Automatic TIG (Tungsten Inert Gas) welding method for plates

By forming a groove and adjusting the electrode angle and movement during automatic TIG welding, the problem that the front and rear ends of the butt weld cannot be formed in automatic welding is solved, efficient aluminum alloy plate welding is achieved, and Class I weld quality and high-efficiency production are achieved .

CN118789076APending Publication Date: 2024-10-18SICHUAN AEROSPACE FENGHUO SERVO CONTROL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078149.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The existing automatic TIG welding technology is difficult to form at the beginning and end of the butt weld, and the welding quality and production efficiency are low. It cannot meet the Class I weld requirements in the "Technical Requirements for Welding of Aluminum and Aluminum Alloys".

Method used

An automatic TIG welding method is used to form a groove at the joint of the plates, and the arc starting, welding and arc closing angles of the electrode are adjusted during the welding process, combined with the swing and dwell actions of the electrode, to ensure the stability and consistency of the weld. It avoids the use of starting and closing arc plates and reserved process tails.

Benefits of technology

It is possible to directly complete automatic TIG welding without adding a starting and closing arc plate or reserving a process tail. The weld quality reaches Grade I standard, the pass rate of one-time inspection reaches more than 99%, and the production efficiency increases by more than 300%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118789076A_ABST
    Figure CN118789076A_ABST
Patent Text Reader

Abstract

The invention discloses an automatic TIG (Tungsten Inert Gas) welding method for a plate. The automatic TIG welding method comprises the following steps: (1) forming a groove; (2) arcing preheating is conducted, specifically, an electrode is arranged at the height position 5-10 mm away from the bottom of the groove, the electrode starts to move from the position 5-30 mm away from the starting end of the groove to the tail end of the groove, when the electrode is 4-8 mm away from the tail end of the groove, the electrode is lifted upwards for the first time and continues to move towards the tail end of the groove, and when the electrode reaches the tail end of the groove, the first-time lifting is stopped; (3) welding: lifting the electrode for the second time, and gradually swinging left and right for sealing; the electrode swings to return and then moves towards the starting end of the groove; (4) arc extinguishing and sealing: when the non-last layer is welded, arc extinguishing is gradually carried out when the electrode is 3mm-7mm away from the starting end; and when the last layer is welded, the electrode is slowly lifted up when reaching the end face of the starting end, swings left and right after reaching the end face and then returns, and arc extinguishing is gradually performed. The problem that automatic welding cannot achieve forming at the head end and the tail end of a butt welding seam can be solved, the welding machining quality can be effectively guaranteed, and the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a plate welding technology, and in particular to an automatic TIG welding method for a plate. Background Art

[0002] At present, taking aluminum alloy as an example, TIG welding (argon arc welding) of aluminum alloy plate butt welds can be divided into three methods according to the degree of automation: manual welding, semi-automatic welding, and automatic welding. However, in the current production process, no matter which of the above methods is used, the welding quality is extremely difficult to meet the requirements of Class I welds in the "Technical Requirements for Fusion Welding of Aluminum and Aluminum Alloys", and the first inspection pass rate is relatively low, generally less than 50%, and even after 1 to 2 repair welding, it may not be qualified.

[0003] (1) Manual TIG welding

[0004] Generally, only one set of welding parameters is needed to complete the welding of a single-layer weld, and the welding quality is guaranteed by the operator's experience and technique. The advantages are flexible operation, good weld quality, and small deformation and stress; the disadvantages are that it is too dependent on the operator's welding technique and experience, the heat-affected zone of the weld is large, the production efficiency is low, the consistency is poor, and the arc, high temperature, dust, metal gas, radiation, etc. generated by welding are harmful to the operator's health.

[0005] (2) Semi-automatic TIG welding

[0006] Currently, only some welding operations have been automated, while the rest of the work still needs to be done manually. Its advantages and disadvantages are between manual welding and automatic welding.

[0007] (3) Automatic TIG welding

[0008] Single-layer welds generally require three sets of welding parameters, namely arc starting, welding, and arc ending. The advantages are high production efficiency, good welding quality and consistency, and can reduce the labor intensity of operators; the disadvantages are high equipment costs and poor flexibility during the welding process. Most importantly, if the ends of the butt weld are directly welded automatically, defects such as molten pool welding liquid outflow, weld collapse and burn-through will occur. If the heat input is slightly smaller, the parent material will be difficult to melt, and defects such as incomplete fusion or incomplete penetration will occur. Therefore, it is almost impossible to complete the weld formation at the ends of the weld only through automatic welding. There is currently no precedent for directly forming butt welds through automatic welding at home and abroad.

