Polarizing film, laminated polarizing film, image display panel, and image display device

By directly bonding the transparent protective film to the polarizing film in the polarizing film and improving the adhesion through methods such as ultraviolet rays or electron beams, the problem of reduced orthogonal b value of the polarizing film in a hot and humid environment is solved and the durability of the display is achieved. performance and display performance.

CN118786368APending Publication Date: 2024-10-15NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023921.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-20
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In a hot and humid environment, the orthogonal b value of the polarizing film is easily reduced, resulting in a decrease in display performance. Especially when the transparent protective film on the viewing side is thin, the polarizing film has a blue problem.

Method used

A polarizing film structure is adopted, in which at least one of the first transparent protective film and the second transparent protective film is directly bonded to the polarizing film without passing through an adhesive layer or adhesive layer, and the first transparent protective film serves as a transparent layer on the visible side The protective film is thicker than the second transparent protective film and is bonded using ultraviolet or electron beam methods to improve adhesion, prevent moisture intrusion, and suppress changes in the orthogonal b value in a hot and humid environment.

Benefits of technology

It effectively prevents the iodine in the polarizing film from flowing out to the adhesive layer, prevents moisture intrusion, stabilizes the polarization performance, suppresses the change of the orthogonal b value in a hot and humid environment, and improves the durability and display performance of the display.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786368A_ABST
    Figure CN118786368A_ABST
Patent Text Reader

Abstract

The present invention pertains to a polarizing film constituting an image display panel, the polarizing film being provided with a first transparent protective film, a polarizing film, and a second transparent protective film in this order, the first transparent protective film and / or the second transparent protective film being directly bonded to the polarizing film without having an adhesive layer or an adhesive layer interposed therebetween, the first transparent protective film is a transparent protective film on the visible side and is thicker than the second transparent protective film. The polarizing film is capable of suppressing a change in the orthogonal b value even in a humid and hot environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizing film, a laminated polarizing film, an image display panel and an image display device. Background Art

[0002] In the past, as polarizing films used in various image display devices such as liquid crystal display devices and organic EL display devices, polyvinyl alcohol films that have been dyed (containing dichroic substances such as iodine and dichroic dyes) have been used because they have both high transmittance and high polarization degree. The polarizing film can be manufactured by subjecting the polyvinyl alcohol film to various treatments such as swelling, dyeing, cross-linking, and stretching in a bath, followed by washing and drying. In addition, the polarizing film is usually used in the form of a polarizing film (polarizer) having a transparent protective film such as triacetyl cellulose bonded to one or both sides with an adhesive.

[0003] The above-mentioned polarizing film can be stacked with other optical layers as needed and used in the form of a stacked polarizing film (optical laminate). In addition, the above-mentioned polarizing film or the above-mentioned stacked polarizing film (optical laminate) can be used in the form of an image display panel bonded to an image display unit such as a liquid crystal unit and an organic EL element. Furthermore, the above-mentioned image display panel is bonded to a front surface transparent plate (window layer) on the visible side, a front surface transparent component such as a touch panel, etc. via an adhesive layer or a bonding agent layer, and is used as the various image display devices mentioned above (patent document 1).

[0004] In addition, as the above-mentioned polarizing film (polarizing plate), there are also known polarizing films in which a polarizing film and a transparent protective film are directly bonded together without an adhesive layer or a pressure-sensitive adhesive layer (Patent Documents 2 to 5).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2014-102353

[0008] Patent Document 2: International Publication No. 2005 / 085918

[0009] Patent Document 3: Japanese Patent Application Publication No. 2002-303725

[0010] Patent Document 4: Japanese Patent Application Publication No. 2002-303726

[0011] Patent Document 5: Japanese Patent Application Publication No. 2002-303727 Summary of the invention

[0012] Problems to be solved by the invention

[0013] There is a strong demand for thinner polarizing films and polarizing films. In the above-mentioned image display device, for example, if the transparent protective film on the visible side is thin, there is a problem that the orthogonal b value decreases in a hot and humid environment and the polarizing film in the display has a blue tint.

[0014] In view of the above circumstances, an object of the present invention is to provide a polarizing film capable of suppressing a change in the orthogonal b value even in a hot and humid environment.

[0015] Another object of the present invention is to provide a laminated polarizing film, an image display panel, and an image display device using the above polarizing film.

[0016] Solutions to the problem

[0017] That is, the present invention relates to a polarizing film constituting an image display panel.

[0018] The above-mentioned polarizing film comprises a first transparent protective film, a polarizing film, and a second transparent protective film in sequence. At least one of the first transparent protective film and the second transparent protective film is directly bonded to the above-mentioned polarizing film without passing through an adhesive layer or a bonding agent layer. The first transparent protective film is a transparent protective film on the visible side, and its thickness is thicker than that of the second transparent protective film.

[0019] Moreover, the present invention relates to a laminated polarizing film in which the above-mentioned polarizing film is bonded to an optical layer.

[0020] The present invention also provides an image display panel in which the polarizing film is bonded to the side opposite to the visible side of the polarizing film of the polarizing film or the side opposite to the visible side of the polarizing film of the laminated polarizing film in an image display unit.

[0021] The present invention also relates to an image display device including a front surface transparent member on the polarizing film or laminated polarizing film side of the image display panel.

