 wt % of a hydrophobic additive; and
[0030] iv. Optionally up to 70 wt% filler.
[0031] The method of the present invention allows structural components having soft or uncured coatings on their surfaces to be stacked, bundled or rolled without risk of blocking. It uses a curing step that requires less time and cost than that required to fully cure the residual uncured coating. It avoids the costs and problems associated with anti-blocking additives and slip sheets. DETAILED DESCRIPTION
[0032] The method of the present invention uses an anti-blocking outer coating to prevent the structural components from sticking during storage and transportation.
[0033] Structural components are discussed in the Background. Examples of structural components include beams, plates, studs, dowels, cylinders, tubes, sheets, membranes, and other shaped articles. Examples of shaped articles include door components, window components, fence and deck components, stair components, furniture components, decorative moldings, and housings for mechanical equipment.
[0034] The structural component may optionally include wood, metal, polymer, concrete, fiberglass, or glass. In some embodiments, the structural component includes wood, and in some of those embodiments, the structural component is in the form of a beam, board, sheet, stud, dowel, or component for a door, window, or furniture. In some embodiments, the structural component includes a polymer, metal, or fiberglass, and in some of those embodiments, the structural component is a rolled sheet or film.
[0035] All solid objects, including structural components, inherently have surfaces. In the present invention, at least one surface of the structural component (referred to as "adhesion-forming surface") includes a primary coating composition applied thereto. The primary coating composition is easy to adhere after step (a). "Easy to adhere" means that if the adhesion-forming surface and another surface are pressed together for at least one hour at a temperature of up to 50°C, the primary coating composition will adhere to the surface (except the adhesion-forming surface). In some cases, adhesion can be performed by pressing another surface onto the adhesion-forming surface at a pressure of 1psi, or 2psi, or 4psi at a temperature of 25°C or 50°C for 1 or 2 or 4 or 8 or 24 hours or at least a week.
[0036] Because the primary coating composition is not fully cured, it may be susceptible to blocking. In some embodiments, full curing of the primary coating composition (making it less susceptible to blocking) requires standing at ambient temperature for at least 2 hours, or at least 6 hours, or at least 24 hours, or at least 72 hours, or at least one week.
[0037] Alternatively, the primary coating composition may be susceptible to blocking because it has a low glass transition temperature, making it susceptible to blocking even when fully cured. For example, the primary coating composition may have a glass transition temperature of less than 50°C, or not more than 40°C, or not more than 30°C, or not more than 25°C, or not more than 20°C, or not more than 10°C, or not more than 0°C.
[0038] In some embodiments, the primary coating composition is a paint, varnish, shellac, sealant, or weatherable coating. In some embodiments, the primary coating composition is decorative when fully cured, optionally containing pigments or metal flakes. In some embodiments, the primary coating composition is a clear coat. In some embodiments, the primary coating composition is waterproof or weatherable when fully cured. In some embodiments, the primary coating is abrasion resistant or scratch resistant when fully cured. In some embodiments, the primary coating is acid resistant or resistant to other chemicals when fully cured.
[0039] Primary coating compositions and their components are known and commercially available. In many embodiments, paints comprise solvents, binders and pigments. In many embodiments, varnishes comprise solvents, resins, drying oils and driers. In many embodiments, shellacs comprise resins and solvents, optionally with pigments. In many embodiments, weather-resistant coatings contain hydrophobic polymers dissolved or emulsified in solvents. In some embodiments, the solvent for the primary coating composition is organic, and in some embodiments, the solvent is aqueous. The primary coating composition may also contain polymers, additives and fillers to provide improved weather resistance or other properties. Common additives and their uses are described in J. Bieleman (ed.), Additives for Coatings "Additives for Coatings", Wiley-VCH Verlag GmbH (2000).
[0040] To prevent blocking, an anti-blocking topcoat composition is applied to the blocking-forming surface on top of the partially or fully cured primary coating composition. The anti-blocking topcoat composition comprises a solvent, a binder and a film-forming high Tg polymer having a glass transition temperature (Tg) above 80°C.
