Specific gas enrichment method based on laser stealth processing technology
By using laser stealth processing to form secondary holes inside the metal organic framework material, the problem of low gas detection sensitivity in the existing technology is solved, efficient gas screening and enrichment is achieved, and detection efficiency is improved.
Patent Information
- Application Number
- CN202410929114.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The pore size of existing metal-organic framework materials is small, resulting in low detection sensitivity and poor detection limits after specific gas screening, making it impossible to achieve in-situ enrichment of gases.
Laser stealth processing technology is used to form secondary holes inside the metal organic framework material to achieve screening and enrichment of specific gases and improve detection sensitivity and detection limit.
By forming larger secondary holes inside the MOFs material, efficient gas enrichment is achieved, detection sensitivity and detection limit are improved, and the problem of low detection efficiency caused by molecular diffusion is avoided.
Smart Images

Figure CN118789145A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of laser processing, and in particular relates to a specific gas enrichment method based on laser stealth processing technology. Background Art
[0002] Specific gas screening is of great significance to human environmental health and sustainable energy utilization. For example, screening methane, ethane, etc. from natural mixed gases plays an important role in improving combustion efficiency. For example, screening carbon monoxide, carbon dioxide, etc. from harmful gases and converting them into combustible fuels such as methanol and ethanol is also of great value to energy conversion. For example, screening harmful gases such as formaldehyde from the air is also of great significance to human environmental health. At the same time, enriching and detecting the purity and gas composition of the screened gas also plays a very important strategic role in reducing detection costs and improving detection efficiency.
[0003] Since the microscopic topological structure of metal organic framework materials (MOFs materials) adapts to the structure of highly symmetric molecules, MOFs materials are good materials for screening specific gas molecules. Figure 1 As shown, the prior art utilizes the ordered nanopores of MOFs materials and utilizes the size and shape of the pores to screen the gas molecule mixtures.
[0004] CN202310277401.0 discloses a scheme for separating TMS and isopentane by using copper-based MOFs constructed with adamantane tetracarboxylic acid ligands, wherein the metal-organic framework material is Cu2(ATC)(2H2O)·5H2O, and ATC is 1,3,5,7-adamantane tetracarboxylic acid with four hydrogen radicals removed. This technical scheme utilizes the adjustable pore characteristics of MOFs to accurately synthesize MOFs suitable for TMS separation and purification, thereby being used for separation of TMS and isopentane mixtures produced in industrial production, thus filling the gap of MOFs in this separation application. At the same time, separation using ATC-Cu can obtain extremely pure TMS, which has better separation effect than zeolite molecular sieves and is more energy-efficient than distillation.
[0005] However, the pore size of metal-organic framework materials is relatively small, most of which are concentrated at the nanoscale. The screening method remains at the relay level, that is, flow screening of molecules one by one. Since there is no in situ enrichment of the screened molecules in a relay container, the subsequent detection sensitivity of such single molecules is low and the detection limit is poor. Summary of the invention
[0006] The purpose of the present invention is to provide a specific gas enrichment method based on laser stealth processing technology. The method utilizes laser stealth processing technology to stealthily process secondary holes inside a metal organic framework material without damaging the surface of the material, while achieving screening of specific gases and enrichment of the single gas after screening inside the material, thereby improving the detection limit and detection sensitivity.
[0007] Another object of the present invention is to utilize the above-mentioned specific gas enrichment method based on laser stealth processing technology to screen and enrich specific gases.
[0008] In order to achieve the above object, the present invention adopts the following technical solution: A specific gas enrichment method based on laser stealth processing technology comprises the following steps: S1: Synthesize MOFs single crystal materials with characteristic size above 30 μm; S2: Using laser to perform invisible processing inside the MOFs single crystal material in step S1 to form secondary holes; S3: placing the material in step S2 in a mixed gas for gas screening and enrichment.
[0009] Furthermore, the pore diameter of the MOFs single crystal material in step S1 is less than 2 nm.
[0010] Furthermore, the MOFs single crystal material in step S1 includes but is not limited to HKUST-1, MOF-5 or ZIF-8.