[0022] Effects of the Invention

[0023] The details of the mechanism of action of the effect of the polarizing film of the present invention can be estimated as follows. It should be noted that the interpretation of the present invention is not limited to this mechanism of action.

[0024] The polarizing film of the present invention relates to a polarizing film, which constitutes an image display panel, wherein the polarizing film sequentially comprises a first transparent protective film, a polarizing film, and a second transparent protective film, wherein at least one of the first transparent protective film and the second transparent protective film is directly bonded to the polarizing film without an adhesive layer or an adhesive layer, and the first transparent protective film is a transparent protective film on the visible side, and the thickness is thicker than the thickness of the second transparent protective film. As described above, it can be inferred that in the polarizing film of the present invention, since at least one of the first transparent protective film and the second transparent protective film is directly bonded to the polarizing film without an adhesive layer or an adhesive layer, the iodine in the polarizing film can be prevented from flowing out to the adhesive layer or the adhesive layer in a humid and hot environment. Furthermore, since the thickness of the first transparent protective film as the transparent protective film on the visible side is thicker than the thickness of the second transparent protective film, it is a structure that can prevent moisture from intruding into the polarizing film when exposed to a humid and hot environment, and moisture is easily separated from the unit side, and thus the change of the orthogonal b value in a humid and hot environment can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic cross-sectional view showing one embodiment of a polarizing film.

[0026] Figure 2 This is a schematic cross-sectional view showing one embodiment of an image display panel and an image display device.

[0027] Explanation of symbols

[0028] 10: Polarizing film

[0029] 11: Polarizing film

[0030] 12: No. 1 transparent protective film

[0031] 13: Second transparent protective film

[0032] 20 and 30: Adhesive layer or adhesive layer

[0033] 80: Front surface transparent component

[0034] 90: Image display unit

[0035] 100: Image display panel

[0036] 200: Image display device DETAILED DESCRIPTION

[0037] Figure 1 Schematic cross-sectional view showing one embodiment of the polarizing film of the present invention. Figure 1, one embodiment of the polarizing film 10 is shown in which the first transparent protective film 12 on the visible side, the polarizing film 11 , and the second transparent protective film 13 are directly bonded together in this order without an adhesive layer or a pressure-sensitive adhesive layer.

[0038] Figure 2 Schematic cross-sectional view showing one embodiment of the image display panel and the image display device of the present invention. Figure 2 , an embodiment of an image display panel 100 is shown in which the image display unit 90 is bonded with the polarizing film 10 on the opposite side of the visible side of the polarizing film via the adhesive layer or the adhesive layer 30. Figure 2 , one embodiment of an image display device 200 is shown in which a front surface transparent member 80 is provided on the polarizing film side of an image display panel 100 via a pressure-sensitive adhesive layer or an adhesive layer 20 .

[0039] <Polarizing film>

[0040] The polarizing film of the present invention is a polarizing film constituting an image display panel, and the polarizing film sequentially comprises a first transparent protective film, a polarizing film, and a second transparent protective film, and at least one of the first transparent protective film and the second transparent protective film is directly bonded to the polarizing film without an adhesive layer or a bonding agent layer, and the first transparent protective film is a transparent protective film on the visible side, and the thickness is thicker than the thickness of the second transparent protective film. It should be noted that the visible side (visible surface) refers to the visible side of the image display panel.

[0041] <Polarizing film>

[0042] The polarizing film is formed by adsorbing and aligning a dichroic substance such as iodine or a dichroic dye in a polyvinyl alcohol film. From the viewpoint of initial polarization performance of the polarizing film, the polarizing film is preferably an iodine-based polarizing film containing iodine as the dichroic substance.

[0043] The polyvinyl alcohol (PVA) film can be used without particular limitation. The polyvinyl alcohol (PVA) film has light transmittance in the visible light region and disperses and adsorbs dichroic substances such as iodine and dichroic dyes. As the material of the polyvinyl alcohol film, polyvinyl alcohol or its derivatives can be cited. As the derivatives of the polyvinyl alcohol, for example, polyvinyl formal, polyvinyl acetal; olefins such as ethylene and propylene; derivatives modified with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid and their alkyl esters, acrylamide, etc. The average polymerization degree of the polyvinyl alcohol is preferably about 100 to 10,000, more preferably about 1,000 to 10,000, and further preferably about 1,500 to 4,500. In addition, the saponification degree of the polyvinyl alcohol is preferably about 80 to 100 mol%, more preferably about 95 mol% to 99.95 mol. It should be noted that the average polymerization degree and the saponification degree can be obtained according to JIS K 6726.

[0044] The polarizing film can be obtained by a conventional method for producing a polarizing film, for example, by subjecting the polyvinyl alcohol film to any swelling step and washing step, and at least to a dyeing step, a crosslinking step, and a stretching step.

[0045] From the viewpoint of improving the initial polarization degree of the polarizing film, the thickness of the polarizing film is preferably 1 μm or more, more preferably 2 μm or more, and from the viewpoint of preventing the warping of the panel, it is preferably 15 μm or less, more preferably 10 μm or less, and further preferably 8 μm or less. In particular, in order to obtain a polarizing film having a thickness of about 8 μm or less, the following method for producing a thin polarizing film can be used, in which a laminate comprising a polyvinyl alcohol resin layer formed on a thermoplastic resin substrate is used as the polyvinyl alcohol film.