[0009] At present, the commonly used method at home and abroad is to add arc starting and closing plates or reserve process tails to introduce welding defects at the beginning and end of the butt weld. After the entire weld is welded, the arc starting and closing plates or process tails are removed by mechanical processing or electrical processing. This method can only alleviate the problem that automatic welding cannot form at the beginning and end of the butt weld to a certain extent, but the subsequent removal processing may cause damage or stress to the parts; at the same time, the entire production process is relatively cumbersome, which greatly weakens the processing efficiency of automatic welding and is far away from the original intention of automated production.

[0010] Therefore, there is an urgent need to invent an automatic TIG welding method for plates to overcome the problem that automatic welding cannot form at the beginning and end of the butt weld, which can not only ensure the welding processing quality, but also improve production efficiency. Summary of the invention

[0011] The purpose of the present invention is to provide an automatic TIG welding method for plates, which can not only overcome the problem that automatic welding cannot form a shape at the beginning and end of the butt weld, but also effectively ensure the welding processing quality and improve production efficiency.

[0012] To achieve the purpose of the present invention, the technical solution adopted is: an automatic TIG welding method for a plate, wherein the single-sided welding layer is a single layer in total, specifically comprising the following steps:

[0013] S1. Bevel formation: butt the two plates to be welded together to form a bevel at the butt joint of the two plates;

[0014] S2. Arc preheating: Place the electrode at a height of 5mm to 10mm from the bottom of the groove, and move the electrode from 5mm to 30mm from the starting end of the groove to the end of the groove. When the electrode is 4mm to 8mm away from the end of the groove, lift it up for the first time, and stop lifting it at the end of the groove.

[0015] S3, welding: start welding while the electrode is lifted for the second time, and gradually swing left and right to seal; then perform transition and welding, and the electrode swings back to the positive position and moves toward the starting end of the groove;

[0016] S4. Arc closure and sealing: When the electrode reaches 3mm to 7mm away from the starting end of the groove, adjust the welding angle. After staying for a certain period of time, continue to move toward the end face of the starting end of the groove and lift it for the third time. When the electrode reaches the end face of the starting end of the groove, swing left and right and then return to the center, and gradually extinguish the arc.

[0017] Furthermore, when the single-sided welding layer is not less than two layers, when welding a layer other than the last layer, the electrode adjusts the welding angle when it reaches 3mm to 7mm from the starting end of the groove, stays for a certain time, then lifts up for the third time and gradually extinguishes the arc; when welding the last layer, the electrode adjusts the welding angle when it reaches 3mm to 7mm from the starting end of the groove, stays for a certain time, then continues to move toward the end face of the starting end of the groove and lifts up for the third time, and when the electrode reaches the end face of the starting end of the groove, it swings left and right and then returns to the center, and gradually extinguishes the arc.

[0018] Furthermore, the height of the first lift is 2 mm to 5 mm.

[0019] Furthermore, in the arc starting preheating stage, the angle between the electrode axis direction and the electrode forward direction is 65° to 85°.

[0020] Furthermore, in the arc starting preheating stage, the angle between the electrode axis direction and the electrode forward direction is 72.5°.

[0021] Furthermore, during the welding stage, the angle between the electrode axis direction and the electrode forward direction is 95° to 105°.

[0022] Furthermore, during the welding stage, the angle between the electrode axis direction and the electrode forward direction is 97.5°.

[0023] Furthermore, during the welding stage, the electrode stays for 0s to 1s after being swung into position; during the arc closing and sealing stage, the electrode stays for 0.5s to 1.5s after being swung into position.

[0024] Furthermore, during the welding stage, the electrode stays for 0.5 seconds after being swung into place; during the arc closing and sealing stage, the electrode stays for 1 second after being swung into place.

[0025] Furthermore, in the arc closing and sealing stage, after the welding angle is adjusted, the angle between the electrode axis direction and the electrode forward direction is 100°.