[0011] Furthermore, step S1 adopts a general solvent thermal synthesis method, the synthesis temperature is 70° C.-120° C., and the synthesis time is 10 h-48 h.
[0012] Furthermore, in step S2, a pulsed laser with a wavelength of 532 nm-1064 nm, a laser power of 2 W-3 W, and a laser spot diameter of 5 μm-10 μm is used.
[0013] Furthermore, in step S2, processing is performed inside the MOFs single crystal material at a depth of 10 μm-20 μm from the surface.
[0014] Furthermore, in step S2, the laser processing time is 10 s-30 s.
[0015] Furthermore, in step S2, the diameter of the secondary pore is 20 μm-30 μm and is located at the center of the MOFs single crystal material.
[0016] Furthermore, in step S3, the types of the mixed gas include but are not limited to methanol / carbon monoxide mixed gas and methane / ethane mixed gas.
[0017] The present invention has the following beneficial effects: (1) Compared with the previously simply synthesized metal organic framework materials, the present invention first synthesizes metal organic framework material crystals with specific nanopore shapes and nanopores modified with specific chemical groups based on the chemical and physical properties of specific gases to screen the mixed gas; then, by using laser invisible processing at the center of the material, a larger secondary hole is formed inside the material. Therefore, while screening small-sized gases, the screened gas is directly enriched in situ, avoiding the problem of low detection efficiency due to molecular diffusion after screening.
[0018] (2) The small-sized gas enrichment degree based on the method of the present invention is high, the enrichment time is shorter, and the enrichment efficiency is higher. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Gas screening technology for the prior art; Figure 2 is a schematic diagram of the method of the present invention; Figure 3 TEM image of the HKUST-1 single crystal material with secondary pores in Example 1. DETAILED DESCRIPTION
[0020] The present invention is described in detail below with reference to the accompanying drawings and embodiments: As used herein, the term "laser invisible processing technology" refers to a technology that focuses the laser light inside a material for processing without causing any processing damage to the surface of the material.
[0021] As used herein, the term "metal organic framework material" refers to a long-range ordered crystalline material having orderly arranged pores less than 10 nm in size inside the material.
[0022] As used herein, the term "characteristic size" refers to the length between the two farthest points on the surface of a single crystal particle. For example, when describing the characteristic size of a MOFs single crystal material as being greater than 30 μm, it means that the length between the two farthest points on the surface of the MOFs single crystal material is greater than or equal to 30 μm.
[0023] As used herein, unless otherwise specified, numerical ranges include both the starting and ending values of the range. For example, when describing the wavelength of a laser as "532 nm-1064 nm", this means that both 532 nm and 1064 nm are valid values of the wavelength.
[0024] As used herein, unless otherwise specified, the materials, reagents, devices, etc. used in the present invention are all commercially available products.
[0025] like Figures 2 to 3 As shown, the specific gas enrichment method based on laser stealth processing technology of the present invention comprises the following steps: S1: Synthesize MOFs single crystal materials with characteristic size above 30 μm; S2: Using laser to perform invisible processing inside the MOFs single crystal material in step S1 to form secondary holes; S3: placing the material in step S2 in a mixed gas for gas screening and enrichment.
[0026] In step S1, there is no particular limitation on the method for synthesizing the MOFs single crystal material, and the MOFs single crystal material can be synthesized using conventional methods known to those skilled in the art.
[0027] In one embodiment of the present invention, a general solvent thermal synthesis method is used to synthesize MOFs single crystal material. Specifically, step S1 includes: dissolving the selected metal salt and organic ligand in a mixed solution of DMF, water and ethanol in a volume ratio of 1:1:1, and then standing at a temperature of 70°C-120°C for 10 h-48 h to generate MOFs single crystal material.
[0028] After synthesizing MOFs single crystal materials of appropriate size, a series of post-treatments are required to obtain the final MOFs single crystal samples. Specifically, step S1 also includes: replacing the generated MOFs single crystal materials with 15 mL-35 mL of pure ethanol liquid for immersion, then filtering the crystals, and then drying them in a vacuum drying oven for 20 h-28 h to obtain dry MOFs crystals.