[0046] A polarizing film (thin polarizing film) can be obtained by an existing method for manufacturing a polarizing film, for example, by implementing a process of preparing a laminate by forming a polyvinyl alcohol resin layer (PVA resin layer) containing a polyvinyl alcohol resin (PVA resin) on one side of a long thermoplastic resin substrate; while transporting the obtained laminate in the length direction, performing an optional insolubilization treatment process, a cross-linking treatment process and a cleaning treatment process on the above-mentioned laminate; and at least performing an auxiliary stretching treatment process in a gas atmosphere, a dyeing treatment process and a stretching treatment process in an aqueous solution to obtain the laminate.

[0047] The polarizing film preferably exhibits absorption dichroism at any wavelength in the wavelength range of 380nm to 780nm. The monomer transmittance of the polarizing film is preferably 46.0% or less, more preferably 45.0% or less. On the other hand, the monomer transmittance is preferably 41.5% or more, more preferably 42.0% or more, and further preferably 42.5% or more. The polarization degree of the polarizing film is preferably 99.990% or more, and preferably 99.998% or less. The polarizing film used in the embodiment of the present invention can take into account both high monomer transmittance and high polarization degree. Representatively, the monomer transmittance is the Y value obtained by measuring and correcting for visibility using an ultraviolet visible spectrophotometer. In addition, the monomer transmittance is the value when the refractive index of one surface of the polarizer is converted to 1.50 and the refractive index of the other surface is converted to 1.53. Representatively, the polarization degree is based on the parallel transmittance Tp and the orthogonal transmittance Tc obtained by measuring and correcting for visibility using an ultraviolet visible spectrophotometer, and is obtained by the following formula.

[0048] Polarization degree (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0049] In addition, the orthogonal b value of the polarizing film is preferably greater than -10, more preferably greater than -7, and further preferably greater than -5. The upper limit of the orthogonal b value is preferably less than +10, more preferably less than +5. The orthogonal b value represents the hue when the polarizing film (polarizing film) is arranged in an orthogonal state. For example, when the orthogonal b value is as low as less than -10, the black display looks bluish and the display performance is reduced. It should be noted that the orthogonal b value can be measured by a spectrophotometer represented by LPF200.

[0050] <1st and 2nd transparent protective films>

[0051] The first transparent protective film is a transparent protective film on the visible side and is thicker than the second transparent protective film. It should be noted that, hereinafter, either the first transparent protective film or the second transparent protective film may be simply referred to as a transparent protective film.

[0052] The thickness of the first transparent protective film can be appropriately determined. From the perspective of durability and color change in a hot and humid environment, it is preferably 10 μm or more, more preferably 13 μm or more, further preferably 15 μm or more, and further preferably 20 μm or more. From the perspective of thinning the polarizing film, it is preferably 100 μm or less, more preferably 60 μm or less, and further preferably 30 μm or less. In addition, the thickness of the second transparent protective film can be appropriately determined. From the perspective of durability and color change in a hot and humid environment, it is preferably 1 μm or more, more preferably 3 μm or more, and further preferably 50 μm or less, and more preferably 20 μm or less.

[0053] From the viewpoint of durability in a hot and humid environment and thinning of the polarizer, the ratio of the thickness of the first transparent protective film to the thickness of the second transparent protective film (thickness of the first transparent protective film / thickness of the second transparent protective film) is preferably greater than 1.2, more preferably greater than 2.0. In addition, from the viewpoint of suppressing curling of the polarizer, it is preferably less than 15.0, more preferably less than 10.0.

[0054] The first and second transparent protective films are not particularly limited, and various transparent protective films used in polarizing films can be used. As the material constituting the transparent protective film, for example, a thermoplastic resin having excellent transparency, mechanical strength, thermal stability, moisture barrier properties, isotropy, etc. can be used. As the thermoplastic resin, for example, cellulose ester resins such as cellulose triacetate, polyester resins such as polyethylene terephthalate and polyethylene naphthalate, polyether sulfone resins, polysulfone resins, polycarbonate resins, nylon, polyamide resins such as aromatic polyamide, polyimide resins, polyolefin resins such as polyethylene, polypropylene, and ethylene-propylene copolymers, (meth) acrylic resins, cyclic or cyclic polyolefin resins having a norbornene structure (norbornene resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof can be cited. In addition, the transparent protective film may be a cured layer formed of a thermosetting resin or an ultraviolet curing resin such as (meth) acrylic acid, urethane, acrylic urethane, epoxy, silicone, etc. Among these, cellulose ester resins, polycarbonate resins, (meth) acrylic resins, cyclic polyolefin resins, and polyester resins are preferred.

[0055] The transparent protective film may use a phase difference plate having a front phase difference of 40 nm or more and / or a thickness direction phase difference of 80 nm or more. The front phase difference is usually controlled to be in the range of 40 to 200 nm, and the thickness direction phase difference is usually controlled to be in the range of 80 to 300 nm. When a phase difference plate is used as the transparent protective film, the phase difference plate also acts as a transparent protective film, so that thinness can be achieved.

[0056] As the above-mentioned phase difference plate, for example, there can be mentioned: a birefringent film formed by unidirectional or bidirectional stretching of a polymer raw material, an oriented film of a liquid crystal polymer, a phase difference plate formed by an oriented layer of a liquid crystal polymer supported by a film, etc. There is no particular restriction on the thickness of the phase difference plate, which is usually about 1 to 150 μm. It should be noted that the above-mentioned phase difference plate can also be used by laminating it on a transparent protective film without phase difference.