[0026] Furthermore, in the arc closing and sealing stage, the electrode stays for 0.5s to 1.5s after adjusting the welding angle.

[0027] Furthermore, in steps S2 to S4, the ambient temperature is 15° C. to 30° C., the humidity is ≤70%, and the purity of argon is ≥99.99%.

[0028] Furthermore, the air supply time before step S3 and the continued air supply time after step S4 are both no less than 5 seconds.

[0029] Furthermore, the groove formed at the butt joint of the two plates to be welded is one of Y-shaped, V-shaped, U-shaped and X-shaped.

[0030] Furthermore, taking aluminum alloy plates as an example, before arc preheating, the preheating temperature of the parts is 60°C to 150°C, the preheating time is 30min to 60min, and pads are placed under the two plates during welding.

[0031] The beneficial effects of the present invention are:

[0032] By adopting the automatic TIG welding method of the plate provided by the present invention, automatic TIG welding can be directly completed without adding arc starting and closing plates or reserving process tails, thereby improving welding stability and workpiece consistency. At the same time, the weld quality can meet the Class I weld requirements in the "Technical Requirements for Fusion Welding of Aluminum and Aluminum Alloys", and the one-time inspection pass rate can reach more than 99%. Compared with manual welding, automatic welding with starting and closing plates, and automatic welding with process tails, the production efficiency is improved by more than 300%. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The accompanying drawings illustrate exemplary embodiments of the present invention and together with the description serve to explain the principles of the present invention. These drawings are included to provide a further understanding of the present invention and are incorporated in and constitute a part of this specification.

[0034] Figure 1 is a schematic structural diagram of the aluminum alloy plate in Example 2;

[0035] Figure 2 is a schematic diagram of the structure after two aluminum alloy plates are butt-jointed in Example 2;

[0036] Figure 3 is a pulse waveform diagram of the welding robot during the welding process in Example 2;

[0037] Figure 4 is a schematic diagram of establishing a three-dimensional rectangular coordinate system before welding in Example 2;

[0038] Figure 5 is an enlarged view of the three-dimensional rectangular coordinate system in Example 2;

[0039] Figure 6 is a schematic diagram of double-sided double-layer welding in Example 2;

[0040] Figure 7-Figure 17 This is a diagram showing the movement trajectory of the electrode during welding of the first layer of the front / back weld in Example 2;

[0041] Figure 18-Figure 30 This is a diagram showing the movement trajectory of the electrode during welding of the second layer of the front / back weld in Example 2. DETAILED DESCRIPTION

[0042] The present invention will be further described in detail below in conjunction with the accompanying drawings and implementations. It is to be understood that the specific implementations described herein are only used to explain the relevant content, rather than to limit the present invention. It is also necessary to explain that, for ease of description, only the parts related to the present invention are shown in the accompanying drawings.

[0043] It should be noted that, in the absence of conflict, the embodiments and features of the embodiments of the present invention can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0044] Example 1

[0045] This embodiment provides an automatic TIG welding method for a plate. When single-sided welding and the total welding layer on the single side is one layer, that is, single-sided single-layer welding, the specific steps are as follows:

[0046] S1. Groove formation: Process the welding groove on the plate to be welded, and clean and dry the plate to be welded, welding wire, etc. mechanically or chemically. Clamp and fix the two plates to be welded by two clamps respectively, and butt the two plates to be welded, so that a V-shaped groove, Y-shaped groove or U-shaped groove is formed between the upper surfaces of the two butted plates to be welded. During the butt-joining process of the two plates to be welded, if the stability of the two plates to be welded can be guaranteed, the two butted plates to be welded do not need to be spot welded; if the stability of the two plates with welding cannot be guaranteed, the two butted plates to be welded need to be spot welded.

[0047] S11. Establishing a three-dimensional rectangular coordinate system: After the two plates to be welded are butt-jointed, a three-dimensional rectangular coordinate system is established at one end of the V-shaped groove. The three-dimensional rectangular coordinate system takes one end of the bottom of the groove as the origin O(0, 0, 0) (the origin is the bottom end of the groove), wherein the X-axis direction is consistent with the length direction of the V-shaped groove, the Y-axis direction is consistent with the width direction of the V-shaped groove, and the Z-axis direction is consistent with the depth direction of the V-shaped groove, that is, the X-axis origin is based on the end face of one end of the groove, the Y-axis origin is based on the middle section of the groove, and the Z-axis origin is based on the lowest point of the groove.