[0029] In the present invention, the soaking time in the ethanol liquid is generally at least two days, and during the soaking period, the ethanol liquid needs to be replaced every 8 hours to ensure the soaking effect.
[0030] As known to those skilled in the art, the pore shapes and sizes of different types of MOFs materials are different, which can be controlled by selecting different types of reaction raw materials. For example, in one embodiment of the present invention, the metal ions in the metal salt are metal ions with specific orientations, including but not limited to Cu 2+ 、Zn 2+ The organic ligand is generally selected to be an organic ligand with good rigidity and strong directionality, including but not limited to terephthalic acid and trimesic acid. Based on the selected metal salt and organic ligand, the MOFs single crystal material in step S1 includes but is not limited to HKUST-1, MOF-5 and ZIF-8.
[0031] In the present invention, the MOFs single crystal material synthesized in step S1 has nanoscale pores. The nanoscale pores inside the MOFs single crystal material itself should be compatible with the gas with smaller molecular size in the mixed gas, generally about 2 nm or less, to ensure that the smaller molecules in the mixed gas can pass through the nanoscale pores inside the MOFs crystal, while the larger molecules cannot pass through the nanoscale pores, thereby achieving screening of the two. In addition, the size of the MOFs single crystal material should be large enough to ensure that the size of the single crystal particles is larger than the size of the laser spot, avoiding ablation of the outer surface of the single crystal, so as to achieve processing inside without damaging its surface morphology. Therefore, the synthesized MOFs single crystal material should be a MOFs single crystal material with a characteristic size of more than 30 μm to ensure the smooth progress of laser stealth processing.
[0032] In the present invention, the laser processing device used in step S2 is a conventional device and will not be described in detail here.
[0033] During the laser stealth processing, the thermal effect of the laser is used to ablate secondary holes inside the MOFs single crystal. Since the general MOFs crystal has low absorbance to lasers with a wavelength of 532 nm-1064 nm, it can be ensured that the laser spot within this wavelength range can be focused inside the MOFs crystal body. Therefore, the laser used in the present invention is a pulsed laser with a wavelength of 532 nm-1064 nm. At the same time, the laser spot diameter must be smaller than the size of the MOFs single crystal material to ensure that it will not affect the outer surface of the single crystal. Therefore, the laser spot diameter is preferably 5 μm-10 μm. In addition, in conjunction with the laser spot size, the laser power used is 2 W-3 W. If the laser power is too large, it may penetrate the MOFs crystal or ablate the MOFs crystal, resulting in the inability to form suitable secondary holes inside it.
[0034] In addition, an appropriate laser processing time should be selected. If the processing time is too short, it is impossible to ensure that the secondary holes of appropriate size are generated; and if the processing time is too long, excessive ablation may result. Therefore, in the present invention, the laser processing time is 10 s-30 s.
[0035] In addition, in order to avoid damage to the surface of MOFs crystals caused by laser thermal effects, during the laser stealth processing, under appropriate laser processing parameters, the laser is focused on the inside of the MOFs single crystal material at a depth of 10 μm-20 μm from the surface to create secondary holes inside the MOFs single crystal material. At the same time, during the processing, the processing position is observed in real time by the imaging system in the laser processing device to ensure that the secondary hole is located at the center of the MOFs single crystal material through the movement of the motion platform.
[0036] In the present invention, the size of the secondary pores is adapted to the size of the single crystal material and the size of the gas molecules to be accommodated. For example, secondary pores with a diameter of more than 20 μm can be formed to accommodate the gas molecules after screening, thereby achieving the enrichment of the mixed gas.
[0037] According to the present invention, the MOFs single crystal material with secondary pores inside can achieve the screening and enrichment of specific mixed gases under the cooperation of the nano-scale pores and micron-scale secondary pores of the material itself. Generally speaking, the specific mixed gas that needs to be screened and enriched is selected according to the pore diameter of the MOFs material. For the present invention, the pore diameter below 2 nm can be used to screen small-sized gases such as methane, carbon monoxide, etc. Therefore, for example, the types of specific mixed gases of the present invention include but are not limited to methanol / carbon monoxide mixed gas and methane / ethane mixed gas.