[0041] The purpose of the solvent is to dissolve the binder and high Tg polymer or to keep them in a suspension or emulsion so as to facilitate the step of applying them to the adhesion-forming surface. The solvent is substantially removed from the adhesion-forming surface during the curing step. For the sake of clarity, the term "solvent" does not mean that all components of the anti-adhesion outer coating composition are soluble in the solvent. Some or all components of the anti-adhesion outer coating composition can be insoluble and maintained in a suspension or emulsion in a solvent.
[0042] The solvent for coating is well known. In some embodiments, the solvent is an organic solvent, such as acetone, pentane, hexane, toluene, xylene, solvent oil, methyl ethyl ketone; n-butyl acetate, ethylene glycol or lower alcohols such as propanol or butanol. In some embodiments, the solvent is aqueous. The aqueous solvent can be substantially neutral (pH 6 to 8), acidic (pH 2 to 6) or alkaline (pH 8 to 12). In some embodiments, the solvent is an acidic aqueous solvent. In some embodiments, the organic solvent may have the advantages of dissolving more components of the anti-adhesion outer coating composition and / or drying faster, but the aqueous solvent may have the advantages of reducing the emission of volatile organic compounds from the anti-adhesion outer coating composition. The solvent is generally commercially available from a variety of sources.
[0043] The purpose of the binder is to form a film on the adhesion-forming surface, and to keep the solid components of the anti-adhesion outer coating composition on the adhesion-forming surface after the curing step. The binder for coating is well known. The example of conventional binders includes acrylic polymers, alkyd polymers, polyurethane polymers, epoxy polymers, polyester polymers and phenolic resins. The example of other known binders includes some natural resins and starch, styrene-butadiene polymers and silanes. Examples are described in publications such as U.S. Patent 6,660,788B2, European Patent Publication EP 0 819 744 A2, German Patent Publication DE 3,123,598A1 and by the Department of Chemistry, University of York, https: / / www.essentialchemicalindustry.org / materials-and-applications / paints.html (March 18, 2013) published in "Paints《Paints》".
[0044] In certain embodiments, the binding agent comprises an acrylic polymer. An acrylic polymer is a polymer or copolymer containing repeating units derived from an acrylic monomer. Acrylic monomers include acrylic acid, methacrylic acid and their esters. Exemplary esters used in acrylic monomers include alkyl esters, for example, alkyl groups containing 1 to 8 carbon atoms or 1 to 4 carbon atoms, or in some cases methyl groups or ethyl groups. Particularly useful acrylic monomers are acrylic acid, methacrylic acid, butyl acrylate, 2-ethylhexyl acrylate, methyl acrylate, ethyl acrylate, methyl methacrylate and ethyl methacrylate.
[0045] Exemplary acrylic polymers may contain at least 70%, or at least 80%, or at least 90%, or at least 95% of repeating units derived from acrylic acid monomers. Exemplary acrylic polymers may contain up to 100% of repeating units derived from acrylic acid monomers. Some exemplary acrylic polymers are copolymers containing units derived from two or more acrylic acid monomers, such as copolymers of butyl acrylate with methyl methacrylate and / or methacrylic acid. Some exemplary acrylic polymers may also contain repeating units derived from non-acrylic ethylenically unsaturated comonomers, such as ethylene, propylene, butylene, or styrene.
[0046] The selection of acrylic monomers and their proportions depends on the intended use of the acrylic polymer. The binder typically has a glass transition temperature (Tg) of at least -45°C and at most +65°C. Binders that will be subject to large thermal expansion at low temperatures, such as outdoor coatings in cold climates, can be selected to have a low Tg, such as at most -15°C, or -20°C, or -30°C. Binders that will be subject to little thermal expansion, such as indoor coatings, can have a higher Tg, such as at least 0°C or at least 10°C. It is known that increasing the content of certain monomers such as methyl methacrylate will increase the Tg of the resulting polymer, and it is known that increasing the content of other monomers such as butyl acrylate will reduce the Tg of the resulting polymer.