[0048] S2. Arc starting preheating: After the three-dimensional rectangular coordinate system is established, a small current ignites the arc, and the robot arm drives the electrode to move toward the tail end of the groove at a distance of 5mm to 15mm from the origin of the Z axis of the three-dimensional rectangular coordinate system and 5mm to 30mm from the origin of the X axis of the three-dimensional rectangular coordinate system, that is, the arc starting coordinates of the electrode are (5-30, 0, 5-15); the electrode is driven by the robot arm to lift up the electrode for the first time when it is 4mm to 8mm away from the tail end of the groove, and the robot arm drives the electrode to lift up for the first time while continuing to move toward the tail end of the groove, and the electrode stops lifting for the first time when it moves to a position flush with the end face of the tail end of the groove. At this time, the Z axis coordinate of the electrode is greater than the Z axis coordinate of the electrode in the initial state.

[0049] S3. Welding:

[0050] Starting welding and sealing: the robot arm drives the electrode to be lifted for the second time, and during the second lifting of the electrode, the robot arm drives the electrode to swing to the left side of the groove (Y+ direction) and then to the right side of the groove (Y- direction), or the robot arm drives the electrode to swing to the right side of the groove (Y- direction) and then to the left side of the groove (Y+ direction). After the robot arm drives the electrode to swing to both sides of the groove, the robot arm drives the electrode to gradually return to the central axis of the groove, that is, the robot arm drives the electrode to gradually return to the Y-axis coordinate of 0, and the electrode returns to the height position of the first lifting; specifically, when the robot arm drives the electrode to swing left and right toward the groove, the electrode is lifted for the second time when it swings in the forward direction, and the electrode keeps the height unchanged when it swings back;

[0051] Transition and welding: After the robot arm drives the electrode to gradually return to the center axis of the groove, the robot arm drives the electrode to gradually move toward the starting end of the groove, that is, the robot arm drives the electrode to gradually move toward the origin of the X-axis coordinate.

[0052] S4. Arc closure and sealing: When the robot arm drives the electrode to a distance of 3mm to 7mm from the origin of the X-axis coordinate, the robot arm drives the electrode to rotate and adjusts the angle between the electrode axis direction and the electrode forward direction. Then, the robot arm drives the electrode to gradually move to the starting end of the groove. The electrode moves toward the starting end of the groove and the robot arm drives the electrode to lift up for the third time. When the electrode is flush with the end surface of the starting end of the groove, that is, the X-axis coordinate of the electrode is 0, the robot arm drives the electrode to swing to the left side of the groove (Y+ direction) and then to the right side of the groove (Y- direction), or the robot arm drives the electrode to swing to the right side of the groove (Y- direction) and then to the left side of the groove (Y+ direction) based on the height. In the process of the robot arm driving the electrode to swing left and right toward the groove, the X-axis coordinate and Z-axis coordinate of the electrode do not change, only the Y-axis coordinate of the electrode changes; the arc is gradually extinguished after the electrode returns to the normal position.

[0053] In this embodiment, when the electrode is 4 mm to 8 mm away from the rear end of the groove, the height of the first upward lift is 2 mm to 5 mm.

[0054] In this embodiment, in the arc starting preheating stage, the angle between the electrode axis direction and the electrode forward direction is 65°~85°, that is, the angle between the electrode axis direction coordinate X+ direction is 65°~85°; preferably, in the arc starting preheating stage, the angle between the electrode axis direction and the electrode forward direction is 72.5°; in the welding stage, the angle between the electrode axis direction and the electrode forward direction is 95°~105°, that is, the angle between the electrode axis direction coordinate X+ direction is 95°~105°; preferably, in the welding stage, the angle between the electrode axis direction and the electrode forward direction is 97.5°.

[0055] In this embodiment, during the welding stage, the robot arm drives the electrode to swing into place and stays for 0s to 1s; during the arc closing and sealing stage, the robot arm drives the electrode to swing into place and stays for 0.5s to 1.5s; preferably, during the welding stage, the robot arm drives the electrode to swing into place and stays for 0.5s; during the arc closing and sealing stage, the robot arm drives the electrode to swing into place and stays for 1s.