[0057] The transparent protective film may also contain any appropriate additives such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, anti-coloring agents, flame retardants, antistatic agents, pigments, colorants, etc. In particular, when the transparent protective film contains ultraviolet absorbers, the light resistance of the polarizing film can be improved.

[0058] A hard coating layer, an anti-reflection layer, an anti-adhesion layer, a diffusion layer, an anti-glare layer, or other layers may also be provided on the side of the first and second transparent protective films not bonded with the polarizing film. It should be noted that the hard coating layer, the anti-reflection layer, the anti-adhesion layer, the diffusion layer, the anti-glare layer, or other layers may be provided as a layer different from the protective film in addition to being provided as the protective film itself.

[0059] At least one of the first transparent protective film and the second transparent protective film is directly bonded to the polarizing film without an adhesive layer or an adhesive layer.

[0060] The method of directly bonding at least one of the first transparent protective film and the second transparent protective film to the polarizing film without passing through an adhesive layer or an adhesive layer can be cited as follows: a method of crimping, a method of bonding by irradiating energy rays such as ultraviolet rays, electron beams, etc., and in particular, from the viewpoint of improving adhesion, it is preferred to bond the transparent protective film and any one of the polarizing films, or both of the bonding surfaces by irradiating ultraviolet light and surface treatment, and then bond via a volatile medium, and dry the volatile medium. By the presence of the volatile medium, it is possible to fit closely to the bonding surface without mixing in bubbles, etc., and further, by drying the volatile medium, the adhesion of the bonding surface (interface) is significantly improved. As ultraviolet light, for example, the wavelength is preferably 250-100nm, more preferably 200-100nm, wherein, from the viewpoint of mass production, a wavelength of 172nm using a xenon excimer lamp is particularly preferred.

[0061] In addition, from the viewpoint of processing capacity, the illuminance of the ultraviolet light is preferably 1 mW / cm 2 More preferably, 50 mW / cm 2 In addition, from the viewpoint of adhesiveness, the accumulated light intensity is preferably 1 mJ / cm 2 More preferably, 50 mJ / cm 2 From the viewpoint of film damage, 5000 mJ / cm 2 Less than, more preferably 2000mJ / cm 2In addition, the temperature during ultraviolet irradiation is not particularly limited. From the perspective of stabilization of surface modification, it is preferably about 0 to 50°C, more preferably about 10 to 40°C. In the production of polarizing films, room temperature is convenient. In addition, as for the atmosphere during ultraviolet irradiation, the oxygen concentration can be 21% or less. From the perspective of treatment efficiency, the oxygen concentration is preferably 7.0% or less.

[0062] The volatile medium is not particularly limited, but is preferably a solvent such as water, ethanol, toluene, cyclohexane, or acetone from the viewpoint of drying efficiency, and more preferably water from the viewpoint of environment.

[0063] The heating temperature may be any temperature that can properly dry the volatile medium. For example, when the volatile medium is water, the heating temperature is preferably about 40 to 80° C., and more preferably about 50 to 70° C. In addition, the drying time is affected by the temperature of the polarizing film, and therefore cannot be generalized. The drying time is preferably about 1 minute to 60 minutes, and more preferably about 3 to 15 minutes. The drying step may be performed only once, or may be performed multiple times as needed.

[0064] The above-mentioned bonding can be performed by a roll laminator or the like.

[0065] The bonding interface between the polarizing film and the transparent protective film may include a modified layer or a high elastic layer resulting from treatment during bonding.

[0066] In the above-mentioned polarizing film, the adhesion force (peel strength) between the above-mentioned transparent protective film and the above-mentioned polarizing film at the bonding surface is preferably 0.5N / 15mm or more, more preferably 1.0N / 15mm or more, and further preferably 1.2N / 15mm or more in the peel strength measurement under the conditions of a peeling angle of 90° and a peeling speed of 1000mm / min.

[0067] In the polarizing film, the transparent protective film may be directly bonded to the other side of the polarizing film which is not the bonding side without a pressure-sensitive adhesive layer or an adhesive layer as described above, or the transparent protective film may be bonded via a pressure-sensitive adhesive layer or an adhesive layer.

[0068] As the adhesive forming the adhesive layer, various adhesives that have been used for polarizing films can be used, for example, rubber adhesives, acrylic adhesives, silicone adhesives, urethane adhesives, vinyl alkyl ether adhesives, polyvinyl alcohol adhesives, polyvinyl pyrrolidone adhesives, polyacrylamide adhesives, cellulose adhesives, etc. Among these, acrylic adhesives are preferred.