[0047] Binders must form films under the conditions under which they are applied to the intended substrate. "Film-forming" means that a substance can form a film when applied to a solid surface. The ability of polymers and their solutions or emulsions to form films is known and described in publications such as: P.A. Steward et al., "An Overview of Polymer Latex Film Formation and Properties ", 86 Advances in Colloid and Interface Science " at 195-267 (2000) and J. Guerts et al., "New Waterborne Acrylic Binders for Zero VOC Paints ", 5 J. Coating Technol. Res. "Journal of Coating Technology Research " at 57-63 (2008). Typically, the film-forming ability of a polymer increases with lower molecular weight and / or lower Tg, and decreases with higher molecular weight and / or higher Tg. Binders with a Tg above 25°C may require additives to help them form films, while lower Tg polymers are generally more film-forming.
[0048] In some embodiments, the monomer mixture is selected so that the binder is water-soluble. In other embodiments, the binder is insoluble in water, but an emulsifier is used to keep it in suspension. The emulsifier keeps the insoluble elements suspended in an aqueous solvent. Emulsifiers are usually surfactants, such as anionic surfactants and nonionic surfactants. For example, some commonly used emulsifiers are fatty alkyl sulfates (such as sodium lauryl sulfate), alcohol ether sulfates, aryl sulfonates (such as branched sodium dodecylbenzene sulfonate), alkyl diphenyl oxide disulfonates (such as disodium lauryl phenyl ether disulfonate), nonylphenol ether sulfates (such as ammonium nonylphenol ether sulfate), fatty alcohol ethoxylates, nonylphenol ethoxylates or alkyl phosphates (such as ammonium phosphate), polyoxyethylene tridecyl ether. Suitable emulsifiers can be obtained under the following trademarks: DOWSIL TM TERGITOL TM TRITON TM , RHODAFAC TM 、RHODACAL TM 、DISPONIL TM ,LUTENSOL TM and DOWFAX TM .
[0049] Examples of commercially available binders include those sold under the trade names RHOPLEX TM 、PARALOIDTM and MAINCOTE TM Acrylic polymers and polymer emulsions available under the trademark Dow Chemical.
[0050] The purpose of film-forming high Tg polymer is to add solid components to the anti-adhesion outer coating, and these solid components do not soften at the normal temperature that the structural component may be stored or transported. Suitable high Tg polymer is known and commercially available. The example of high Tg polymer includes some acrylic acid, polystyrene, polyurethane, poly (vinyl alcohol), vinyl acetate ethylene, vinyl acrylic acid, styrene acrylic acid and styrene butadiene polymer. In some embodiments, high Tg polymer has at least 85 ℃ or at least 90 ℃ or at least 95 ℃ or at least 100 ℃ glass transition temperature (Tg). High Tg polymer does not have maximum Tg, but is usually not required to be higher than 200 ℃ or 150 ℃ Tg.
[0051] High Tg polymers must be film-forming. Typically, the film-forming ability of a polymer increases with lower molecular weight and / or lower Tg, and decreases with higher molecular weight and / or higher Tg. In some embodiments, additives may be added to the high Tg polymer to improve its film-forming ability. In some embodiments, the molecular weight of the high Tg polymer may be kept relatively low to improve its ability to form a film.
[0052] In some embodiments, the high Tg film-forming polymer is water-soluble or water-swellable under selected conditions. Without wishing to be bound, it is hypothesized that the interaction of the water-soluble or water-swellable polymer with water may impart increased flexibility to the higher molecular weight and higher Tg polymer, which increases its film-forming ability. Certain acrylic polymers may be suspended in an emulsion under acidic conditions, but are water-soluble or water-swellable under neutral or alkaline conditions. Aqueous emulsions of such water-soluble or water-swellable film-forming high Tg polymers are commercially available, for example, as ACRYSOL TM The ASE trademark is commercially available from The Dow Chemical Company.