[0056] In this embodiment, in the arc closing and sealing stage, when the robot arm drives the electrode to a distance of 3mm to 7mm from the starting end of the groove, the angle between the electrode axis direction and the electrode forward direction is 100°. At the same time, after the robot arm drives the electrode to adjust the angle, the electrode stays for 0.5s to 1.5s, and then lifts up to extinguish the arc. It should be noted that in this embodiment, whether it is the first or second time to adjust the angle between the electrode axis direction and the electrode forward direction, the position of the electrode tip remains unchanged, that is, when adjusting the angle between the electrode axis direction and the electrode forward direction, the adjustment is made with the electrode tip as the center.

[0057] In this embodiment, in steps S2 to S4, the ambient temperature is 15° C. to 30° C., the ambient humidity is ≤70%, and the purity of argon gas is ≥99.99%.

[0058] In this embodiment, the air supply time before step S3 and the continued air supply time after step S4 are both no less than 5 seconds.

[0059] In this embodiment, after the two clamps respectively clamp and fix the two plates to be welded, the plates and the parts required for welding need to be preheated. Taking the aluminum alloy plate as an example, the preheating temperature is 60℃~150℃, and the preheating time is 20min~40min. At the same time, when or before the two plates are welded, a pad is placed under the two plates. When the plates to be welded change, the preheating temperature and preheating time of the plates can be adjusted according to actual needs, for example: the preheating temperature is selected to be 120℃, etc.

[0060] In this embodiment, the electrode is a tungsten electrode.

[0061] The TIG welding method provided in this embodiment is applicable to welding with Y-shaped, V-shaped, and U-shaped grooves, but is not only applicable to Y-shaped, V-shaped, and U-shaped grooves, for example, J-shaped grooves, etc., that is, the TIG welding method has no restrictions on the shape of the groove.

[0062] Example 2

[0063] In the automatic TIG welding method of a plate provided in this embodiment, when single-sided welding is performed and the total weld layer on the single side is two layers, that is, single-sided double-layer welding, the welding method of the first weld layer in the groove is different from the welding method disclosed in Embodiment 1, and the difference is that:

[0064] When the first weld layer in the groove is performing arc closing and sealing in step S4, when the robot arm drives the electrode to a distance of 3mm to 7mm from the origin of the X-axis coordinate, the robot arm drives the electrode to rotate and adjusts the angle between the electrode axis direction and the electrode forward direction. The electrode then stays still for 0.5s to 1.5s. Finally, the robot arm drives the electrode to lift it directly upward for the third time, and the arc is gradually extinguished during the third lifting process.

[0065] The welding method of the second welding layer in the groove is the same as that in Example 1.

[0066] Example 3

[0067] The present embodiment provides an automatic TIG welding method for a plate. When single-sided welding is performed and the total number of weld layers on the single side is n layers (n≥3), that is, single-sided n-layer welding, the welding method from the first weld layer to the n-1th weld layer in the groove is the same as the first layer welding method disclosed in Example 2, and the welding method of the nth weld layer is the same as the welding method disclosed in Example 1.

[0068] However, the width of the groove gradually increases from the bottom of the groove to the opening of the groove. Therefore, when the electrode is welding the second, third, ... nth layer, as the number of welding layers increases, the speed at which the robot arm drives the electrode to move along the length direction of the groove can be gradually reduced, thereby ensuring that the solder can fill the entire width of the groove; of course, the path of the electrode in the process of moving along the length direction of the groove can also be adjusted, for example, the path of the electrode is in a zigzag shape, a crescent shape, a circle shape, etc.

[0069] Example 4

[0070] The present embodiment provides an automatic TIG welding method for a plate. When two plates are butted together and the grooves formed are two, front and back, and the groove shape of the front groove is the same as the groove shape of the back groove, that is, double-sided welding, for example, the groove is X-shaped. At this time, the welding method of the front groove is the same as the welding method of the back groove. Specifically, when the welding layer in the front groove is 1 layer, the welding method of the welding layer in the front groove is the same as that in Example 1; when the welding layer in the back groove is 1 layer, the welding method of the welding layer in the back groove is the same as that in Example 1; when the welding layer in the front groove is 2 layers, the welding method of the welding layer in the front groove is the same as that in Example 2; when the welding layer in the back groove is 2 layers, the welding method of the welding layer in the back groove is the same as that in Example 2; when the welding layer in the front groove is n layers, and n≥3, the welding method of the welding layer in the front groove is the same as that in Example 3; when the welding layer in the back groove is n layers, and n≥3, the welding method of the welding layer in the back groove is the same as that in Example 3.