[0038] The working principle of the present invention is as follows: The present invention forms a MOFs single crystal material with an internal pore size of about 2 nm or less by selecting organic ligands with good rigidity and strong directionality and metal ions with specific orientation. Since the sizes of the two gas molecules in the mixed gas are different, the smaller molecules are adapted to the nanopore size of the MOFs crystal, and the larger molecules cannot pass through the nanopore, based on which the screening of the two can be achieved. At the same time, laser invisible processing technology is used to create larger secondary holes with a diameter of 10 μm-20 μm inside the MOFs single crystal material to accommodate the gas molecules after screening, thereby achieving the screening and enrichment of the mixed gas and improving the detection limit and detection sensitivity.
[0039] The present invention is further illustrated by the following examples.
[0040] Embodiment 1: S1: 200 mg of trimesic acid and 400 mg of copper nitrate trihydrate were placed in a 23 mL sealed glass bottle, and then 12 mL of a mixed solution of DMF, water and ethanol with a volume ratio of 1:1:1 was added to fully dissolve it. After standing at 85 °C for 12 h, a HKUST-1 single crystal material with a characteristic size of 50 μm was synthesized. Subsequently, the generated HKUST-1 single crystal material was replaced and immersed in 25 mL of pure ethanol liquid, and the ethanol liquid was replaced every 8 hours for three days. The crystals were then filtered and dried in a vacuum drying oven for 24 h to obtain dry HKUST-1 crystals.
[0041] S2: A nanosecond laser with a wavelength of 1064 nm was selected, the laser power was maintained at 2 W, the processing distance was focused at 2 cm, the spot diameter was 10 μm, and it was focused at a depth of 20 μm from the surface inside the HKUST-1 single crystal material. The processing time lasted for 10 s. After ablation, a secondary hole with a diameter of 22 μm was obtained at the center of the HKUST-1 single crystal particle.
[0042] S3: 100 mg of laser processed HKUST-1 single crystal particles and unprocessed HKUST-1 single crystal were placed in a volume of 1 cm 3 The spherical glass tube is filled with a methane / ethane (volume ratio of 1:1) mixed gas, and the open end of the glass tube is connected to a gas adsorption instrument, which can respond to the pressure change in the tube. Then it is left at 77 K for 1 hour, and the pressure reduction is measured. According to the ideal gas equation: pV=nRT, when the volume and temperature remain unchanged, the amount of methane gas reduced in the glass tube is converted to the amount of methane adsorbed by the single crystal.
[0043] like Figure 3 As shown, after step S2, a secondary hole with a diameter of 22 μm is obtained at the center of the HKUST-1 single crystal particle, and the secondary hole is substantially circular.
[0044] By comparing the results after step S3, it can be seen that the specific adsorption amount of methane by the HKUST-1 single crystal particles of the present invention, i.e., the HKUST-1 single crystal particles processed by laser, is about 2667.9 cm 3 / g, while the specific adsorption capacity of methane by the untreated HKUST-1 single crystal particles is only 532.6 cm 3 / g.
[0045] Embodiment 2: S1: 150 mg of terephthalic acid and 300 mg of copper sulfate pentahydrate were placed in a 25 mL sealed glass bottle, and then 12 mL of a mixed solution of DMF, water and ethanol with a volume ratio of 1:1:1 was added to fully dissolve it, and it was allowed to stand at 100 ° C for 24 h to synthesize a MOF-5 single crystal material with a characteristic size of 60 μm. Subsequently, the generated MOF-5 single crystal material was replaced and soaked in 30 mL of pure ethanol liquid, and the ethanol liquid was replaced every 8 hours for three days. Then the crystals were filtered and dried in a vacuum drying oven for 25 h to obtain dry MOF-5 crystals.
[0046] S2: Select a picosecond laser with a wavelength of 532 nm, keep the laser power at 3 W, focus the processing distance at 2 cm, and focus the spot diameter at 5 μm, focusing at a depth of 20 μm from the surface inside the MOF-5 single crystal particle, and the processing time lasts for 20 seconds. After ablation, a secondary hole with a diameter of 25 μm is obtained at the center of the MOF-5 single crystal particle.