[0053] In some embodiments, the anti-adhesion outer coating composition also includes one or more hydrophobic additives. One purpose of the hydrophobic additive can be to improve the water repellency of the anti-adhesion outer coating, which can minimize the risk of softening the anti-adhesion outer coating as it is continuously exposed to moisture or high humidity. Hydrophobic additives for coatings are known and commercially available. Hydrophobic additives include various waxes (such as paraffin waxes and high melting point waxes); organosilanes, siloxanes and silicones (such as octyl triethoxysilane and polydimethylsiloxane) and hydrophobic polymers (such as polyethylene, polypropylene and polytetrafluoroethylene). In some embodiments, the hydrophobic additive has a melting temperature of at least 60°C, or at least 70°C, or at least 80°C, or at least 85°C, or at least 90°C. The maximum melting temperature of the hydrophobic additive is not required, but a melting point higher than 200°C or 150°C is generally not required. In an aqueous anti-adhesion outer coating composition, an emulsifier as previously described can be used to suspend the hydrophobic additive in the composition. The production of emulsified hydrophobic additives is described in publications such as U.S. Pat. No. 3,096,232 and U.S. Pat. No. 6,033,736. Examples of suitable hydrophobic additives are commercially available under the following trademarks: DOWSIL TM (Dow Chemical Company), Michem Dispersion (Michelman), Lubronil and Wükonil (Münzing), and Aquacer (BYK).
[0054] In some embodiments, the anti-adhesion outer coating composition also includes one or more fillers. Filler is a solid particle added to the coating to improve properties and / or reduce costs. In the composition of the present invention, it is assumed but not intended to be limited that filler can contribute to producing uneven surface texture in the anti-adhesion outer coating, which contributes to the anti-adhesion of the outer coating. Suitable fillers for coating are known and commercially available. The example of suitable filler includes clay (such as kaolin, diatomaceous earth, glass powder and microballoon), aluminum hydroxide and various powdered minerals (such as calcium carbonate, dolomite, feldspar, mica, quartz, silicon dioxide and silicate), talcum and metal carbonate. Other examples of suitable fillers include common mineral pigments, such as titanium dioxide and carbon black. Fillers and their production and use are described in publications such as: Gysau, Fillers for Paints (3rd Edition), Vincentz Network GmbH & Co. (2017); and "Functional Silicate Fillers: Basic Principles", Painting & Coatings Industry (August 1, 2002) (https: / / www.pcimag.com / articles / 84909-functional-silicate-fillers-basic-principles).
[0055] In some embodiments, the filler is a high surface area material. The surface area is typically measured based on the oil absorption value, as described in ASTM D281 (Standard Test Method for Oil Absorption of Pigments by Spatula Rub-Out). In some embodiments, the filler used in the present invention may have an oil absorption value of at least 25 g / 100 g, or at least 30 g / 100 g, or at least 40 g / 100 g, or at least 50 g / 100 g. There is no maximum surface area, but an oil absorption value above 250 g / 100 g may be unnecessary.
[0056] Some common fillers are insoluble and can be suspended in the anti-block coating composition using emulsifiers.
[0057] Examples of suitable fillers are commercially available under the following trademarks: ASP (BASF), Minex and Imsil (Covia), Zoco (American Zinc Recycling), Opacilite and DiaFil and Mica MU (Imerys), Lo-Vel (PPG), Hakuenka and Omyawhite (Omya).
[0058] As previously mentioned, binding agent, high Tg polymer, hydrophobic additive and filler are solids in the anti-adhesion outer coating composition.In some embodiments, advantageously, the solids in the anti-adhesion outer coating composition are maximized to reduce drying time and minimize the volatile organic solvents released from the composition in the drying process.In some embodiments, based on the gross weight of the composition, the solids content of the anti-adhesion outer coating composition is at least 5 % by weight or at least 10 % by weight or at least 15 % by weight or at least 20 % by weight or at least 24 % by weight.There is no maximum solids content, as long as the anti-adhesion outer coating composition can be applied smoothly and easily.In some embodiments, based on the gross weight of the composition, the solids content of the aqueous composition is at most 70 % by weight or at most 50 % by weight or at most 40 % by weight or at most 33 % by weight.
[0059] The amount of binding agent should be enough to form a stable coating, which means that the solid components of the composition are firmly adhered to the film-forming surface. In some embodiments of the anti-adhesion outer coating composition, the binding agent accounts for at least 0.25 weight % or at least 0.5 weight % or at least 1 weight % or at least 1.2 weight % of the composition (including solvent). In some embodiments of the anti-adhesion outer coating composition, the binding agent accounts for at most 25 weight % or at most 20 weight % or at most 10 weight % or at most 5 weight % or at most 3 weight % of the composition (including solvent). In some embodiments of the anti-adhesion outer coating composition, the binding agent accounts for at least 1 weight % or at least 2 weight % or at least 3 weight % or at least 5 weight % of solid (excluding solvent). In some embodiments of the anti-adhesion outer coating composition, the binding agent accounts for at most 50 weight % or at most 20 weight % or at most 10 weight % of solid (excluding solvent).