[0071] However, it should be noted that when the grooves formed by the two plates after butt joint are two, the front and back welding layers are welded alternately, that is, the first layer on the front → the first layer on the back → the second layer on the front → the second layer on the back → the third layer on the back...

[0072] In addition, when there are two grooves on the front and back sides formed after the two plates are butt-jointed, a stainless steel gasket is still required to be set on the back side of the groove when welding the first layer of the front groove, but no stainless steel gasket is required when welding the back groove and subsequent welding layers.

[0073] In this embodiment, although it is pointed out that the groove is X-shaped, the shape and depth of the two grooves are not limited as long as the two plates have two grooves on both sides after being butted together. That is, this embodiment is not only applicable to X-shaped grooves.

[0074] Example 5

[0075] In this embodiment 5, automatic TIG welding is mainly performed on aluminum alloy plates. The model of the aluminum alloy plate is 2A14, the state of the aluminum alloy plate is T6, and the specification of the aluminum alloy plate is δ8×100×210. At this time, the long side of the aluminum alloy plate has two chamfers. When the two aluminum alloy plates are butt-jointed, the butt joints of the two aluminum alloy plates form an "X"-shaped groove. The angle of the groove is 45°, and the blunt edge thickness of the groove is 0.5 mm. Specifically, the structure of the aluminum alloy plate is as follows: Figure 1 As shown, the structure of two aluminum alloy plates after butt joint is as follows Figure 2 shown.

[0076] In this embodiment 5, the welding machine used is the Magic Wave 5000Job G / F model of the Fronius brand, and the welding robot used is the M-20iD of the FANUC brand. 25 The welding wire model is BJ380A, the electrode is lanthanum tungsten WL20, and the pulse waveform during welding is as follows Figure 3 shown, and Figure 3 The meanings of the symbols in are as follows:

[0077] I1: peak current, unit A;

[0078] I G : Base current, unit A;

[0079] t1: AC cycle, unit: s;

[0080] ACF: AC frequency, unit: Hz; ACF = 1 / t1;

[0081] t2: peak time, unit: s;

[0082] t3: base time, unit: s;

[0083] dcY duty cycle: unit %, dcY = t2 / (t2+t3);

[0084] FP pulse frequency: unit Hz, FP = 1 / (t2 + t3);

[0085] BAL balance value: the range is between -5 and +5; when the BAL balance value is closer to -5, the melting effect is better and the cleaning ability is worse; when the BAL balance value is closer to +5, the cleaning ability is better and the melting effect is worse.

[0086] When welding two aluminum alloy plates, the welding environment is controlled at about 25℃, the humidity is about 50%, and the purity of argon gas is ≥99.99%. Before welding, the aluminum alloy plates and welding wires are mechanically or chemically cleaned and dried. The aluminum alloy plates can be fixed by clamps and then butt-jointed, and a stainless steel liner is added on the back of the weld. The preheating parameters of the aluminum alloy plates after butt-jointing are 120℃ and 30min. If the clamps can firmly fix the aluminum alloy plates, the butt-jointed aluminum alloy plates do not need to be spot welded, otherwise, the butt-jointed aluminum alloy plates need to be spot welded; during the spot welding process, the temperature between the middle layers is controlled below 120℃, gas is supplied 5s in advance before welding, and gas is continued for 10s after welding. The post-heating parameters of the aluminum alloy plates after welding are 120℃ and 4h~6h, and finally cooled with the furnace.

[0087] In order to describe the welding motion trajectory, that is, the operating state of the electrode tip, such as Figure 4 As shown in the figure, a three-dimensional rectangular coordinate system is established. When welding, the front weld and the back weld are performed alternately. However, whether it is the front weld or the back weld, it is described with reference to the three-dimensional rectangular coordinate system. The three-dimensional rectangular coordinate system determines the origin O(0, 0, 0) and the positive direction of each axis. The three-dimensional rectangular coordinate system is enlarged as shown in the figure below. Figure 5 As shown, in this embodiment 5, the electrode is always in the XZ plane during the entire welding process, and the angle between the electrode and the X+ direction is defined as the welding angle.