[0069] In addition, as the adhesive forming the above-mentioned adhesive layer, various adhesives that have been used for polarizing films can be used, for example, isocyanate adhesives, polyvinyl alcohol adhesives, gelatin adhesives, vinyl latexes, water-based polyesters, etc. These adhesives are usually used in the form of adhesives made of aqueous solutions (water-based adhesives) and contain 0.5 to 60% by weight of solid components. As the above-mentioned adhesives, in addition to the above, active energy ray-curing adhesives such as ultraviolet curing adhesives and electron beam curing adhesives can be mentioned. As the above-mentioned active energy ray-curing adhesive, for example, (meth)acrylate adhesives can be mentioned. As the curable component in the above-mentioned (meth)acrylate adhesive, for example, compounds having a (meth)acryloyl group and compounds having a vinyl group can be mentioned. Examples of compounds having a (meth)acryloyl group include: (meth)acrylic acid alkyl esters such as (meth)acrylic acid chain alkyl esters having 1 to 20 alkyl carbon atoms, (meth)acrylic acid alicyclic alkyl esters, and (meth)acrylic acid polycyclic alkyl esters; hydroxyl group-containing (meth)acrylic acid esters; epoxy group-containing (meth)acrylic acid esters such as glycidyl (meth)acrylate, etc. (meth)acrylate adhesives may also contain nitrogen-containing monomers such as hydroxyethyl (meth)acrylamide, N-methylol (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-ethoxymethyl (meth)acrylamide, (meth)acrylamide, and (meth)acryloyl morpholine. (Meth)acrylate adhesives may contain tripropylene glycol diacrylate, 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, cyclic trimethylolpropane formal acrylate, dimethoxypropane methyl acrylate, and the like. Multifunctional monomers such as alkanediol diacrylate and EO modified diglycerol tetraacrylate are used as crosslinking components. In addition, as a cationic polymerization curing adhesive, a compound having an epoxy group or an oxetane group can also be used. The compound having an epoxy group is not particularly limited as long as it has at least two epoxy groups in the molecule, and various commonly known curable epoxy compounds can be used. In addition, as a cationic polymerization curing adhesive, a compound having an epoxy group or an oxetane group can also be used. Among these, from the viewpoint of curability and productivity, an active energy ray curing adhesive of a (meth)acrylate adhesive is preferably used.

[0070] The coating of the above-mentioned adhesive can be carried out on either the transparent protective film side or the above-mentioned polarizing film side, or on both sides. After lamination, a drying process is carried out as needed to form an adhesive layer made of the coated dried layer. After the above-mentioned drying process, ultraviolet rays or electron beams can be irradiated as needed. The thickness of the above-mentioned adhesive layer is not particularly limited. When using an aqueous adhesive, it is preferably about 30 to 5000 nm, more preferably about 100 to 1000 nm. When using an ultraviolet curing adhesive, an electron beam curing adhesive, etc., it is preferably about 0.1 to 100 μm, more preferably about 0.5 to 10 μm.

[0071] <Laminated polarizing film>

[0072] In the laminated polarizing film (optical laminate) of the present invention, the polarizing film is attached to the optical layer. The optical layer is not particularly limited, for example, one or more layers of reflective plates, semi-transmissive plates, phase difference plates (including 1 / 2, 1 / 4 wave plates), viewing angle compensation films, etc., which are sometimes used in the formation of liquid crystal display devices, etc., can be used. As the laminated polarizing film, a reflective polarizing film or a semi-transmissive polarizing film formed by further laminating a reflective plate or a semi-transmissive reflective plate on the polarizing film, an elliptical polarizing film or a circular polarizing film formed by further laminating a phase difference plate on the polarizing film, a wide viewing angle polarizing film formed by further laminating a viewing angle compensation film on the polarizing film, or a polarizing film formed by further laminating a brightness enhancement film on the polarizing film can be cited.

[0073] An adhesive layer for laminating image display units such as liquid crystal cells and organic EL elements, and other components such as front surface transparent plates on the visible side and front surface transparent components such as touch panels, etc., may be provided on one or both sides of the above-mentioned polarizing film or the above-mentioned laminated polarizing film. As the adhesive layer, an adhesive layer is preferred. The adhesive forming the above-mentioned adhesive layer is not particularly limited, and an adhesive such as an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyether, a fluorine-based polymer, a rubber-based polymer may be appropriately selected for use. It is particularly preferred to use an adhesive having excellent optical transparency, showing appropriate wettability, cohesion and adhesion, and excellent weather resistance, heat resistance, etc., such as an adhesive containing an acrylic polymer.

[0074] The adhesive layer can be provided on one or both sides of the polarizing film or the laminated polarizing film in an appropriate manner. As for the provision of the adhesive layer, for example, there can be mentioned: preparing an adhesive solution and directly providing it on the polarizing film or the laminated polarizing film by an appropriate development method such as a casting method or a coating method; or forming an adhesive layer on a diaphragm and transferring it to the polarizing film or the laminated polarizing film. The thickness of the adhesive layer can be appropriately determined according to the purpose of use, the adhesive force, etc., and is generally 1 to 500 μm, preferably 5 to 200 μm, and more preferably 10 to 100 μm. The material having an adhesive layer provided on at least one side of the polarizing film or the laminated polarizing film is called a polarizing film with an adhesive layer, or a laminated polarizing film with an adhesive layer.

[0075] <Image display panel and image display device>

[0076] The image display panel of the present invention has the image display unit bonded with the polarizing film of the polarizing film on the opposite side of the visible side, or the polarizing film of the laminated polarizing film on the opposite side of the visible side. In addition, the image display device of the present invention has a front surface transparent member on the polarizing film or laminated polarizing film side (visible side) of the image display panel.