[0060] In some embodiments of the anti-adhesion outer coating composition, the film-forming high Tg polymer accounts for at least 1% by weight of the composition (including solvent), or at least 2% by weight, or at least 3% by weight, or at least 5% by weight. In some embodiments of the anti-adhesion outer coating composition, the film-forming high Tg polymer accounts for at most 20% by weight of the composition (including solvent), or at most 15% by weight, or at most 10% by weight. In some embodiments of the anti-adhesion outer coating composition, the film-forming high Tg polymer accounts for at least 2% by weight of the solid content (excluding solvent), or at least 4% by weight, or at least 6% by weight, or at least 10% by weight. In some embodiments of the anti-adhesion outer coating composition, the high Tg polymer accounts for at most 50% by weight of the solid content (excluding solvent), or at most 40% by weight, or at most 30% by weight.
[0061] In some embodiments of the anti-adhesion outer coating composition, the hydrophobic additive accounts for at least 1% by weight, or at least 2% by weight, or at least 3% by weight of the composition (including the solvent). In some embodiments of the anti-adhesion outer coating composition, the hydrophobic additive accounts for at most 20% by weight, or at most 15% by weight, or at most 10% by weight of the composition (including the solvent). In some embodiments of the anti-adhesion outer coating composition, the hydrophobic additive accounts for at least 2% by weight, or at least 5% by weight, or at least 10% by weight of the solid content (excluding the solvent). In some embodiments of the anti-adhesion outer coating composition, the hydrophobic additive accounts for at most 40% by weight, or at most 30% by weight, or at most 20% by weight of the solid content (excluding the solvent).
[0062] In some embodiments of the anti-adhesion outer coating composition, filler accounts for at least 5% by weight, or at least 8% by weight, or at least 10% by weight, or at least 12% by weight of the composition (including solvent). In some embodiments of the anti-adhesion outer coating composition, filler accounts for at most 50% by weight, or at most 30% by weight, or at most 20% by weight of the composition (including solvent). In some embodiments of the anti-adhesion outer coating composition, filler accounts for at least 5% by weight, or at least 10% by weight, or at least 20% by weight, or at least 30% by weight, or at least 40% by weight of the solid content (excluding solvent). In some embodiments of the anti-adhesion outer coating composition, filler accounts for at most 70% by weight or at most 60% by weight of the solid content (excluding solvent).
[0063] Optionally, the anti-adhesion outer coating composition can also contain other additives, such as thickeners, defoamers, surfactants, stabilizers, wetting agents, leveling agents and coalescing agents, antioxidants and biocides. Common additives and their use are described in J.Bieleman (ed.), Additives for Coatings "Additives for Coatings", Wiley-VCH Verlag GmbH (2000). In some embodiments, other additives account for no more than 5% by weight of aqueous compositions (including solvents), or no more than 3% by weight, or no more than 2% by weight, or no more than 1% by weight. In some embodiments, other additives account for no more than 10% by weight of solids in aqueous compositions, or no more than 5% by weight, or no more than 2% by weight.
[0064] In the method of the present invention, it is advantageous to select the components of the anti-adhesion outer coating composition so that the anti-adhesion outer coating composition is cured to the extent that it is not easy to quickly adhere under the conditions of the curing step. The faster curing rate of the anti-adhesion outer coating composition allows the structural components to be stacked, bundled or rolled up, without the need to spend time to fully cure the primary coating composition. In some embodiments, the components of the anti-adhesion outer coating composition are selected so that after curing under the conditions of the curing step and being no more than 1 hour, or no more than 30 minutes, or no more than 15 minutes, or no more than 5 minutes, or no more than 2 minutes, or no more than 1 minute, the anti-adhesion outer coating composition is not easy to adhere.