[0088] In this embodiment 5, looking from the X+ direction to the X- direction in the three-dimensional rectangular coordinate system, the schematic diagram of double-sided double-layer welding is as follows: Figure 6 As shown, the welding sequence is to weld the first layer of the front weld (front base), then weld the first layer of the back weld (back base), then weld the second layer of the front weld (front cover), and finally weld the second layer of the back weld (back cover). In these 4 layers, each layer is composed of 7 sets of welding parameters, and the 7 sets of welding parameters and operation trajectories correspond to 7 functions, namely arc preheating, welding sealing, climbing transition, main welding one, main welding two, attenuation transition, arc sealing. In this embodiment 5, the common welding parameters are shown in Table 1.

[0089] Table 1 shows the common parameters.

[0090]

[0091] In this embodiment 5, when the first layer of the front weld and the first layer of the back weld are welded, the running tracks of the electrodes on the front weld and the back weld are as follows: Figures 7 to 17 As shown, the coordinates of the electrode running trajectory are shown in Table 2.

[0092] Table 2 shows the running tracks of the electrodes during welding of the first layer of the front weld and the first layer of the back weld.

[0093]

[0094] Among them, when welding the first layer of the front weld, the main welding parameters of the first layer of the front weld are shown in Table 3 below, and the parameters from number 1 to number 7 in Table 3 correspond to the trajectories from number 1 to number 7 in Table 2, respectively.

[0095] Table 3 shows the main welding parameters of the first layer of the front weld

[0096]

[0097] When welding the first layer of the back weld, main welding parameters of the first layer of the back weld are shown in Table 4 below. The parameters from number 1 to number 7 in Table 4 correspond to the trajectories from number 1 to number 7 in Table 2, respectively.

[0098] Table 4 shows the main welding parameters of the first layer of the back weld

[0099]

[0100] In this embodiment 5, when the second layer of the front weld and the second layer of the back weld are welded, the running tracks of the electrodes on the first layer of the front weld and the first layer of the back weld are as follows: Figures 18 to 30 As shown, the coordinates of the electrode running trajectory are shown in Table 5.

[0101] Table 5 shows the running track of the electrode when welding the second layer of the front weld and the second layer of the back weld.

[0102]

[0103]

[0104] When welding the second layer of the front weld, main welding parameters of the second layer of the front weld are shown in Table 6 below. The parameters from number 1 to number 7 in Table 6 correspond to the trajectories from number 1 to number 7 in Table 5, respectively.

[0105] Table 6 shows the main welding parameters of the second layer of the front weld

[0106]

[0107] When welding the second layer of the back weld, main welding parameters of the second layer of the back weld are shown in Table 7 below. The parameters from number 1 to number 7 in Table 7 correspond to the trajectories from number 1 to number 7 in Table 5, respectively.

[0108] Table 7 shows the main welding parameters of the second layer of the back weld

[0109]

[0110] By using the automatic TIG welding method of the plate provided by the present invention, automatic TIG welding of aluminum alloy plates is successfully achieved. After appearance inspection, fluorescent penetration test, X-ray flaw detection, metallographic analysis and tensile strength test, the welding quality meets the Grade I weld requirements in the "Technical Requirements for Fusion Welding of Aluminum and Aluminum Alloys". The one-time inspection pass rate of welding using this method reaches more than 99%, and compared with manual welding, adding automatic welding of the starting and closing arc plates, and automatic welding with process tails, the production efficiency is increased by more than 300%.

[0111] In addition, according to the different plate thicknesses in actual production operations, the idea provided by this method can be used to achieve automatic TIG welding of aluminum alloy plates by appropriately increasing or decreasing the number of welding layers of the front weld and the back weld.

[0112] In the following, the butt joint of two plates is described in the form of a joint. The butt joint of two plates in the present invention is formed. Although the butt joint is used as an example for explanation in the present invention, the welding method disclosed in the present invention is still applicable to corner joints, lap joints, T-joints, etc. In addition, the welding method in the present invention is not limited to the welding between two aluminum alloy plates, but is also applicable to the welding between two steel plates or between two iron plates or between a steel plate and an iron plate. That is, the welding method in the present invention has no specific limitation on the material of the plate, and the materials of the two plates welded to each other can be the same or different.