[0077] As the above-mentioned image display unit, for example, there can be mentioned: a liquid crystal unit, an organic EL unit, etc. As the above-mentioned liquid crystal unit, for example, any of a reflective liquid crystal unit that uses external light, a transmissive liquid crystal unit that uses light from a light source such as a backlight, and a semi-transmissive and semi-reflective liquid crystal unit that uses both light from the outside and light from the light source can be used. In the case where the above-mentioned liquid crystal unit uses light from a light source, the image display device (liquid crystal display device) is also provided with a polarizing film on the side opposite to the visible side of the image display unit (liquid crystal unit), and is also provided with a light source. The polarizing film on the light source side is preferably bonded to the liquid crystal unit via an appropriate adhesive layer. As the driving method of the above-mentioned liquid crystal unit, any type of method such as VA mode, IPS mode, TN mode, STN mode, bend orientation (π type) can be used.

[0078] As the organic EL unit, for example, an organic EL unit in which a transparent electrode, an organic light-emitting layer and a metal electrode are sequentially stacked on a transparent substrate to form a light-emitting body (organic electroluminescent light-emitting body) can be appropriately used. The organic light-emitting layer is a laminate of various organic thin films, and can adopt various layer structures, including, for example: a laminate of a hole injection layer formed of a triphenylamine derivative and a light-emitting layer formed of a fluorescent organic solid such as anthracene, a laminate of these light-emitting layers and an electron injection layer formed of a perylene derivative, or a laminate of a hole injection layer, a light-emitting layer and an electron injection layer.

[0079] As the front surface transparent member disposed on the visible side of the above-mentioned image display unit, for example, there can be cited: a front surface transparent plate (window layer), a touch panel, etc. As the above-mentioned front surface transparent plate, a transparent plate with appropriate mechanical strength and thickness can be used. As such a transparent plate, for example, a transparent resin plate such as an acrylic resin or a polycarbonate resin, or a glass plate, etc. can be used. As the above-mentioned touch panel, various touch panels such as a resistive film method, an electrostatic capacitance method, an optical method, an ultrasonic method, etc., a glass plate with a touch sensor function, a transparent resin plate, etc. can be used. In the case of using a touch panel of an electrostatic capacitance method as the above-mentioned front surface transparent member, it is preferred to set a front surface transparent plate made of glass or a transparent resin plate on the side closer to the visible side than the touch panel.

[0080] Example

[0081] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0082] <Example 1>

[0083] <Production of polarizing film>

[0084] A laminated body having a 9 μm thick PVA layer formed on an amorphous PET substrate was subjected to auxiliary stretching in a gas atmosphere at a stretching temperature of 130°C to produce a stretched laminated body, and then the stretched laminated body was dyed to produce a colored laminated body, and further, the colored laminated body was stretched in boric acid water at a stretching temperature of 65 degrees to produce an optical film laminated body including a 5 μm thick polarizing film stretched integrally with the amorphous PET substrate in a manner that the total stretching ratio reached 5.94 times. By such two-step stretching, an optical film laminated body including a polarizing film with a thickness of 5 μm was obtained, in which the PVA molecules of the PVA layer formed on the amorphous PET substrate were highly oriented, and the iodine adsorbed by dyeing was highly oriented in one direction in the form of a polyiodide ion complex.

[0085] <Production of polarizing film>

[0086] In a nitrogen-substituted atmosphere with an oxygen concentration of about 2.5%, an excimer UV treatment device (SVC342S-1N2-MN3-KWO1 manufactured by Ushio Electric Co., Ltd., xenon excimer lamp) was used to irradiate the polarizing film surface of the optical film laminate including the polarizing film obtained above and the cycloolefin resin film with a thickness of 25 μm (ZF12 manufactured by Zeon Co., Ltd., Japan) as the first transparent protective film with excimer UV light (wavelength 172 nm, peak illuminance 75 mW / cm 2 、Accumulated light quantity 450mJ / cm 2), surface modification was performed. Next, water was applied to the surface modified surface of each film, and before the water dried, the polarizing film and the transparent protective film were bonded together using a laminator, and then dried in an oven at 60°C for 5 minutes and 30 seconds to obtain a polarizing film in which the polarizing film and the first transparent protective film were directly bonded. In addition, the PET substrate of the polarizing film was peeled off, and a 3 μm thick cycloolefin resin film as the second transparent protective film was bonded in the same order as above (the cycloolefin resin film with release liner was obtained as follows: 10 g of cycloolefin polymer (COP) film (trade name "ZEONOR Film ZF14") was added to 90 g of a 2:3 mixed solvent of 2,4-trichlorobenzene and toluene to prepare a COP solution, and then the prepared COP solution was applied on the PET film (release liner) using a wire rod coater #13, and then dried in an oven at 60°C for 3 minutes, thereby laminating a 3 μm thick COP film on the release liner.), to obtain a polarizing film with transparent protective films directly bonded to both sides of the polarizing film.

[0087] <Evaluation of changes in orthogonal b-values ​​in a hot and humid environment>

[0088] The polarizing film obtained above was exposed to an environment of 60°C and 95% RH for 240 hours, and the orthogonal b value before and after exposure was measured using a spectrophotometer with an integrating sphere (V7100 manufactured by JASCO Corporation), and the change in the orthogonal b value Δb = (orthogonal b value before exposure) - (orthogonal b value after exposure) was obtained. The smaller the change in the orthogonal b value Δb, the better the durability in a harsh hot and humid environment. Δb is preferably less than 4.0, and more preferably less than 2.0.