[0065] Aqueous antiblock topcoat compositions particularly useful in the methods of the present invention comprise the following solid components dissolved or suspended in an aqueous solvent:
[0066] a) 1 to 10 wt % of a binder;
[0067] b) 1 to 20 wt% of a film-forming, high Tg polymer having a glass transition temperature of at least 80°C;
[0068] c) 1 to 25 wt % of a hydrophobic additive; and
[0069] d) optionally up to 70% by weight of fillers,
[0070] wherein (1) the solids content of the composition is at least 5% by weight; (2) the weight percentages listed for each of components (a)-(d) are based on the total weight of solids in the aqueous composition; and
[0071] and (3) the pH of the aqueous composition is between 2 and 6.
[0072] The binder has the description, exemplary embodiments, and exemplary concentrations described previously. In some embodiments, the binder is an acrylic polymer having a Tg no greater than 25°C.
[0073] The film-forming high Tg polymer has the description, exemplary embodiments, and exemplary concentrations described previously. In some embodiments, the film-forming high Tg polymer is an acrylic polymer, and in some embodiments, the acrylic polymer emulsifies in acidic solutions and is water-soluble or water-swellable in neutral or alkaline solutions.
[0074] The hydrophobic additives and fillers have the descriptions, exemplary embodiments and exemplary concentrations described previously. The aqueous composition may also have other additives as described previously.
[0075] In some embodiments, the pH of the aqueous composition is at least 4 or at least 5. In some embodiments, the pH of the aqueous composition is at most 7 or at most 6.
[0076] In the method of the present invention, the anti-adhesion outer coating composition is applied to the adhesion-forming surface. Known application methods can be used, such as spraying, brushing, roller coating, curtain coating or dipping. In some embodiments, the anti-adhesion outer coating composition is sprayed on the adhesion-forming surface.
[0077] After being applied to the adhesion-forming surface, the anti-adhesion outer coating composition is subjected to a curing step until it is no longer prone to adhesion (the term previously defined). In some embodiments, the temperature of the curing step is at least 20°C, or at least 35°C, or at least 50°C, or at least 75°C, or at least 100°C. In some embodiments, the curing temperature is at most 300°C, at most 250°C, or at most 225°C, or at most 200°C, or at most 160°C. In some embodiments, curing is accompanied by an air flow to take away solvent from the anti-adhesion composition. In some embodiments, curing is carried out under an air atmosphere, and in some embodiments, curing is carried out under an inert atmosphere such as nitrogen. In some embodiments, the curing step is completed in no more than 1 hour, or no more than 30 minutes, or no more than 15 minutes, or no more than 5 minutes, or no more than 2 minutes, or no more than 1 minute.
[0078] After the curing step is completed, the adhesion-forming surface of the structural assembly contains a layer of at least one primary coating composition, which is covered with a layer of at least one anti-adhesion outer coating. The region of the primary coating composition may be easy to adhere, except that the anti-adhesion outer coating of the solidification prevents the primary coating composition from contacting the surface except the adhesion-forming surface and therefore prevents adhesion. In some embodiments, the adhesion-forming surface (with anti-adhesion outer coating) can be pressed on another surface for at least 1 hour, or at least 6 hours, or at least 24 hours, and there is basically no adhesion. In some embodiments, the temperature in this pressure process can be up to 50 ° C. In some embodiments, the pressure can be up to 1psi, or at least 2psi, or at least 3psi. In some embodiments, the relative humidity can be up to 50%, or 57%, or 90%, or 100%.
[0079] The content of the anti-adhesion outer coating of drying reflects the solid content of the anti-adhesion outer coating composition applied and cured, with identical exemplary components and concentration.In some embodiments, the anti-adhesion outer coating of curing contains a solvent that is no more than 5 % by weight, or no more than 3 % by weight, or no more than 1 % by weight, or no more than 0.5 % by weight.There is no solvent of the required content in the outer coating, but in some cases, it may be unrealistic to remove the solvent to a content lower than 0.1 % by weight.The anti-adhesion outer coating does not have the necessary thickness, but in some embodiments, the average thickness of the outer coating is at least 5 μm, or at least 10 μm, or at least 25 μm, and in some embodiments, the average thickness is at most 600 μm, or at most 500 μm, or at most 300 μm.