[0113] It should be understood by those skilled in the art that the above embodiments are only for the purpose of clearly illustrating the present invention, and are not intended to limit the scope of the present invention. For those skilled in the art, other changes or modifications may be made based on the above disclosure, and these changes or modifications are still within the scope of the present invention.

Claims

1. An automatic TIG welding method for a plate, characterized in that: The single-sided welding layer is a single layer, which includes the following steps: S1. Bevel formation: butt the two plates to be welded together to form a bevel at the butt joint of the two plates; S2. Arc preheating: Place the electrode at a height of 5mm to 10mm from the bottom of the groove, and move the electrode from 5mm to 30mm from the starting end of the groove to the end of the groove. When the electrode is 4mm to 8mm away from the end of the groove, lift it up for the first time, and stop lifting it at the end face of the end of the groove. S3, welding: the electrode is lifted for the second time and gradually swung left and right to seal; the electrode swings back to the straight position and moves toward the starting end of the groove; S4. Arc closure and sealing: When the electrode reaches 3mm to 7mm away from the starting end of the groove, adjust the welding angle. After staying for a certain period of time, continue to move toward the end face of the starting end of the groove and lift it for the third time. When the electrode reaches the end face of the starting end of the groove, swing left and right and then return to the center, and gradually extinguish the arc.

2. The automatic TIG welding method of a plate according to claim 1, characterized in that: When the single-sided welding layer is not less than two layers, when welding a layer other than the last one, the welding angle is adjusted when the electrode reaches 3mm to 7mm away from the starting end of the groove, and it is lifted up for the third time after staying for a certain time and the arc is gradually extinguished; when welding the last layer, the welding angle is adjusted when the electrode reaches 3mm to 7mm away from the starting end of the groove, and it is lifted up for a third time after staying for a certain time and the arc is gradually extinguished.

3. The automatic TIG welding method of a plate according to claim 1 or 2, characterized in that: The height of the first lift is 2mm to 5mm.

4. The automatic TIG welding method of a plate according to claim 1 or 2, characterized in that: During the arc starting preheating stage, the angle between the electrode axis direction and the electrode forward direction is 65° to 85°.

5. The automatic TIG welding method of a plate according to claim 4, characterized in that: During the arc starting preheating stage, the angle between the electrode axis direction and the electrode forward direction is 72.5°.

6. The automatic TIG welding method of a plate according to claim 1 or 2, characterized in that: During the welding stage, the angle between the electrode axis direction and the electrode forward direction is 95° to 105°.

7. The automatic TIG welding method of a plate according to claim 6, characterized in that: During the welding stage, the angle between the electrode axis direction and the electrode forward direction is 97.5°.

8. The automatic TIG welding method of a plate according to claim 1 or 2, characterized in that: During the welding stage, the electrode stays for 0s to 1s after swinging into position; during the arc closing and sealing stage, the electrode stays for 0.5s to 1.5s after swinging into position for the second time.

9. The automatic TIG welding method of a plate according to claim 8, characterized in that: During the welding stage, the electrode stays for 0.5 seconds after swinging into position; during the arc closing and sealing stage, the electrode stays for 1 second after swinging into position for the second time.

10. The automatic TIG welding method of a plate according to claim 1 or 2, characterized in that: In the arc closing and sealing stage, after the welding angle is adjusted, the angle between the electrode axis direction and the electrode forward direction is 100°.

11. The automatic TIG welding method of a plate according to claim 1 or 2, characterized in that: During the arc closing and sealing stage, the electrode stays for 0.5s to 1.5s after adjusting the welding angle.

12. The automatic TIG welding method of a plate according to claim 1 or 2, characterized in that: The ambient temperature in steps S2 to S4 is 15° C. to 30° C., the humidity is ≤70%, and the purity of argon is ≥99.99%.

13. The automatic TIG welding method of a plate according to claim 1 or 2, characterized in that: The air supply time before step S3 and the continued air supply time after step S4 are both not less than 5 seconds.

14. The automatic TIG welding method of a plate according to claim 1 or 2, characterized in that: The groove formed at the butt joint of two plates to be welded is one of Y-type, V-type, U-type and X-type.