[0089] <Evaluation of Adhesion Strength (Peel Strength) of First Transparent Protective Film>

[0090] A double-sided tape (No. 500, manufactured by Nitto Denko Corporation) was attached to the first transparent protective film side of the polarizing film formed by directly bonding the polarizing film to the first transparent protective film and the second transparent protective film. Further, a size of 200 mm parallel to the stretching direction of the polarizing film and 15 mm in the orthogonal direction was cut, and a cut was made between the polarizing film and the first transparent protective film with a cutter, and then the release film of the double-sided tape was peeled off, and the adhesive surface was attached to the glass plate. The polarizing film and the first transparent protective film were peeled off along the 90-degree direction at a peeling speed of 1000 mm / min using an angle-variable adhesive / film peeling analysis device (VPA-2, manufactured by Kyowa Interface Chemical Co., Ltd.), and the peeling strength (N / 15mm) was measured.

[0091] <Evaluation of Adhesion Strength (Peel Strength) of Second Transparent Protective Film>

[0092] The PET substrate on the second transparent protective film side of the polarizing film formed by directly bonding the above-mentioned polarizing film to the first transparent protective film and the second transparent protective film was peeled off, and a double-sided tape (No. 500, manufactured by Nitto Denko Corporation) was pasted on the peeling surface. Further, a size of 200 mm parallel to the stretching direction of the polarizing film and 15 mm in the orthogonal direction was cut out, and a cut was made between the polarizing film and the second transparent protective film with a cutter, and then the peeling film of the double-sided tape was peeled off, and the adhesive surface was pasted on the glass plate. The polarizing film and the second transparent protective film were peeled off along the 90-degree direction at a peeling speed of 1000 mm / min using an angle-variable adhesive / film peeling analysis device (VPA-2, manufactured by Kyowa Interface Chemical Co., Ltd.), and the peeling strength (N / 15mm) was measured.

[0093] <Example 2>

[0094] A polarizing film having transparent protective films directly bonded to both surfaces of the polarizing film was obtained by the same operation as in Example 1 except that a 13 μm-thick cycloolefin resin film (ZF14 manufactured by Zeon Corporation) was used as the first transparent protective film.

[0095] <Example 3>

[0096] As the first transparent protective film, the following active energy ray-curable adhesive was applied on a cycloolefin resin film with a thickness of 25 μm (ZF12 manufactured by Japan Zeon Co., Ltd.) using a wire rod coater, and then laminated to the polarizing film surface of the optical film laminate including a polarizing film with a thickness of 5 μm obtained in Example 1 using a laminator. In this state, active energy rays were irradiated from the transparent protective film side to cure the adhesive. Otherwise, a polarizing film having a transparent protective film directly bonded to one side of the polarizing film was obtained by the same operation as in Example 1.

[0097] [Active energy ray-curable adhesive]

[0098] 2-Hydroxyethylacrylamide (manufactured by KJ Chemical Co., Ltd., trade name: HEAA) 16.5 parts by weight, 4-vinylphenylboronic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) 1 part by weight, 2-hydroxy-3-phenoxypropyl acrylate (manufactured by Toagosei Co., Ltd., trade name: Aronix M-5700) 30.5 parts by weight, 1,9-nonanediol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., trade name: LIGHT ACRYLATE 1,9ND-A) 25 parts by weight, hydroxypivalic acid diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., trade name: LIGHT ACRYLATE HPP-A) 13 parts by weight, an oligomer obtained by polymerizing a (meth)acrylate (manufactured by Toagosei Co., Ltd., trade name: ARFON UP-1190) 15 parts by weight, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one (IGM 3 parts by weight of 2,4-diethylthioxanthone (manufactured by Nippon Kayaku Co., Ltd., trade name: KAYACURE-DETX-S)

[0099] [Active energy rays]

[0100] Visible light (gallium-encapsulated metal halide lamp) was used as active energy ray. Irradiation device: Light HAMMER 10 manufactured by Heraeus. Valve: V valve. Peak illuminance: 800 mW / cm 2 , cumulative exposure 800 / mJ / cm 2 (Wavelength: 380 to 440 nm) The illuminance of visible light was measured using a Sola-Check system manufactured by Solatell.

[0101] <Example 4>

[0102] Using a wire bar coater, the above-mentioned active energy ray-curable adhesive was applied onto a 3 μm thick cycloolefin resin film as the second transparent protective film (a cycloolefin resin film with a release liner obtained as follows: after preparing a COP solution by adding 10 g of a cycloolefin polymer (COP) film (trade name "ZEONOR Film ZF14") to 90 g of a 2:3 mixed solvent of 2,4-trichlorobenzene and toluene, the prepared COP solution was applied to a PET film (release liner) using a wire bar coater #13, and then dried in an oven at 60°C for 3 minutes, thereby laminating a 3 μm thick COP film on the release liner.), and using a laminator, it was laminated to the polarizing film surface of the polarizing film formed by directly bonding the polarizing film obtained in Example 1 to the first transparent protective film. In this state, active energy rays were irradiated from the transparent protective film side to cure the adhesive. Except for this, a polarizing film having a transparent protective film directly bonded to one side of the polarizing film was obtained by the same operation as Example 1.