[0080] Unlike many outer coatings used on structural components, the anti-adhesion outer coating of the present invention does not require high weather resistance or wear resistance. The anti-adhesion outer coating only needs to remain in place until the primary coating composition is fully cured and can not form adhesion. In many cases, the primary coating composition is fully cured within a few days or weeks after the curing step is completed. In many cases, the primary coating composition is fully cured before the structural component is received by the user and put into use. In many embodiments, after the structural component is put into use, the anti-adhesion outer coating is no longer needed. The anti-adhesion outer coating can be allowed to wear or weather over time, such as floor wax or polishing agent. In some embodiments, this use difference may affect the selection of additives in the anti-adhesion outer coating composition. The additives providing oxidation resistance, light resistance, scratch resistance, wear resistance and weather resistance can be unimportant and can be excluded from the anti-adhesion outer coating composition. The anti-adhesion outer coating intended to be worn or weathered in common use can be called a sacrificial outer coating.
[0081] In some embodiments, after 6 months of normal use, at least 25 weight %, or at least 50 weight %, or at least 75 weight % of the outer coating has been worn away from the structural component. In other embodiments, the structural component can be used for sheltering purposes, such as in a wall, and substantially no outer coating is worn away.
[0082] Example
[0083] The present invention is further illustrated by the following examples, which are intended to be illustrative and not limiting. Comparative examples are included to show the beneficial effects of some of the components of the present invention.
[0084] Substrate preparation
[0085] Preparation of Slow Curing Primary Coating Compositions An aqueous suspension of the pigment was prepared by blending the materials listed in Table 1A until a suspension formed.
[0086]
[0087]
[0088] After the suspension is formed, reduce the shear in the mixture and add the materials listed in Table 1 B in the order listed. Continue mixing for an additional hour or until smooth.
[0089]
[0090] 1 The polymer emulsion contains a random copolymer of 86% butyl acrylate, 12.3% methyl methacrylate and 1.7% methacrylic acid, with a Tg of -35°C and a concentration of 55% solids.
[0091] The materials in Table 1A and Table 1B add up to 100 wt%. The resulting primary coating composition contained 41 volume % solids and 56 wt% solids. A 100 mm wide GARDCO TM The primary coating composition was applied to aluminum Q panels (A412 ground finish, Q Labs Corporation) using a multi-gap square applicator (Paul N Gardner Company, Inc.) to cast a 381 micron thick wet film onto the substrate. Each coated panel was dried for 7 days under ambient conditions (21° C. and 50% RH).
[0092] Topcoat compositions and application :
[0093] Water in the amount shown in Table 2 was added to the container, and then the other ingredients shown in Table 2 were added to the container in the order and amounts shown in Table 2 and blended until uniform. The amounts shown are all parts by weight. The pH of each outer coating composition was tested.
[0094] Use 50mm wide GARDCO TM Each overcoat composition was applied to several of the previously described coated substrates using a multi-gap square applicator (Paul N. Gardner Company) to cast a 76 micron thick wet film onto the coated substrate. Some of the overcoated substrates were dried for 1 to 3 days at ambient conditions (about 21° C. and about 50% relative humidity). Other overcoated substrates were dried in an oven at 50° C. and about 30% relative humidity for 24 hours and then equilibrated at ambient conditions for 1-7 days.
[0095] test
[0096] Ambient temperature adhesion : Aluminum Q panels (A612 grinding and finishing, Q Labs) were cut into 5.12 cm × 5.12 cm (2 in × 2 in) squares, and the cut squares were placed directly on 5.12 cm × 5.12 cm (2 in × 2 in) squares of each ambient temperature cured outer coated panel. Each stack of panels was subjected to 10 psi pressure. The pressure was maintained for 4 hours and then removed. After 1 minute, the Q panels were removed to determine the anti-blocking properties. The nature of the coating damage and the amount of coating removed were recorded. If the Q panel was easily removed, the coating was qualified. If the removal of the Q panel required effort or damage to the primary coating or the anti-blocking outer coating, the coating was unqualified. For each coated Q panel, a total of two square coatings were tested under the indicated weight load, and if the results were the same (qualified or unqualified), the results were accepted. The results are shown in Table 2.