[0047] S3: 100 mg of laser processed MOF-5 single crystal particles and unprocessed MOF-5 single crystals were placed in a volume of 1 cm 3 The spherical glass tube is filled with a methanol / carbon monoxide (volume ratio of 1:1) mixed gas, and the open end of the glass tube is connected to a gas adsorption instrument, which can respond to the pressure change in the tube. Then it is left at 77 K for 1 hour, and the pressure decrease is measured. According to the ideal gas equation: pV=nRT, when the volume and temperature remain unchanged, the amount of carbon monoxide gas reduced in the glass tube is converted to the amount of carbon monoxide adsorbed by the single crystal.
[0048] By comparing the results after step S3, it can be seen that the specific adsorption capacity of carbon monoxide by the MOF-5 single crystal particles of the present invention, that is, the MOF-5 single crystal particles processed by laser, is about 1877.8 cm 3 / g, while the specific adsorption capacity of untreated MOF-5 single crystal particles for carbon monoxide is only 268.7 cm 3 / g.
[0049] In summary, according to the method of the present invention, pulsed laser ablation is used to obtain micron-sized secondary pores inside a MOFs single crystal having nanoscale pores that can screen small-sized gas molecules. The micron-sized secondary pores can accommodate a large number of specific molecules after screening. The size combination of the nanoscale pores and the micron-sized secondary pores can simultaneously achieve the screening and enrichment of small-sized molecules, thereby improving the detection limit and detection sensitivity of a single gas after screening.
[0050] The specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in this field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in this technical field through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the existing technology should be within the scope of protection determined by the claims.
Claims
1. A specific gas enrichment method based on laser stealth processing technology, characterized in that: The following steps are involved: S1: Synthesize MOFs single crystal materials with characteristic size above 30 μm; S2: Using laser to perform invisible processing inside the MOFs single crystal material in step S1 to form secondary holes; S3: placing the material in step S2 in a mixed gas for gas screening and enrichment.
2. The specific gas enrichment method based on laser stealth processing technology according to claim 1 is characterized in that: The pore diameter of the MOFs single crystal material in step S1 is less than 2 nm.
3. The specific gas enrichment method based on laser stealth processing technology according to claim 1 is characterized in that: In step S2, a pulsed laser with a wavelength of 532 nm-1064 nm, a laser power of 2 W-3 W, and a laser spot diameter of 5 μm-10 μm is used.
4. The specific gas enrichment method based on laser stealth processing technology according to claim 1 is characterized in that: In step S2, processing is performed inside the MOFs single crystal material at a depth of 10 μm-20 μm from the surface.
5. The specific gas enrichment method based on laser stealth processing technology according to claim 1 is characterized in that: In step S2, the laser processing time is 10 s-30 s.
6. The specific gas enrichment method based on laser stealth processing technology according to claim 1, characterized in that: In step S2, the diameter of the secondary pore is 20 μm-30 μm and is located at the center of the MOFs single crystal material.
7. The specific gas enrichment method based on laser stealth processing technology according to claim 1 is characterized in that: In step S3, the types of mixed gas include methanol / carbon monoxide mixed gas and methane / ethane mixed gas.
8. The specific gas enrichment method based on laser stealth processing technology according to claim 1 is characterized in that: Step S1 adopts a solvent thermal synthesis method, the synthesis temperature is 70° C.-120° C., and the synthesis time is 10 h-48 h.
9. Use of the specific gas enrichment method based on laser stealth processing technology as described in any one of claims 1 to 8 to screen and enrich specific gases.
10. The use according to claim 9, characterized in that: The types of the specific gas include methanol / carbon monoxide mixed gas and methane / ethane mixed gas.
Citation Information
Patent Citations
Organic metal frameworks nano material, and preparation and application thereof
CN112755183A
Metal organic framework microstructure laser manufacturing device and method
CN112898590A
Metal organic framework material as well as preparation method and application thereof
CN116003809A
Method for synthesizing hollow carbon spheres by laser-induced aluminum metal organic framework and application of hollow carbon spheres
CN117228656A
Appratus for Dynamic Pile Load Test