[0103] <Example 5>

[0104] <Production of polarizing film>

[0105] A polyvinyl alcohol film with an average degree of polymerization of 2400 and a saponification degree of 99.9 mol% and a thickness of 45 μm was immersed in warm water at 30°C for 60 seconds to swell. Next, it was immersed in an aqueous solution of 0.3% iodine / potassium iodide (weight ratio = 1 / 7), and the film was dyed while being stretched to 2.6 times. Then, it was stretched in a 4 wt% boric acid aqueous solution at 65°C so that the total stretching ratio reached 6 times. After stretching, it was dried in an oven at 55°C for 1 minute to obtain a PVA-type polarizing film. The thickness of the polarizing film is 18 μm and the moisture content is 15 wt%.

[0106] <Production of polarizing film>

[0107] Using the polarizing film obtained above, the same operation as in Example 1 was performed to obtain a polarizing film in which transparent protective films were directly bonded to both surfaces of the polarizing film.

[0108] <Comparative Example 1>

[0109] The above-mentioned active energy ray curing adhesive was applied to a cycloolefin resin film (ZF12 manufactured by Japan Zeon Co., Ltd.) with a thickness of 25 μm as the first transparent protective film using a wire bar coater, and the polarizing film surface of the optical film laminate including a polarizing film with a thickness of 5 μm obtained in Example 1 was laminated using a laminator. In this state, active energy rays were irradiated from the transparent protective film side to cure the adhesive. In addition, the PET substrate located on the opposite side of the first transparent protective film was peeled off, and the cycloolefin resin film with a thickness of 3 μm described in Example 1 as the second transparent protective film was laminated in the same order as above, and a polarizing film in which the transparent protective film was connected to both sides of the polarizing film via an active energy ray adhesive was obtained.

[0110] <Comparative Example 2>

[0111] A polarizing film in which the transparent protective films were in contact with both surfaces of the polarizing film via an active energy ray adhesive was obtained in the same manner as in Comparative Example 1 except that a 13 μm-thick cycloolefin resin film (ZF14 manufactured by Zeon Corporation) was used as the first transparent protective film.

[0112] <Comparative Example 3>

[0113] As the first transparent protective film, a 3 μm thick cycloolefin resin film was used (a cycloolefin resin film with a release liner obtained as follows: 10 g of a cycloolefin polymer (COP) film (trade name "ZEONOR Film ZF14") was added to 90 g of a 2:3 mixed solvent of 2,4-trichlorobenzene and toluene to prepare a COP solution, and then the prepared COP solution was applied to a PET film (release liner) using a wire bar coater #13, and then dried in an oven at 60°C for 3 minutes, thereby laminating a 3 μm thick COP film on the release liner.), and as the second transparent protective film, a 13 μm thick cycloolefin resin film (ZF14, manufactured by Zeonor Co., Ltd. of Japan) was used. Except for this, a polarizing film having transparent protective films directly bonded to both sides of the polarizing film was obtained by the same operation as in Example 1.

[0114] <Comparative Example 4>

[0115] A roll laminator was used to press a 40 μm thick cycloolefin resin film (manufactured by Japan Zeon Co., Ltd., ZF14) as a first transparent protective film onto the polarizing film surface of the optical film laminate containing the polarizing film obtained in Example 1 at a temperature of 145°C to obtain a polarizing film in which the polarizing film and the first transparent protective film were directly bonded. In addition, the PET substrate of the polarizing film was peeled off, and a 40 μm thick cycloolefin resin film (manufactured by Japan Zeon Co., Ltd., ZF14) was pressed at a temperature of 145°C to obtain a polarizing film in which the polarizing film and the transparent protective film were directly bonded.

[0116] The polarizing films obtained in the above-mentioned examples and comparative examples were used to perform the same evaluation as in Example 1. The results are shown in Table 1. It should be noted that the polarizing film obtained in Comparative Example 4 was wrinkled and cracked when exposed to an environment of 60°C and 95% RH for 240 hours in the above-mentioned <Evaluation of Changes in Orthogonal b Values ​​in a Wet and Hot Environment>.

[0117]

Claims

1. A polarizing film constituting an image display panel, The polarizing film comprises a first transparent protective film, a polarizing film, and a second transparent protective film in this order. At least one of the first transparent protective film and the second transparent protective film is directly bonded to the polarizing film without an adhesive layer or a bonding agent layer. The first transparent protective film is a transparent protective film on the visible side, and is thicker than the second transparent protective film.

2. The polarizing film according to claim 1, wherein The thickness of the first transparent protective film is 10 μm or more.

3. The polarizing film according to claim 1 or 2, wherein: The polarizing film has a thickness of 20 μm or less.

4. The polarizing film according to any one of claims 1 to 3, wherein The ratio of the thickness of the first transparent protective film to the thickness of the second transparent protective film (the thickness of the first transparent protective film / the thickness of the second transparent protective film) is 1.2 or more.

5. The polarizing film according to any one of claims 1 to 4, wherein The first transparent protective film and the second transparent protective film are directly bonded to the polarizing film without an adhesive layer or a pressure-sensitive adhesive layer. 6 . A laminated polarizing film comprising the polarizing film according to claim 1 bonded to an optical layer.

7. An image display panel, wherein: The side opposite to the visible side of the polarizing film of any one of claims 1 to 5 or the side opposite to the visible side of the polarizing film of the laminated polarizing film of claim 6 is bonded to an image display unit. 8 . An image display device comprising a front surface transparent member on the polarizing film or laminated polarizing film side of the image display panel according to claim 7 .