[0097] The same test was performed on two coated Q panel substrate squares having a primary coating but no anti-block topcoat. The squares without the topcoat also failed.
[0098] High temperature adhesion The foregoing test was repeated on the oven cured overcoated panels except that the pressed panels were placed in an oven at 50°C and about 30% relative humidity for 4 hours prior to testing. The results are shown in Table 2.
[0099]
[0100] Test Method
[0101] Glass transition temperature: ASTM E1356-08 (2014) Determination of glass transition temperature by differential scanning calorimetry
[0102] Oil absorption: ASTM D281(2021) determines the oil absorption of pigments by spatula rubbing.
Claims
1. An aqueous composition comprising the following solid components dissolved or suspended in an aqueous solvent: a) a binder in an amount sufficient to form a stable coating; b) 1 to 20 wt% of a film-forming high Tg polymer having a glass transition temperature (Tg) of at least 80°C; c) 1 to 25 wt % of a hydrophobic additive; and d) optionally up to 70% by weight of fillers, wherein (1) the solids content of the composition is at least 5 weight percent; (2) the weight percentages listed for each of components (a)-(d) are based on the total weight of the aqueous composition including solvent; and (3) the aqueous composition has a pH between 2 and 6.
2. The aqueous composition according to claim 1, wherein the binder comprises an acrylic polymer having a Tg of no more than 25°C.
3. The aqueous composition of claim 1, wherein the high Tg polymer comprises an acrylic polymer having a glass transition temperature of at least 90°C.
4. The aqueous composition of claim 1, wherein the high Tg polymer can form an emulsion in an acidic solution but is water-soluble or water-swellable in a neutral solution or an alkaline solution.
5. The aqueous composition of claim 1, wherein the hydrophobic additive comprises a wax, a silane, or a polyolefin polymer.
6. The aqueous composition according to any one of claims 1, comprising at least 8 wt% filler, based on the total weight of the composition.
7. The aqueous composition according to claim 1, wherein based on the total weight of the composition: a) the binder comprises an acrylic polymer having a Tg not exceeding 25°C and accounts for 1 wt% to 10 wt% of the aqueous composition; b) the high Tg polymer comprises an acrylic polymer having a glass transition temperature of at least 90°C and comprises at least 2% by weight of the aqueous composition; c) the hydrophobic additive comprises a wax, a silane or a polyolefin polymer and comprises at least 2% by weight of the aqueous composition; d) the filler comprises at least 8% by weight of the aqueous composition; e) the solids content of the aqueous composition is at least 20% by weight.
8. The aqueous composition of claim 1, wherein the composition is substantially free of antioxidant additives or light stabilizing additives.
9. A method for preventing adhesion of a structural component, the method comprising the following steps: a) providing a structural component comprising at least one surface ("adhesion-forming surface") coated with a primary coating composition that facilitates adhesion; b) applying an anti-blocking topcoat composition comprising the following components to the block-forming surface: i) solvent, ii) a binder, and iii) a film-forming high Tg polymer having a glass transition temperature above 80°C; and c) curing the anti-blocking top coating composition under conditions suitable for forming an anti-blocking top coating that is not prone to adhesion, Wherein "readily blocks" with respect to a composition means that the composition will adhere to a surface other than the block-forming surface which is pressed against the block-forming surface at a temperature of up to 50° C. for at least one hour.
10. A structural member comprising at least one surface coated with: a) at least one layer of a primary coating composition; and b) at least one layer of an anti-blocking top coating on top of said primary coating composition, said anti-blocking top coating comprising: i) 1 to 50 wt % of a binder; ii) 2 to 50 wt% of a film-forming, high Tg polymer having a glass transition temperature of at least 80°C; iii) 2 to 40 wt % of a hydrophobic additive; and iv) Optionally up to 70% by weight of fillers.
Citation Information
Patent Citations
Coating composition comprising autoxidisable component
CN101981126A
Coating compositions having increased block resistance
CN102089394A
Aqueous latex coating compositions
CN103261306A
Heat sealable substrate and a process for making the same
US20120302660A1
Highly Pigmented Aqueous Coating Compositions With Improved Resistance To Blocking
US20140200296A1